Composite material taking collagen as matrix and preparation method thereof

Through the composite material of collagen and star polymer, a layered fiber structure of the human cornea is formed, which solves the problem of insufficient performance of existing artificial corneal materials, and achieves biocompatibility with high light transmittance and good mechanical properties. Corneal repair.

CN118987358APending Publication Date: 2024-11-22SOUTHERN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411156424.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing artificial corneal materials cannot effectively simulate the layered fiber structure of the human cornea, resulting in insufficient optical, mechanical and biological properties, which makes it difficult to meet clinical needs.

Method used

A composite material of collagen and star polymer is used to form a multi-layer structure through temperature and wet drying treatment, which simulates the layered fiber structure of the human cornea and combines growth factors to improve biocompatibility and mechanical properties.

Benefits of technology

It realizes the high light transmittance, good mechanical properties and biocompatibility of composite materials, and is suitable for the regeneration and repair of corneal or other biological tissues, and is used as medical materials in organisms or their tissues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118987358A_ABST
    Figure CN118987358A_ABST
Patent Text Reader

Abstract

The invention provides a composite material taking collagen as a matrix, a preparation method of the composite material and an artificial cornea, and relates to the technical field of biological materials. The composite material comprises collagen, the collagen comprises a plurality of layers of collagen fibers, and each layer of collagen fibers comprises a plurality of collagen fibers extending in the approximately same direction; and a star polymer that is present in the collagen. The composite material provided by the invention has a layered fiber fine structure similar to that of a natural cornea, is high in light transmission and good in mechanical property and biocompatibility, is suitable for an artificial cornea or other biological tissues, and can be used as an artificial organ to be applied to an organism or tissues thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of biomaterials, and in particular to a composite material with collagen as a matrix, a preparation method thereof, and an artificial cornea. Background Art

[0002] The cornea is a transparent thin film tissue located on the front wall of the eyeball. It is a protective barrier against pathogen attacks on the eyeball. The thickness of the cornea varies from species to species. For example, the thickness of the human cornea is about 500μm, the thickness of the rabbit cornea is about 300μm, the thickness of the pig cornea is about 1000μm, and the thickness of the cow cornea is about 1000-2000μm. Another important function of the cornea is to allow light to pass through the pupil and converge into the retina of the fundus for imaging, similar to the lens of a camera. However, the cornea is susceptible to damage, including corneal ulcers caused by bacteria or viruses, corneal damage caused by chemicals or mechanical means, and keratoconus and corneal dystrophy caused by tumors and autoimmune diseases. Corneal damage can easily cause corneal perforation, edema, scar formation and other lesions, leading to blindness. Corneal diseases have become the fourth leading cause of blindness in the world, and are mainly treated clinically through corneal transplantation. However, there is a serious shortage of natural corneal donors, and if the patient receiving the corneal donor has a previous history of rejection or corneal vascularization, the transplantation failure rate can be as high as 70%.

[0003] Using artificial corneas to replace natural corneal donors has always been a research hotspot in the field of ophthalmology. The most widely used artificial cornea in the world is the Boston KPro, which mainly uses the organic synthetic polymer material polymethylmethacrylate (PMMA). Since PMMA is not biodegradable and its mechanical strength is far from that of the human cornea, it cannot be integrated with human tissues, so its clinical promotion is very limited. The Osteo-odonto-keratoprosthesis (OOKP), which was developed at the same time, uses autologous canine root tissue and surrounding ligament tissue that can better integrate with the eyeball, and places a small plastic lens in the middle, so that patients can see the light again. Compared with the Boston KPro, the Osteo-odonto-keratoprosthesis has a smaller rejection reaction and a higher success rate, but its function and aesthetics are unsatisfactory, and the surgical process is very complicated and difficult.

[0004] In recent years, bioengineered artificial corneas have gradually developed, mainly including two materials: decellularized animal corneas and collagen membranes. Decellularized animal corneas, because they come from animals, have the risk of rejection in the human body; while collagen-based artificial corneas are still limited by their comprehensive optical, mechanical and biological properties, and are difficult to meet the clinical needs of artificial corneas.

[0005] From a histological point of view, the main component of a healthy cornea is collagen, and its superior optical and mechanical properties are attributed to the very fine layered fiber structure of collagen in the cornea. During the development of the human corneal stroma, the formation of this fine structure of collagen fibers in the cornea is controlled by a series of factors. The corneal stroma contains a class of proteoglycans, namely small leucine-rich proteoglycans (SLRP), which have a structure of multiple sugar chains connected to the core protein, and play an extremely critical role in regulating the thickness of collagen fibers, the spacing between collagen fibers and the spacing between fiber layers, and the arrangement and orientation of collagen fibers. In addition, the microenvironment in the cornea, such as osmotic pressure, also affects the formation of collagen fibers. Therefore, compared with collagen fibers in other organs, collagen fibers in the human cornea are thinner (only about 30nm in diameter) and arranged more regularly and orderly. However, the content of SLRP in natural cornea is very small and difficult to extract. Traditional in vitro prepared collagen materials do not contain SLRP and are generally prepared using isotonic pH buffer, which results in larger collagen fibers and random arrangement. Summary of the invention

[0006] Based on this, it is necessary to provide a composite material with collagen as a matrix, a preparation method thereof, and an artificial cornea.

[0007] In a first aspect, the present specification provides a composite material with collagen as a matrix, comprising: collagen, wherein the collagen comprises multiple layers of collagen fibers, each layer of collagen fibers comprises multiple collagen fibers extending in substantially the same direction; and star-shaped polymers present in the collagen.

[0008] In some embodiments, the extending direction of the collagen fibers in each layer is different from the extending direction of the collagen fibers in another adjacent layer.

[0009] In some embodiments, the multilayered collagen fibers are formed under the induction of the star polymer.

[0010] In some embodiments, the linear branches of the star polymer include at least one of polyethylene glycol (PEG), polyethylene glycol derivatives, polypropylene glycol (PPG), polypropylene glycol derivatives, polyacrylic acid (PAA), polyacrylic acid derivatives, polyvinyl alcohol (PVA), polyvinyl alcohol derivatives, polyethyleneimine (PEI), polyethyleneimine derivatives, and polypeptide chains (PP).

[0011] In some embodiments, the relative molecular mass of the star polymer is between 10 3 ~10 6 between.

[0012] In some embodiments, the collagen includes at least one of type I collagen, type II collagen, type III collagen, type IV collagen, type V collagen, and type XI collagen.

[0013] In some embodiments, the mass ratio of the collagen to the star polymer is 100:(0.1-20).

[0014] In some embodiments, the composite material has a thickness of 30 μm to 2000 μm.

[0015] In some embodiments, the thickness of each collagen layer in the composite material is 0.1 μm to 10 μm.

[0016] In some embodiments, the diameter of the collagen fibers is 5 nm to 100 nm.

[0017] In some embodiments, the composite material has a light transmittance greater than 70% at a wavelength of 550 nm.

[0018] In some embodiments, the composite material further comprises: water mixed in the collagen.

[0019] In a second aspect, the present specification provides an application of a composite material in preparing a matrix for repairing biological tissues.

[0020] In a third aspect, the present specification provides an artificial cornea, wherein the artificial cornea is prepared using any of the composite materials described above.

[0021] In a fourth aspect, the present specification provides a method for preparing a composite material, comprising the following steps: obtaining a collagen solution with a pH value less than 7, and obtaining a star-shaped polymer solution with a pH value greater than 7; mixing the collagen solution and the star-shaped polymer solution to obtain a mixed solution; and subjecting the mixed solution to gelation and temperature-controlled and humidity-controlled drying treatments in sequence to obtain the above-mentioned composite material, wherein the temperature-controlled and humidity-controlled drying treatment refers to controlling the temperature and humidity conditions to dry the composite material.

[0022] In some embodiments, the concentration of collagen in the collagen solution is 1 mg / mL to 10 mg / mL; and the concentration of the star polymer in the star polymer solution is 0.01 mg / mL to 2.0 mg / mL.

[0023] In some embodiments, the star polymer solution uses a pH buffer as a solvent, and the pH buffer is at least one of a phosphate buffer, an amino acid buffer, a citric acid buffer, a carbonate buffer, an acetate buffer, a barbituric acid buffer, a cell culture medium buffer, a 4-hydroxyethylpiperazineethanesulfonic acid (HEPES) buffer, and a tris(hydroxymethyl)aminomethane hydrochloride (Tris-HCl) buffer.

[0024] In some embodiments, the star polymer solution uses a pH buffer as a solvent, and the pH buffer has an osmotic pressure of 5 to 260 mOsm / L.

[0025] In some embodiments, the mixed solution also includes growth factors, and the growth factors are at least one of epidermal growth factor (EGF), fibroblast growth factor (FGF), platelet-derived growth factor (PDGF), human insulin-like growth factor (IGF), hepatocyte growth factor (HGF), bone morphogenetic protein (BMP), transforming growth factor (TGF), and vascular endothelial growth factor (VEGF).

[0026] In some embodiments, the preparation method further comprises: subjecting the composite material to a hydration treatment.

[0027] It can be seen from the above technical scheme that the composite material provided in this specification includes collagen and star-shaped polymer, wherein the multiple linear branches of the star-shaped polymer can be combined with collagen through intermolecular forces, so that the multiple linear branches of the star-shaped polymer cling to the collagen, control the collagen to form a multilayer structure, and in each layer, the collagen fibers extend in the same direction. The composite material provided in this specification has a layered fiber fine structure similar to that of a natural cornea, and the composite material has high light transmittance, good mechanical properties and biocompatibility, and is suitable for regeneration and repair of cornea or other biological tissues, and is used as a medical material in organisms or their tissues. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a schematic diagram of the structure of the composite material self-assembly process in some embodiments of this specification;

[0029] Figure 2 A in the figure is a statistical diagram of the diameter of collagen fibers of collagen fibers without star-shaped polymers obtained according to the composite material preparation route of this specification; Figure 2 B is a statistical diagram of the diameter of collagen fibers of the star-shaped polymer-containing collagen fiber material obtained according to the composite material preparation route of this specification;

[0030] Figure 3 The transmittance test results of the composite materials of some embodiments and comparative examples of this specification at a wavelength of 550nm;

[0031] Figure 4 A flow chart of a method for preparing a composite material according to some embodiments of this specification;

[0032] Figure 5 A schematic diagram of the preparation route of the composite material of some embodiments of this specification;

[0033] Figure 6 The collagen fiber diameter results of the composite materials of some embodiments of this specification under different osmotic pressure conditions;

[0034] Figure 7 Cryo-electron microscopy photos of the mixed solutions of collagen and star-shaped polymers in some embodiments of this specification;

[0035] Figure 8 A in the figure is a cross-sectional photograph of a composite material according to some embodiments of the present specification under a transmission electron microscope (TEM); Figure 8 B is another cross-sectional photograph of the composite material according to some embodiments of the present specification under a transmission electron microscope (TEM); Figure 8 C in FIG. 1 is another cross-sectional photograph of the composite material according to some embodiments of the present specification under a transmission electron microscope (TEM);

[0036] Fig. 9 A bar graph showing the Young's modulus of the hydrated composite materials subjected to tensile mechanical tests of some embodiments and comparative examples of the present specification;

[0037] Fig.10 A bar graph showing elongation at break of hydrated composite materials in tensile mechanical tests of some embodiments and comparative examples of this specification;

[0038] Fig.11 A bar graph showing the suture retention strength (SRS) of suture mechanical tests of hydrated composite materials of some embodiments and comparative examples of the present specification;

[0039] Fig.12 The results of culturing rabbit corneal primary epithelial cells on the composite materials of some embodiments of this specification;

[0040] Fig.13 The results of culturing primary rabbit corneal stromal cells on the composite materials of some embodiments of this specification;

[0041] Fig.14 This is a living experiment diagram of the anterior lamellae of the rabbit cornea transplanted with composite materials according to some embodiments of the present specification;

[0042] Fig.15 Transmission electron microscope (TEM) photos of collagen fiber materials without star-shaped polymers of some comparative examples of this specification;

[0043] Fig.16The transmission electron microscope (TEM) photos of collagen fiber materials of some comparative examples of this specification which do not contain star polymers and are prepared with isotonic pH buffer. DETAILED DESCRIPTION

[0044] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0046] For the convenience of description, the terms that may appear in this manual are first explained as follows:

[0047] Star polymers are polymers with three or more linear branches radially connected from one branching point.

[0048] Collagen (also called collagen) is a structural protein widely present in connective tissues in animals (bone tissue, skin tissue, corneal tissue, etc.). Collagen can be extracted from animal tissues or prepared by artificial synthesis. Artificially synthesized recombinant collagen usually does not have a fiber structure, but collagen in animals generally exists in a fiber structure. Collagen mainly includes type I collagen, type II collagen, type III collagen, type IV collagen, type V collagen and type XI collagen, with type I collagen being the most common.

[0049] Each polypeptide chain of collagen has about 1,000 amino acid residues. Usually, Gly represents glycine, and X and Y represent other amino acids besides glycine, among which proline and hydroxyproline are the most abundant. The structure of collagen, taking type I collagen as an example, has a quaternary structure. The amino acids in its primary structure are arranged repeatedly in the Gly-XY sequence; the secondary structure of collagen is that each peptide chain forms a left-handed helix, which is mainly caused by the electrostatic repulsion between proline and hydroxyproline at the X and Y positions; the tertiary structure of collagen is that three left-handed helical polypeptide chains further coil around each other through hydrogen bonds and other interactions to form tropocollagen with a right-handed superhelical structure. Tropocollagen further self-assembles to form a quaternary structure, namely collagen fibers.

[0050] The main component of the human cornea is collagen, which mainly includes three parts: epithelium, stroma and endothelium. Among them, the stroma in the middle accounts for about 90% of the thickness of the entire cornea, with a thickness of about 0.5mm. It is mainly composed of collagen fibers with a diameter of about 30nm arranged in parallel to form a multi-layer lamellar structure at a certain angle to each other. Compared with the diameter of collagen fibers in other tissues (generally about 100-200nm), the collagen fibers in the cornea are thinner, which greatly reduces the scattering of visible light (390-780nm), bringing excellent transparency to the corneal tissue. At the same time, the collagen fibers in the cornea have a unique layered structure, and the collagen fibers in each layer are arranged in a consistent and extremely regular orientation. Compared with randomly arranged collagen fiber materials, the density of collagen fibers per unit volume is greatly increased, thereby increasing the interaction within and between collagen fibers per unit volume. Different layers of collagen fibers have different orientations, and the entire cornea is formed by more than 200 layers of collagen fibers stacked on top of each other. It is this unique layered fiber structure that effectively enhances the radial toughness, tensile properties and tear resistance of corneal tissue.

[0051] The present specification provides a composite material with collagen as a matrix, which has a layered fiber fine structure similar to the native cornea of ​​the human body. The composite material includes collagen and star-shaped polymers, the collagen includes multiple layers of collagen fibers, and each layer of collagen fibers includes multiple collagen fibers extending along substantially the same direction; the star-shaped polymer exists in the collagen.

[0052] In the composite material provided in this specification, the star-shaped polymer is mixed in the collagen. Figure 1 Schematic diagram of the structure of the composite material self-assembly process in some embodiments of this specification. Figure 1As shown, similar to the small leucine-rich proteoglycan (SLRP) in the cornea, the multiple linear branches of the star polymer can be combined with collagen through intermolecular forces, so that the multiple linear branches of the star polymer can climb on the collagen fibers, and regulate the collagen to form more slender fibers during the collagen fiber formation process. Further, during the temperature-controlled and humidity-controlled drying self-assembly process of the collagen fibers, the gelled collagen composite material is slowly dried layer by layer from the surface of the material. Since the star polymer plays a lubricating role on the surface of the collagen fibers, it is beneficial for the adjacent collagen fibers to be arranged into a more orderly structure, promote the collagen fibers in each layer to extend in a generally similar direction, and control the collagen fibers to form a bionic multilayer structure. In addition, during the self-assembly process of the collagen fibers under temperature-controlled and humidity-controlled conditions, it should be noted that due to the relatively large aspect ratio of the collagen fibers, the collagen fibers cannot be completely in a straight line shape in actual situations, which results in that two different collagen fibers in the same layer generally cannot be completely parallel. Furthermore, a certain angle is allowed between two different collagen fibers in the same layer in the extension direction. Therefore, the "substantially the same direction" mentioned in this specification means that the collagen fibers in the same layer are basically parallel, so that their extension directions (fiber orientations) are basically the same. Due to the softness of collagen, the fiber direction can be a straight line direction or a curved line direction, rather than extending in a straight line and / or in a completely consistent direction in a strict mathematical sense.

[0053] In summary, the composite material provided in this specification has a layered fiber structure similar to that of a natural cornea, that is, the collagen in the composite material presents a layered structure, and the extension directions of the collagen in adjacent layers are different. Such a layered fiber structure brings excellent mechanical properties close to those of the native human cornea to the composite material, so that the composite material has good toughness and tensile properties. The structure of multiple layers with different fiber orientations is a typical structure of a composite material. Compared with materials of a single material, composite materials have the advantages of better strength and toughness. The better the interlayer fiber orientation, the finer the fibers, and the higher the flexibility of the composite material. Since the fiber directions of each layer are different, the tensile strength of the composite material in all directions is very high. Compared with traditional collagen fiber materials (collagen fibers are randomly arranged and have a thicker diameter), the composite material has better flexibility and tensile strength, that is, better suturing properties.

[0054] It is understandable that in the composite materials provided in some embodiments of the present specification, the extension directions of the collagen fibers of the two adjacent layers are different, and the collagen fibers of the two adjacent layers may be at a certain angle α (0°<α≦90°) according to their extension directions. For example, α may be 0.1°, 1°, 5°, 10°, 20°, 30°, 40°, 50°, 65°, 75°, 85°, 90°, or an angle between any two of the above angle values. Among them, when α is 0°, the extension directions of the collagen fibers of the two adjacent layers are parallel, that is, the extension directions of the collagen of the two adjacent layers are the same; when α is 90°, it means that the collagen fibers of the two adjacent layers are orthogonally arranged.

[0055] In some embodiments, the multilayered collagen fibers are formed under the induction of the star polymer.

[0056] The superior performance of the human cornea is due to the unique layered fiber structure of its collagen fibers, and the formation of the ultrastructure of collagen fibers is generally believed to be controlled by a key class of proteoglycans, namely small leucine-rich proteoglycans (SLRP). SLRP accounts for 4%-5% of the dry weight of the human cornea, mainly including decorin, lumican, mimecan and keratocan. Among them, decorin mainly controls the spacing of collagen fibers and the adhesion between fiber layers, and the latter three SLRPs mainly control the thickness of collagen fibers. However, the content of SLRP in tissues is extremely small and it is not easy to extract, so it is difficult to directly apply it to the preparation of artificial corneas. The star-shaped polymer used in this application can effectively replace SLRP, induce collagen to form a multilayer structure in vitro, and control the spacing of collagen fibers, the adhesion between fiber layers and the thickness of collagen fibers, so that a composite material with a layered fiber structure similar to that of a natural cornea can be prepared in an in vitro environment, thereby obtaining the superior physical and chemical properties of a natural cornea.

[0057] In some embodiments, the linear branches of the star polymer include at least one of polyethylene glycol (PEG), polyethylene glycol derivatives, polypropylene glycol (PPG), polypropylene glycol derivatives, polyacrylic acid (PAA), polyacrylic acid derivatives, polyvinyl alcohol (PVA), polyvinyl alcohol derivatives, polyethyleneimine (PEI), polyethyleneimine derivatives, and polypeptide chains (PP).

[0058] Star polymers are copolymers with three or more linear branches radially connected from a branch point. In terms of molecular structure, star polymers have branch points as cores and linear macromolecules (or functional small molecules) as arms. Generally speaking, the number of linear branches (arms) of star polymers is 3, 4, 6, 8 or more.

[0059] The star-shaped polymer provided in this specification has three or more linear branches (arms), for example, the linear branches of the star-shaped polymer may be, but are not limited to, 3, 4, 6, 8 or more.

[0060] In some embodiments, the linear branches of the star polymer can be PEG derivatives, for example, the PEG derivative can be at least one of polyethylene glycol, polyethylene glycol carboxyl, polyethylene glycol amino, polyethylene glycol active ester, polyethylene glycol maleimide, polyethylene glycol sulfhydryl, polyethylene glycol aldehyde, polyethylene glycol acrylate, polyethylene glycol methacrylate, polyethylene glycol isocyanate, polyethylene glycol lipoic acid, polyethylene glycol silane, polyethylene glycol biotin, polyethylene glycol pyridine, polyethylene glycol dopamine, etc.

[0061] When the star polymer has three linear branches, the star polymer can be three-arm polyethylene glycol (3-ARM-PEG-OH), three-arm polyethylene glycol methacrylate (3-ARM-PEG-MA), three-arm polyethylene glycol acrylate (3-ARM-PEG-AA), three-arm polyethylene glycol valeric acid (3-ARM-PEG-GAA), three-arm polyethylene glycol maleimide (3-ARM-PEG-MAL), three-arm polyethylene glycol carboxylic acid (3-ARM-PEG-COOH), three-arm polyethylene glycol amine (3-ARM-PEG-NH2), three-arm polyethylene glycol thiol (3-ARM-PEG-SH), three-arm polyethylene glycol propionaldehyde (3-ARM-PEG-CHO), three-arm polyethylene glycol isocyanate (3-ARM-PEG-NCO), three-arm polyethylene glycol succinimidyl succinate (3-ARM-PEG-SS) or at least one of the other three-branched star polymers.

[0062]

[0063]

[0064] When the number of linear branches of the star polymer is 4, the star polymer can be four-arm polyethylene glycol (4-ARM-PEG-OH), four-arm polyethylene glycol carboxyl (4-ARM-PEG-COOH), four-arm polyethylene glycol amino (4-ARM-PEG-NH2), four-arm polyethylene glycol active ester (4-ARM-PEG-NHS), four-arm polyethylene glycol maleimide (4-ARM-PEG-MAL), four-arm polyethylene glycol thiol (4-ARM-PEG-SH), four-arm polyethylene glycol aldehyde (4-ARM-PEG-CHO), four-arm polyethylene glycol acrylate ... The invention relates to a polymer having at least one of four branched chains: a four-arm polyethylene glycol methacrylate (4-ARM-PEG-MA), a four-arm polyethylene glycol isocyanate (4-ARM-PEG-NCO), a four-arm polyethylene glycol lipoic acid (4-ARM-PEG-LA), a four-arm polyethylene glycol silane (4-ARM-PEG-Silane), a four-arm polyethylene glycol biotin (4-ARM-PEG-Biotin), a four-arm polyethylene glycol pyridine (4-ARM-PEG-OPSS), a four-arm polyethylene glycol dopamine (4-ARM-PEG-DOPA) or other four-branched star polymers.

[0065]

[0066]

[0067] When the number of linear branches of the star-shaped polymer is 6, the star-shaped polymer can be six-arm polyethylene glycol (6-ARM-PEG-OH), six-arm polyethylene glycol carboxyl (6-ARM-PEG-COOH), six-arm polyethylene glycol amino (6-ARM-PEG-NH2), six-arm polyethylene glycol active ester (6-ARM-PEG-NHS), six-arm polyethylene glycol maleimide (6-ARM-PEG-MAL), six-arm polyethylene glycol thiol (6-ARM-PEG-SH), six-arm polyethylene glycol aldehyde (6-ARM-PEG-CHO), six-arm polyethylene glycol acrylate ... The invention relates to a six-arm polyethylene glycol methacrylate (6-ARM-PEG-MA), a six-arm polyethylene glycol isocyanate (6-ARM-PEG-NCO), a six-arm polyethylene glycol lipoic acid (6-ARM-PEG-LA), a six-arm polyethylene glycol silane (6-ARM-PEG-Silane), a six-arm polyethylene glycol biotin (6-ARM-PEG-Biotin), a six-arm polyethylene glycol pyridine (6-ARM-PEG-OPSS), a six-arm polyethylene glycol dopamine (6-ARM-PEG-DOPA) or at least one of other six-branched star polymers.

[0068]

[0069]

[0070]

[0071] When the number of linear branches of the star-shaped polymer is 8, the star-shaped polymer can be polyethylene glycol-cage polysilsesquioxane (PEG POSS Cage Mixture, referred to as POSS-PEG), eight-arm polyethylene glycol (8-ARM-PEG-OH), eight-arm polyethylene glycol carboxyl (8-ARM-PEG-COOH), eight-arm polyethylene glycol amino (8-ARM-PEG-NH2), eight-arm polyethylene glycol active ester (8-ARM-PEG-NHS), eight-arm polyethylene glycol maleimide (8-ARM-PEG-MAL), eight-arm polyethylene glycol thiol (8-ARM-PEG-SH), eight-arm polyethylene glycol aldehyde (8-ARM-PEG-CHO), eight-arm polyethylene glycol acrylate ... The invention relates to at least one of eight-arm polyethylene glycol methacrylate (8-ARM-PEG-MA), eight-arm polyethylene glycol isocyanate (8-ARM-PEG-NCO), eight-arm polyethylene glycol lipoic acid (8-ARM-PEG-LA), eight-arm polyethylene glycol silane (8-ARM-PEG-Silane), eight-arm polyethylene glycol biotin (8-ARM-PEG-Biotin), eight-arm polyethylene glycol pyridine (8-ARM-PEG-OPSS), eight-arm polyethylene glycol dopamine (8-ARM-PEG-DOPA) or other eight-branched star polymers.

[0072]

[0073]

[0074]

[0075] Polyethylene glycol (PEG) is a type of polymer that can absorb and retain a large amount of water. It has good biocompatibility, is non-toxic, has low immunogenicity, and can be excreted from the body through the human kidneys. Polyhedral oligomeric silsesquioxane (POSS) is a nanohybrid material at the molecular level. Its molecular size is between 1-3nm. It consists of an inorganic skeleton composed of Si-O-Si bonds in the core and an organic-inorganic hybrid structure composed of peripheral organic substituents. The peripheral organic substituents give POSS good molecular design. POSS has a great improvement in polymer toughness, thermal properties and mechanical properties. At the same time, POSS is non-toxic and tasteless and has good biocompatibility.

[0076] In some embodiments, the linear branches of the star polymer can also be polypropylene glycol, polypropylene glycol derivatives, polyacrylic acid, polyacrylic acid derivatives, polyvinyl alcohol, polyvinyl alcohol derivatives, polyethylene imine, polyethylene imine derivatives, polypeptide chains, etc.

[0077] PPG derivatives can be polymer compounds formed by polypropylene glycol and other functional groups (such as hydroxyl, methyl, carboxymethyl, glutamylamino, maleimide, carboxyl, amino, thiol, aldehyde, isocyanate, disulfide functional group, sulfhydryl, N-hydroxysuccinimide, acrylate, lipoic acid, silane, orthopyridyl disulfide, 3,4-dihydroxyphenylalanine, biotin, etc.). The types of other functional groups involved in PPG derivatives can be the same as the types of other functional groups involved in PEG derivatives. In addition, the number of linear side chains (arms) corresponding to PPG derivatives can also be 3, 4, 6, 8 or more.

[0078] Similarly, PVA derivatives can be polymer compounds formed by polyvinyl alcohol and other functional groups (such as hydroxyl, methyl, carboxymethyl, glutamylamino, maleimide, carboxyl, amino, thiol, aldehyde, isocyanate, disulfide functional group, sulfhydryl, N-hydroxysuccinimide, acrylate, lipoic acid, silane, orthopyridyl disulfide, 3,4-dihydroxyphenylalanine, biotin, etc.). The types of other functional groups involved in PPG derivatives can be the same as the types of other functional groups involved in PEG derivatives. In addition, the number of linear side chains (arms) corresponding to PVA derivatives can also be 3, 4, 6, 8 or more.

[0079] PAA derivatives can be polymer compounds formed by polyacrylic acid and other functional groups (such as hydroxyl, methyl, carboxymethyl, glutamylamino, maleimide, carboxyl, amino, thiol, aldehyde, isocyanate, disulfide functional group, sulfhydryl, N-hydroxysuccinimide, acrylate, lipoic acid, silane, orthopyridyl disulfide, 3,4-dihydroxyphenylalanine, biotin, etc.). The types of other functional groups involved in PPG derivatives can be the same as the types of other functional groups involved in PEG derivatives. In addition, the number of linear side chains (arms) corresponding to PAA derivatives can also be 3, 4, 6, 8 or more.

[0080] PEI derivatives can be polymer compounds formed by polyethyleneimine and other functional groups (such as hydroxyl, methyl, carboxymethyl, glutamylamino, maleimide, carboxyl, amino, thiol, aldehyde, isocyanate, disulfide functional group, sulfhydryl, N-hydroxysuccinimide, acrylate, lipoic acid, silane, orthopyridyl disulfide, 3,4-dihydroxyphenylalanine, biotin, etc.). The types of other functional groups involved in PPG derivatives can be the same as the types of other functional groups involved in PEG derivatives. In addition, the number of linear side chains (arms) corresponding to PEI derivatives can also be 3, 4, 6, 8 or more.

[0081] The structural formulas of the polymers involved in the polypropylene glycol derivatives, polyacrylic acid derivatives, polyvinyl alcohol derivatives, and polyethyleneimine derivatives are not described in detail here.

[0082] It is to be understood that the above star polymers can be used alone or in combination.

[0083] In addition, although the number of linear branches (arms) of star-shaped polymers is generally 3, 4, 6, 8 or more due to limitations of synthesis conditions and other factors, the number of linear branches (arms) of the star-shaped polymers provided in this specification is not limited to this, and star-shaped polymers with other numbers of linear branches (arms) are also included in the scope of the star-shaped polymers of this specification.

[0084] In some embodiments, the collagen includes at least one of type I collagen, type II collagen, type III collagen, type IV collagen, type V collagen, and type XI collagen. For example, the collagen can be type I collagen, type II collagen, type III collagen, type V collagen, type XI collagen, or any other suitable collagen type. The above different types of collagen can be mixed or used alone, with type I collagen being the main type of collagen.

[0085] It is understandable that the above-mentioned types of collagen are merely examples of the types of collagen in the composite materials provided in this specification, and do not limit the types of collagen in the composite materials provided in this specification.

[0086] In some embodiments, the relative molecular mass of the star polymer is between 10 3 -10 6The relative molecular mass of the star polymer depends on the molecular type of its support, the number of linear branches contained in the star polymer, the molecular chain length of the linear branches, the type of functional groups, etc. Different star polymers have different relative molecular masses. For example, the relative molecular mass of the star polymer can be 1000-10000, 10000-100000, 1000000-1000000. Specifically, the relative molecular mass of the star polymer can be 1000, 2000, 5000, 10000, 20000, 50000, 80000, 100000, 50000, 80000, 1000000 or a value between any two of the above values.

[0087] In the composite material provided in the present specification, compared with the case where the linear branches of the star-shaped polymer are small molecule compounds, when the linear branches of the star-shaped polymer are high-molecular-weight long-chain compounds, the intermolecular force between the star-shaped polymer and collagen is stronger, and the star-shaped polymer is more likely to cling to collagen, thereby improving the assembly efficiency of the collagen layered fiber structure.

[0088] In some embodiments, when the length of the linear side chain of the star polymer is 0.5-10 nm, it is more conducive to the star polymer to stably attach to collagen and regulate the thickness and arrangement of collagen fibers. For example, the length of the linear side chain of the star polymer can be 0.5 nm, 1.0 nm, 1.5 nm, 2.0 nm, 2.5 nm, 3.0 nm, 4.0 nm, 5.0 nm, 10.0 nm, or a value between any two of the above values.

[0089] In some embodiments, the content of the star-shaped polymer in the composite material may be significantly lower than the content of the collagen. For example, the mass ratio of the collagen and the star-shaped polymer in the composite material is 100:(0.1-20). In the composite material provided in this specification, a small amount of star-shaped polymer can cause the collagen to form a layered fiber structure. For example, according to the mass ratio, the mass ratio of the collagen and the star-shaped polymer in the composite material can be 100:0.1, 100:1, 50:1, 100:3, 25:1, 20:1, 50:3, 100:7, 25:2, 100:9, 10:1, 5:1 or a mass ratio between any two of the above ratios.

[0090] Different star polymers may have different types and numbers of linear branches, and star polymers with different types and / or linear branches have different intermolecular forces with collagen, and their ability to adhere to collagen is also different. Under the same other conditions, star polymers with linear branches that are high molecular long chain compounds can better adhere to collagen and induce it to form a layered fiber structure, compared with star polymers with linear branches that are small molecular compounds. At this time, a very small amount of star polymers can induce collagen to form a layered fiber structure.

[0091] Under the condition that other conditions are basically the same, the more linear side chains (arms) a star polymer contains, the more intermolecular forces it can have with more collagen, so as to attach to more collagen. Similarly, when the number of linear side chains contained in a star polymer increases, its dosage can be reduced, which is not only conducive to saving raw materials, but more importantly, the less the amount of exogenous substances added, the smaller the rejection reaction that may be caused in the body.

[0092] Furthermore, animal experiments have shown that the bionic structure of the composite material provided in this specification can promote epidermal cell migration, thereby promoting tissue regeneration and repair, and has good biocompatibility.

[0093] In some embodiments, the thickness of the composite material may be any value between 30 μm and 2000 μm. For example, the thickness of the composite material may be 30 μm, 50 μm, 100 μm, 200 μm, 250 μm, 300 μm, 400 μm, 450 μm, 500 μm, 520 μm, 550 μm, 1000 μm, 2000 μm, or a value between any two of the above thickness values.

[0094] In some embodiments, the composite material has a thickness of 400 μm-550 μm, which is close to the thickness of the corneal stroma of a human body (about 500 μm).

[0095] In some embodiments, the thickness of each layer of collagen in the composite material is between 0.1 μm and 10 μm, that is, the thickness of each layer of collagen in the composite material can be any value between 0.1 μm and 10 μm. For example, the thickness of each layer of collagen in the composite material can be 0.1 μm, 0.2 μm, 0.5 μm, 0.8 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, or a value between any two of the above values.

[0096] In some embodiments, the diameter of the collagen fiber is 5-100 nm, and the composite material containing collagen fibers in this diameter range can be suitable for repairing tissues such as cornea and bones. Specifically, the diameter of the collagen fiber can be any value between 5nm and 100nm. For example, the diameter of the collagen fiber can be 5nm, 10nm, 20nm, 25nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm or a value between any two of the above diameters.

[0097] The main methods for extracting collagen are acid hydrolysis and enzymatic hydrolysis. The acid method has a low yield of collagen extraction and can retain the collagen terminal peptide. The enzymatic method has a higher yield of collagen extraction, but at the same time, the enzymatic hydrolysis process will hydrolyze the terminal peptide of the collagen fibril protein and easily form collagen fibers with more uneven thickness. Experiments have found that the star-shaped polymer provided in this application has a regulating effect on the thickness of collagen fibers and can promote the orderly arrangement of collagen fibers. For collagen fibers with uneven thickness in the original state, under the induction of the star-shaped polymer, the collagen molecular structure can be reorganized to form collagen fibers with uniform thickness. Figure 2 A in the figure is a statistical diagram of the diameter of collagen fibers of collagen fibers without star-shaped polymers obtained according to the composite material preparation route of this specification. Figure 2 B in the figure is a statistical diagram of the diameter of collagen fibers of the star-shaped polymer-containing collagen fiber material obtained according to the composite material preparation route of this specification, Figure 2 A in Figure 2 The preparation method of the composite material B in is the same, the only difference is that Figure 2 In the preparation process of A, no star polymer is added. Figure 2 B in the above corresponds to the addition of a star polymer during the preparation process. Figure 2 A and Figure 2 As shown in B, compared with the collagen fiber size (35±8nm) of the collagen material without star-shaped polymer, the collagen fiber of the collagen material with star-shaped polymer is more uniform in thickness (23±6nm) and has a smaller diameter, which greatly improves the transparency of the collagen material.

[0098] In some embodiments, the composite material has a light transmittance greater than 70% at a wavelength of 550 nm.

[0099] The thickness of the stroma layer in the middle of the human cornea is about 0.5 mm, and the collagen fibers (diameter of about 30 nm) constituting the stroma layer are thin and highly oriented. The above structure of the stroma layer is of great significance to the optical properties of the cornea. As mentioned above, the thickness of the composite material provided in this specification can be close to the thickness of the stroma layer of the human cornea, the diameter of the collagen fibers can be similar to or even smaller than the diameter of the collagen fibers in the stroma layer of the human cornea, and the collagen fibers can form a layered oriented structure similar to the stroma layer of the human cornea. Figure 3 The transmittance test results of the composite materials of some embodiments and comparative examples of this specification at a wavelength of 550nm are shown in FIG. Figure 3 The experimental results show that the composite material provided in this specification has a high light transmittance, and its light transmittance is greater than 70% under the condition of a wavelength of 550nm. For example, the light transmittance of the composite material provided in this specification under the condition of a wavelength of 550nm can be 70.1%, 71%, 75%, 78%, 80%, 85%, 90%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100% or a value between any two of the above light transmittances.

[0100] In some embodiments, the composite material also includes: water molecules mixed in the collagen. The composite material provided in this specification has good water-containing properties. The water is mixed between the collagen fibers of the composite material to maintain the good tensile properties of the composite material itself. Experimental results show that the water content of the hydrated composite material provided in this specification is 50%-98%. For example, the transmittance of the composite material provided in this specification under the condition of a wavelength of 550nm can be 50.1%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 98% or a value between any two of the above water contents.

[0101] As mentioned above, the composite material provided in this specification includes collagen and star-shaped polymers, wherein the multiple linear branches of the star-shaped polymer can be combined with collagen through intermolecular forces, so that the multiple linear branches of the star-shaped polymer are attached to the collagen fibers, and the collagen fibers are controlled to form a multilayer structure, and in each layer, the collagen fibers extend in the same direction. The above-mentioned combination of collagen and star-shaped polymers makes the composite material have a layered fiber fine structure similar to that of a natural cornea, and the composite material has high light transmittance, good mechanical properties and biocompatibility. Therefore, the above-mentioned composite material provided in this specification can be applied to the preparation of a matrix for repairing biological tissues, and the matrix can be a matrix layer of the cornea, a bone matrix, and other matrix materials that can be used to repair biological tissues. That is, the composite material provided in this description can be applied to the preparation of artificial corneas or other biological tissues, and can be applied to organisms or their tissues as artificial organs.

[0102] It is understandable that due to its good light transmittance, mechanical properties and biocompatibility, the composite material provided in this specification can also be used to prepare materials for contact with biological tissues, such as the lens part of contact lenses.

[0103] The composite material provided in this specification can be used to manufacture artificial corneas. It is understandable that the artificial cornea may further include structures or tissues such as an epithelial layer, an elastic layer, and an endothelial layer.

[0104] Figure 4 The flowchart of the preparation method of the composite material provided in some embodiments of this specification is shown. Figure 5 The schematic diagram of the preparation route of the composite material provided in some embodiments of this specification is shown. For example, Figure 4 and Figure 5 As shown, this specification also provides a preparation method of a composite material, including the following steps:

[0105] Step S10, obtaining a collagen solution with a pH value less than 7; and obtaining a star-shaped polymer solution with a pH value greater than 7.

[0106] The pH value of the collagen solution can be adjusted by acidic substances (such as hydrochloric acid, acetic acid, etc.). The pH value of the collagen solution can be 0.1, 1, 2, 3, 4, 5, 6, 6.9 or a value between any two of the above pH values; or, the pH value of the collagen solution is x, and the value of x can be: 0 < x < 7.

[0107] In some embodiments, the temperature of the collagen solution is 2 - 8°C. For example, the temperature of the collagen solution can be 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, 8°C or a value between any two of the above temperature values.

[0108] The pH value of the star-shaped polymer solution can be any value greater than 7. The pH value of the star-shaped polymer solution can be 7.1, 8, 9, 10, 11, 12, 13, 14 or a value between any two of the above pH values. Or, the pH value of the collagen solution is y, and the value of y can be: 7 < y ≤ 14. For example, the star-shaped polymer solution uses a pH buffer as a solvent, and the pH buffer is at least one of a phosphate buffer, an amino acid buffer, a citrate buffer, a carbonate buffer, an acetate buffer, a barbituric acid buffer, a cell culture medium buffer, a 4-(2-hydroxyethyl)-1-piperazineethanesulfonic acid buffer, and a tris(hydroxymethyl)aminomethane hydrochloride buffer. The star-shaped polymer solution can be prepared in a buffer system.

[0109] In some embodiments, the pH value of the star-shaped polymer solution can be adjusted by alkaline substances (such as sodium hydroxide, potassium hydroxide, etc.).

[0110] In some embodiments, the star polymer solution uses a pH buffer as a solvent, wherein the pH buffer can be a hypotonic solution with an osmotic pressure of 5-260 milliosm / liter. For example, the osmotic pressure of the pH buffer can be 5 milliosm / liter, 10 milliosm / liter, 20 milliosm / liter, 50 milliosm / liter, 100 milliosm / liter, 150 milliosm / liter, 200 milliosm / liter, 250 milliosm / liter, 260 milliosm / liter, or a value between any two of the above osmotic pressure values. The osmotic pressure range of normal plasma is 280-310 milliosm / liter, and a solution within the normal plasma osmotic pressure range can be referred to as an isotonic solution, a solution lower than the normal plasma osmotic pressure range is referred to as a hypotonic solution, and a solution higher than the normal plasma osmotic pressure range is referred to as a hypertonic solution. In the embodiment of the present application, a pH buffer lower than the normal plasma osmotic pressure range is used, and the formation of thicker fibers of collagen can be suppressed during the preparation of the composite material, thereby helping to regulate the diameter of the collagen fibers, so that the generated collagen fibers have a smaller diameter.

[0111] Furthermore, the applicant has found through a large number of experiments that, under the same other conditions, the fiber diameter of collagen fibers can increase with the increase of the osmotic pressure of the solution. Figure 6 The diameter of the collagen fibers of the composite materials of some embodiments of this specification under different osmotic pressure conditions are shown in FIG. Figure 6 As shown, as the osmotic pressure of the pH buffer solution gradually increases, the diameter of the corresponding prepared collagen fibers increases.

[0112] In some embodiments, the concentration of collagen in the collagen solution is 1-10 mg / mL; and the concentration of the star polymer in the star polymer solution is 0.01-2.0 mg / mL. For example, in the collagen solution, the concentration of collagen can be 1 mg / mL, 2 mg / mL, 3 mg / mL, 4 mg / mL, 5 mg / mL, 6 mg / mL, 7 mg / mL, 8 mg / mL, 9 mg / mL, 10 mg / mL or a value between any two of the above concentration values. In the star polymer solution, the concentration of the star polymer can be 0.01 mg / mL, 0.05 mg / mL, 0.1 mg / mL, 0.15 mg / mL, 0.20 mg / mL, 0.25 mg / mL, 0.30 mg / mL, 0.35 mg / mL, 0.4 mg / mL, 0.5 mg / mL, 1.0 mg / mL, 2.0 mg / mL or a value between any two of the above temperature values.

[0113] Step S20, mixing the collagen solution and the star-shaped polymer solution to obtain a mixed solution;

[0114] The preparation of the mixed solution can be carried out at 2° C.-10° C. For example, the preparation of the mixed solution can be carried out at 2° C., 3° ​​C., 4° C., 5° C., 6° C., 7° C., 8° C., 9° C., 10° C. or a temperature between any two of the above temperatures.

[0115] Figure 7 : shows a cryo-electron microscopy photograph of a mixed solution of collagen and star-shaped polymers provided according to some embodiments of this specification, wherein the scale bar is 50 nm. Figure 7 As shown, after the collagen solution and the star-shaped polymer solution are mixed, the star-shaped polymer (the darker dots in the figure) can be clearly seen in the resulting mixed solution clinging to the procollagen (the thin and lighter lines in the figure) in the collagen solution.

[0116] It is understandable that during the preparation of the mixed solution, the volume ratio of the collagen solution to the star-shaped polymer solution needs to be reasonably adjusted according to the concentrations of the collagen solution and the star-shaped polymer solution.

[0117] In some embodiments, equal volumes of the collagen solution and the star polymer solution are mixed.

[0118] In some embodiments, the mixed solution also includes a growth factor. For example, the growth factor can be a growth factor or other type of growth factor that can promote corneal repair. The growth factor that can promote corneal repair can be at least one of epidermal growth factor (EGF), fibroblast growth factor (FGF), and transforming growth factor (TGF). The other types of growth factors can be at least one of platelet-derived growth factor (PDGF), human insulin-like growth factor (IGF), hepatocyte growth factor (HGF), bone morphogenetic protein (BMP), and vascular endothelial growth factor (VEGF). In the mixed solution provided in this specification, epidermal growth factor (EGF), fibroblast growth factor (FGF), transforming growth factor (TGF), platelet-derived growth factor (PDGF), human insulin-like growth factor (IGF), hepatocyte growth factor (HGF), bone morphogenetic protein (BMP) and vascular endothelial growth factor (VEGF) can be added separately or mixed.

[0119] Step S30, subjecting the mixed solution to gelation, temperature-controlled and humidity-controlled drying treatments in sequence to obtain the composite material.

[0120] Incubation refers to placing the mixed solution under preset conditions for a preset time, waiting for the chemical substances in the mixed solution to complete the physical and chemical reaction according to their own generation rules. The gelation and temperature-controlled and humidity-controlled drying process is a slow dehydration process carried out at a certain temperature and a certain humidity. The process of gelation, temperature-controlled and humidity-controlled drying of the mixed solution in this step is equivalent to the incubation process of the mixed solution. During the gelation process, part of the collagen begins to fibrosis and self-assemble. Afterwards, during the temperature-controlled and humidity-controlled drying process, the collagen slowly begins to form a layered fiber structure with a complete orientation. This process simulates the development process of the human cornea, so that the collagen has enough time to self-assemble under the induction of the star-shaped polymer, and gradually forms an ordered and dense layered fiber structure, thereby realizing the in vitro reconstruction of the unique layered fiber fine structure of collagen in the cornea, and obtaining a composite material with similar superior performance to the human cornea.

[0121] During the temperature and humidity controlled drying process, the gelled solution in contact with the air first begins to form a layered fiber structure, and then forms a dense layered fiber structure layer by layer from the outside to the inside, until the gelled solution is completely formed into a layered fiber structure, thereby obtaining a composite material. The extension directions of the collagen in adjacent layers of the composite material are different.

[0122] Specifically, step S30 may include:

[0123] Step S31, gelation treatment: incubating the mixed solution at a first preset temperature for a first preset time to form a gelled mixed solution;

[0124] In some embodiments, the first preset temperature may be between 10°C and 50°C. For example, the first preset temperature may be 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, or a temperature between any two of the above temperatures. The first preset time may be between 1-4 hours. For example, the first preset time may be 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 4 hours, or a value between any two of the above values.

[0125] In some embodiments, the mixed solution is placed in a cell culture incubator for gelation, and the carbon dioxide concentration in the cell culture incubator may be between 2% and 10%.

[0126] Step S32, temperature-controlled and humidity-controlled drying treatment: incubating the mixed solution at a second preset temperature for a second preset time to form a composite material with a layered fiber structure.

[0127] In some embodiments, the second preset temperature may be between 1° C. and 50° C. For example, the second preset temperature may be 1° C., 10° C., 20° C., 30° C., 40° C., 50° C., or a temperature between any two of the above temperatures.

[0128] The humidity of the temperature-controlled and humidity-controlled drying process can be between 10% and 90%. For example, the humidity of the temperature-controlled and humidity-controlled drying process can be 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90% or a value between any two of the above humidity levels.

[0129] The second preset time may be between 10 hours and 30 days. For example, the second preset time may be 10 hours, 1 day, 2 days, 3 days, 7 days, 10 days, 20 days, 30 days, or a value between any two of the above values.

[0130] It is found in experiments that the time of temperature-controlled and humidity-controlled drying of the composite material in this specification is related to the thickness of the composite material. Since the thickness of the composite material is related to the drying environment of the mixed liquid (including the size, depth and shape of the container containing the mixed liquid), the drying environment of the mixed liquid has a greater impact on the temperature-controlled and humidity-controlled drying time.

[0131] Figure 8 A in Figure 8 B and Figure 8 C in FIG. 1 respectively show cross-sectional photographs of composite materials provided according to some embodiments of the present specification under a transmission electron microscope (TEM), wherein: Figure 8 The scale bar in A is 0.5 μm. Figure 8 B and Figure 8 The scale bar in C is 2 μm. Figure 8 A- Figure 8 As shown in C, the cross-sectional structure of the composite material presents a layered structure with clear dividing lines between the layers. Different collagen layers have different brightness under an electron microscope, while the brightness of the collagen in the same layer is similar. This indicates that the extension direction of the collagen fibers in each layer is roughly the same, which is different from the extension direction of the collagen fibers in another adjacent layer, which is visually similar to the texture of muscle fibers or the texture of wood after being split along the trunk direction.

[0132] In some embodiments, the method for preparing a composite material may further include step S40: placing the composite material in water for hydration treatment.

[0133] As mentioned above, the preparation process of the composite material needs to go through gelation, temperature control, humidity control and drying. On the one hand, the above process can make the composite material form an ordered and dense layered fiber structure; on the other hand, the above process can remove most of the water, which is beneficial to the storage and transportation of the composite material. When practical application is required, the composite material can be hydrated, that is, the composite material is immersed in water. This process allows water molecules to enter the gaps between the collagen fibers of the composite material, which is convenient for subsequent application. It should be noted that some star-shaped polymers can be washed out of the composite material during the hydration process, which will not affect the layered fiber structure of the composite material.

[0134] In some embodiments, the hydration treatment time may be between 0.1-72 hours. For example, the hydration treatment time may be 0.1 hours, 0.5 hours, 2 hours, 5 hours, 10 hours, 14 hours, 20 hours, 24 hours, 48 ​​hours, 72 hours, or any two of the above values ​​and values ​​therebetween.

[0135] The following is a detailed description with reference to specific examples. The reagents and instruments used in the examples are conventionally selected in the art unless otherwise specified. The experimental methods without specific conditions in the examples are carried out according to conventional conditions, such as those described in literature or books or methods recommended by manufacturers.

[0136] It should be clear that the following examples are only for illustrating the composite material / artificial cornea material and one or several methods for preparing the composite material / artificial cornea material described above. Those skilled in the art can prepare the composite material / artificial cornea material by simply changing the parameters used in each step and material according to this specification without departing from the spirit of this application.

[0137] The methods used for performance testing of the embodiments and comparative examples of this specification are the same.

[0138] 1. Transparency test conditions: The transparency of the collagen membrane sample was tested using an ELISA reader (BioTek) at a wavelength of 550 nm.

[0139] 2. Mechanical properties test conditions: The collagen membrane samples were cut into rectangular tensile test strips for tensile testing. The collagen membrane material was loaded onto the Electro Force 3200 mechanical tester (TAInstruments) and stretched at a speed of 0.05 mm / s until it broke. The load and displacement values ​​were obtained, and the fracture strain was recorded using the supporting software. The Young's modulus value and elongation at break were obtained by analyzing the stress-strain curve. The suture retention (SRS) of the collagen membrane was measured using an ElectroForce 3200 mechanical tester (TA Instruments) and 10-0 nylon suture. The test was performed at an extension rate of 0.05 mm / s at room temperature with a load cell of 22.2 N. The suture was passed through the center of the specimen. The sample was clamped in the upper clamp and the suture was tied to the lower clamp. The peak load force (N) required to displace the suture from the specimen was measured, and the suture retention (SRS) was calculated after thickness normalization.

[0140] 3. Experimental conditions for culturing primary corneal epithelial cells on collagen materials:

[0141] After sterilization, the rabbit corneal epithelial tissue was cut into 1mm×1mm small pieces and implanted on different collagen materials. The cells were cultured in 6-well plates using epithelial cell culture medium to observe the differentiation of limbal stem cells in the corneal epithelial tissue into epithelial cells and their migration to the collagen materials. After 7 days of culture, the corneal epithelial cells implanted on different collagen materials were stained with zonula occludens-1 (ZO-1) and DAPI for immunofluorescence analysis.

[0142] 4. Experimental conditions for culturing primary corneal stromal cells on collagen materials:

[0143] The excised cornea was cut into small pieces and digested with 3 mg / ml collagenase type II at 37°C and 5% CO2 for 30 minutes with mechanical shaking. The corneal fragments were filtered through a 70 μm cell strainer and then digested with 3 mg / ml collagenase type II for 60 minutes. The corneal stromal cells in the filtrate were collected. 2 Corneal stromal cell suspensions were seeded in 6-well plates on different collagen substrates. After 4 days of culture, Live / Dead reagent (containing Calcein AM and Propidium Iodide) was added to stain live and dead cells.

[0144] Example 1

[0145] The preparation method of the composite material of this embodiment comprises the following steps:

[0146] (1) Mixing equal volumes of a collagen solution (5 mg / mL) and a star polymer hypotonic solution (0.25 mg / mL, osmotic pressure 20-200 mOsm / L) at 2-8° C. to obtain a mixed solution;

[0147] (2) transferring the mixed solution to a cell culture incubator (temperature of 10° C. to 50° C., CO 2 concentration of 2% to 10%) and incubating for 2-4 hours to obtain a gelled mixed solution;

[0148] (3) transferring the gelled mixed solution to a constant temperature and humidity chamber (temperature of 1° C. to 50° C., humidity of 10% to 90%) and incubating for 1 day to 14 days to obtain a temperature-controlled and humidity-controlled drying composite material;

[0149] (4) Hydrate the dried composite material (temperature 10° C. to 45° C., humidity 20% to 80%) for 0.1 h to 72 h to obtain a composite material.

[0150] This embodiment uses a star polymer with 8 linear branches, selected from any one of 8-ARM-PEG-OH, 8-ARM-PEG-NH2, 8-ARM-PEG-SH, 8-ARM-PEG-NHS, 8-ARM-PEG-COOH, 8-ARM-PAA-COOH, and POSS-PEG.

[0151] The cross-sectional photograph of the composite material prepared using 8-ARM-PEG-OH under a transmission electron microscope (TEM) is shown in FIG. Figure 8 As shown in A. Figure 8 From A in the figure, it can be seen that there is an obvious dividing line in the composite material, which means that the composite material has multiple layered structures and the extension directions of the collagen fibers in the two adjacent layers are different. In addition, compared with the collagen material prepared with isotonic pH buffer, the collagen fibers in the composite material are thinner, with a diameter of about 10nm to 30nm.

[0152] In this embodiment, the transmittance test results of the composite materials prepared by using different star polymers are as follows: Figure 3 shown. Figure 3 In the composite material, the star polymers with 8 linear branches include 8-ARM-PEG-OH, 8-ARM-PAA-COOH, and POSS-PEG. Compared with the collagen membrane prepared by isotonic pH buffer (transmittance of about 40%), these composite materials show superior transmittance, all greater than 70%.

[0153] Fig. 9 The Young's modulus value obtained by the stress-strain curve in the tensile mechanical property test of the composite material (composite collagen membrane) of this embodiment is shown. Fig. 9It can be seen that, compared with the collagen membrane prepared by using isotonic pH buffer solution, the Young's modulus of the composite material of this embodiment is significantly reduced and is closer to the natural cornea.

[0154] Fig.10 The elongation at break value obtained by the stress-strain curve in the tensile mechanical property test of the composite material (composite collagen membrane) of this embodiment is shown. Fig.10 It can be seen that, compared with the collagen membrane prepared by using isotonic pH buffer solution, the elongation at break of the composite material of this embodiment is significantly increased, and is closer to the natural cornea.

[0155] Fig.11 The suture retention strength (SRS) value of the composite material (composite collagen membrane) suture mechanical test of this embodiment is shown. Fig.11 It can be seen that compared with the collagen membrane prepared by isotonic pH buffer in Comparative Example 2, the suture mechanical strength of the composite material of this embodiment is significantly increased, thereby enhancing the sutureability of corneal transplantation surgery.

[0156] Fig.12 The experimental results of culturing primary corneal epithelial cells on the composite material of this embodiment are shown, wherein the scale bar is 20 μm. Fig.12 It can be seen that the primary corneal epithelial cells cultured on the composite material of this example have high activity and high expression of tight junction protein ZO-1 (intercellular fluorescence staining), indicating that the composite material has good biocompatibility.

[0157] Fig.13 The experimental results of culturing primary corneal stromal cells on the composite material of this embodiment are shown, wherein the scale bar is 200 μm. Fig.13 It can be seen that the primary corneal stromal cells cultured on the composite material of this example have high activity, indicating that the composite material has good biocompatibility.

[0158] Fig.14 The figure shows a live experiment of transplanting the anterior corneal lamella of a rabbit using the composite material of this embodiment. Fig.14 It can be seen that in the in vivo experiment of rabbit corneal anterior lamella transplantation, the composite material of this embodiment has good suturing properties and can be directly sutured to the cornea for artificial corneal transplantation surgery.

[0159] Example 2

[0160] The preparation method of the composite material of this embodiment is basically the same as that of Example 1, except that: in this embodiment, a star-shaped polymer with 6 linear branches is used, and in the process of preparing the mixed solution in step (2) of this embodiment, a collagen solution with a concentration of 1 mg / mL is mixed with equal volumes of a solution containing 0.05 μg / mL epidermal growth factor (EGF) solution and 0.01 mg / mL star-shaped polymer.

[0161] The star polymer with 6 linear branches used in this embodiment is selected from any one of 6-ARM-PEG-OH, 6-ARM-PEG-NH2, 6-ARM-PEG-SH, 6-ARM-PEG-MA, 6-ARM-PEG-CHO, 6-ARM-PEG-NHS, and 6-ARM-PEG-COOH.

[0162] The cross-sectional photograph of the composite material prepared using 6-ARM-PEG-MA under transmission electron microscopy (TEM) is shown in the figure. Figure 8 As shown in B. Figure 8 From B in the figure, it can be seen that there is an obvious dividing line in the composite material, which means that the composite material has multiple layered structures and the extension directions of the collagen fibers in the two adjacent layers are different. In addition, compared with the collagen material prepared with isotonic pH buffer, the collagen fibers in the composite material are thinner, with a diameter of about 10nm to 30nm.

[0163] In this embodiment, the transmittance test results of the composite materials prepared by using different star polymers are as follows: Figure 3 shown. Figure 3 In the composite material, the star polymer with 6 linear branches is 6-ARM-PEG-MA. Compared with the collagen membrane prepared by isotonic pH buffer (transmittance is about 40%), the composite material of this embodiment shows excellent transmittance, which is greater than 70%.

[0164] Example 3

[0165] The preparation method of the composite material of this embodiment is basically the same as that of Example 1, except that: in this embodiment, a star-shaped polymer with 4 linear branches is used, and in the process of preparing the mixed solution in step (2) of this embodiment, a collagen solution with a concentration of 5 mg / mL is mixed with a solution containing 50 μg / mL epidermal growth factor (EGF), 50 μg / mL fibroblast growth factor (FGF) and 2 mg / mL star-shaped polymer in a volume ratio of 2:1.

[0166] The star polymer with 4 linear branches used in this embodiment is selected from any one of 4-ARM-PVA-OH, 6-ARM-PEI-NH2, 4-ARM-PEG-SH, 4-ARM-PEG-MA, 4-ARM-PEG-CHO, 4-ARM-PEG-OPSS, and 4-ARM-PEG-COOH.

[0167] The cross-sectional photograph of the composite material prepared using 4-ARM-PVA-OH under a transmission electron microscope (TEM) is shown in FIG. Figure 8 As shown in C. Figure 8From the C in the figure, it can be seen that there is an obvious dividing line in the composite material, which means that the composite material has multiple layered structures and the extension directions of the collagen fibers in the two adjacent layers are different. In addition, compared with the collagen material prepared with isotonic pH buffer, the collagen fibers in the composite material are thinner, with a diameter of about 10nm to 30nm.

[0168] In this embodiment, the transmittance test results of the composite materials prepared by using different star polymers are as follows: Figure 3 shown. Figure 3 In the composite material, the star polymers with 4 linear branches include 4-ARM-PVA-OH, 6-ARM-PEI-NH2, 4-ARM-PEG-CHO, and 4-ARM-PEG-OPSS. Compared with the collagen membrane prepared by isotonic pH buffer (transmittance of about 40%), these composite materials show superior transmittance, which is greater than 70%.

[0169] Example 4

[0170] The preparation method of the composite material of this embodiment is basically the same as that of Example 1, except that: in this embodiment, a star-shaped polymer with 3 linear branches is used, and in the process of preparing the mixed solution in step (2) of this embodiment, a collagen solution with a concentration of 10 mg / mL and a star-shaped polymer solution with a concentration of 1 mg / mL are mixed in a volume ratio of 1:2.

[0171] The star polymer with 3 linear branches used in this embodiment is selected from any one of 3-ARM-PPG-SH, 3-ARM-PEG-NCO, 3-ARM-PEG-LA, 3-ARM-PEG-Silane, 3-ARM-PEG-Biotin, and 3-ARM-PEG-DOPA.

[0172] In this embodiment, the transmittance test results of the composite materials prepared by using different star polymers are as follows: Figure 3 shown. Figure 3 In the composite material, the star polymer with 3 linear branches is 3-ARM-PPG-SH. Compared with the collagen membrane prepared by isotonic pH buffer (transmittance is about 40%), the composite material of this embodiment shows excellent transmittance, which is greater than 70%.

[0173] Comparative Example 1

[0174] The preparation method of the composite material of this comparative example is basically the same as that of Example 1, except that no star-shaped polymer is added in this comparative example.

[0175] Fig.15The figure shows a cross-sectional photograph of a material obtained according to the composite material preparation route provided in this specification under a transmission electron microscope (TEM) without adding a star polymer, wherein the scale bar is 0.2 μm. Fig.15 As shown, it can be clearly seen that without adding the star polymer, the collagen fibers in the material obtained according to the composite material preparation route provided in this specification are in a disordered state.

[0176] In this comparative example, the light transmittance test results of the material prepared without adding the star polymer are as follows: Figure 3 As shown, the light transmittance of the material prepared in this comparative example without adding the star-shaped polymer is about 60% under the condition of wavelength of 550nm.

[0177] Fig. 9 The Young's modulus value obtained by the stress-strain curve in the tensile mechanical property test of the collagen material of this comparative example is shown. Fig. 9 It can be seen that the Young's modulus of the composite material prepared in this comparative example without adding the star-shaped polymer is significantly higher than the Young's modulus of the natural cornea.

[0178] Fig.10 The elongation at break value obtained by the stress-strain curve in the tensile mechanical property test of the collagen material of this comparative example is shown. Fig.10 It can be seen that the elongation at break of the composite material prepared in this comparative example is lower than that of the composite material prepared in Example 1.

[0179] Fig.11 The suture retention strength (SRS) value of the suture mechanical test of the collagen material of this comparative example is shown. Fig.11 It can be seen that the suture mechanical strength of the composite material prepared in this comparative example is lower than that of Example 1, which reduces the sutureability of corneal transplant surgery to a certain extent.

[0180] By comparing Example 1 with Comparative Example 1, it can be seen that after adding the star-shaped polymer in Example 1 of this specification, the transparency of the corresponding composite material prepared is significantly improved, the Young's modulus value is closer to the natural cornea, the elongation at break value is closer to the natural cornea, and the suture holding force value is greater. This is attributed to the fact that the collagen fibers are arranged in a more orderly manner under the influence of the star-shaped polymer. At the same time, the collagen fibers are more uniform in thickness and smaller in diameter.

[0181] Comparative Example 2

[0182] The preparation method of the composite material of this comparative example is basically the same as that of Example 1, except that: in this comparative example, no star polymer is added, and an isotonic pH buffer solution with an osmotic pressure of 290 mOsm / L is used.

[0183] Fig.16The cross-sectional photograph of the collagen material of this comparative example under a transmission electron microscope (TEM) is shown, wherein the scale bar is 0.2 μm. Fig.16 As shown, it can be clearly seen that in the collagen material of this comparative example, the collagen fibers have a larger diameter and are in a disordered state.

[0184] The light transmittance test results of the collagen material in this comparative example are as follows: Figure 3 As shown, the light transmittance of the material prepared in this comparative example without adding the star-shaped polymer at a wavelength of 550 nm is about 40%.

[0185] Fig. 9 The Young's modulus value obtained by the stress-strain curve in the tensile mechanical property test of the collagen material of this comparative example is shown. Fig. 9 It can be seen that the Young's modulus of the composite material prepared in this comparative example without adding the star polymer and using an isotonic pH buffer solution is significantly different from the Young's modulus of the natural cornea.

[0186] Fig.10 The elongation at break value obtained by the stress-strain curve in the tensile mechanical property test of the collagen material of this comparative example is shown. Fig.10 It can be seen that the elongation at break of the composite material prepared in this comparative example is significantly lower than the elongation at break of the composite material prepared in Example 1 and the natural cornea.

[0187] Fig.11 The suture retention strength (SRS) value of the suture mechanical test of the collagen material of this comparative example is shown. Fig.11 It can be seen that the suture mechanical strength of the composite material prepared in this comparative example is significantly lower than that of Example 1. Accordingly, the sutureability of corneal transplantation surgery using the composite material of this comparative example will also be significantly reduced.

[0188] Compared with Comparative Example 1, the transparency of the composite material prepared in Comparative Example 2 is significantly lower, the Young's modulus value is larger, the elongation at break value is smaller, and the suture retention value is smaller. This is attributed to the fact that the collagen fibers are affected by the osmotic pressure of the solution, and the diameter of the collagen fibers prepared by the isotonic solution is larger than that of the hypotonic solution.

[0189] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0190] The above-described embodiments only express several embodiments of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. It should be understood that, on the basis of the technical solutions provided by the technical personnel in the present application, the technical solutions obtained through logical analysis, reasoning or limited experiments are all within the protection scope of the claims attached to the present application. Therefore, the protection scope of the patent of the present application shall be based on the attached claims, and the specification and drawings may be used to interpret the contents of the claims.

Claims

1. A composite material with collagen as a matrix, characterized in that: include: Collagen, wherein the collagen comprises multiple layers of collagen fibers, and each layer of collagen fibers comprises multiple collagen fibers extending in substantially the same direction; as well as Star-shaped polymers present in the collagen.

2. The composite material according to claim 1, characterized in that The extending direction of the collagen fibers in each layer is different from the extending direction of the collagen fibers in another adjacent layer.

3. The composite material according to claim 1, characterized in that The multi-layered collagen fibers are formed under the induction of the star-shaped polymer.

4. The composite material according to claim 1, characterized in that The linear branches of the star polymer include at least one of polyethylene glycol, polyethylene glycol derivatives, polypropylene glycol, polypropylene glycol derivatives, polyacrylic acid, polyacrylic acid derivatives, polyvinyl alcohol, polyvinyl alcohol derivatives, polyethylene imine, polyethylene imine derivatives, and polypeptide chains.

5. The composite material according to claim 1, characterized in that The relative molecular mass of the star polymer is between 10 3 ~10 6 between.

6. The composite material according to claim 1, characterized in that The collagen includes at least one of type I collagen, type II collagen, type III collagen, type IV collagen, type V collagen and type XI collagen.

7. The composite material according to claim 1, characterized in that The mass ratio of the collagen to the star-shaped polymer is 100:(0.1-20).

8. The composite material according to claim 1, characterized in that The composite material has a thickness of 30 μm to 2000 μm.

9. The composite material according to claim 1, characterized in that The thickness of each layer of collagen in the composite material is 0.1 μm to 10 μm.

10. The composite material according to claim 1, characterized in that The diameter of the collagen fiber is 5-100 nm.

11. The composite material according to claim 1, characterized in that The composite material has a light transmittance of more than 70% at a wavelength of 550 nm.

12. The composite material according to claim 1, characterized in that The composite material also includes: water, which is mixed in the collagen.

13. Use of the composite material according to any one of claims 1 to 12 in preparing a matrix for repairing biological tissues.

14. An artificial cornea, characterized in that: The artificial cornea is prepared using the composite material according to any one of claims 1 to 12.

15. A method for preparing a composite material, characterized in that: The following steps are involved: obtaining a collagen solution with a pH value less than 7, and obtaining a star polymer solution with a pH value greater than 7; mixing the collagen solution and the star-shaped polymer solution to obtain a mixed solution; and The mixed solution is sequentially subjected to gelation and temperature-controlled and humidity-controlled drying to obtain the composite material as claimed in any one of claims 1 to 12.

16. The preparation method according to claim 15, characterized in that: The concentration of collagen in the collagen solution is 1 mg / mL to 10 mg / mL; and The concentration of the star-shaped polymer in the star-shaped polymer solution is 0.01 mg / mL to 2.0 mg / mL.

17. The preparation method according to claim 15, characterized in that: The star polymer solution uses a pH buffer as a solvent, and the pH buffer is at least one of a phosphate buffer, an amino acid buffer, a citric acid buffer, a carbonate buffer, an acetate buffer, a barbituric acid buffer, a cell culture medium buffer, a 4-hydroxyethylpiperazineethanesulfonic acid buffer, and a tris(hydroxymethyl)aminomethane hydrochloride buffer.

18. The preparation method according to claim 15, characterized in that: The star polymer solution uses a hypotonic pH buffer as a solvent, and the osmotic pressure of the pH buffer is 5 to 260 milliosm / L.

19. The preparation method according to claim 15, characterized in that: The mixed solution also includes growth factors, which are at least one of epidermal growth factor, fibroblast growth factor, platelet-derived growth factor, human insulin-like growth factor, hepatocyte growth factor, bone morphogenetic protein, transforming growth factor, and vascular endothelial growth factor.

20. The preparation method according to claim 15, characterized in that: Also includes: The composite material is subjected to a hydration treatment.