Coal slime-based fire preventing and extinguishing material for inhibiting spontaneous combustion of coal and preparation method thereof

Through the composite of konjac glucomannan and other materials with modified coal slime, gels are formed, which solves the problems of coal mine fire and waste treatment, realizes the inhibition of coal spontaneous combustion and resource utilization, and improves the mechanical properties and biological properties of coal slime. Degradability.

CN118987555APending Publication Date: 2024-11-22ZAOZHUANG MINING GRP GAOZHUANG COAL IND CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411150294.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Coal mine fires and coal waste treatment problems, and the existing technology is difficult to effectively curb coal spontaneous combustion and resource utilization, affecting the mining environment and safety.

Method used

The modified coal slime is used to combine materials such as konjac glucomannan, acrylic acid, polyacrylamide, potassium thiosulfate and ammonium persulfate to form a gel for underground fire prevention and waste disposal.

Benefits of technology

The resource utilization of coal mine waste and the inhibition of coal spontaneous combustion have been achieved, the coal slime piled up around the mines have been effectively disposed of, filling the goaf area, and improving the mechanical properties and biodegradability of coal slime.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118987555A_ABST
    Figure CN118987555A_ABST
Patent Text Reader

Abstract

The invention discloses a coal slime-based fire preventing and extinguishing material for inhibiting spontaneous combustion of coal and a preparation method thereof, and the coal slime-based fire preventing and extinguishing material comprises the following components by mass: 0.6%-1% of konjac glucomannan, 2%-5% of modified coal slime, 5%-10% of acrylic acid, 3%-5% of polyacrylamide, 0.015%-0.04% of potassium thiosulfate, 0.02%-0.05% of ammonium persulfate, 0.2%-0.4% of N, N-dimethylformamide, and the balance of water. N, N-methylene bisacrylamide and the balance of water. In the preparation process, konjac glucomannan is used as a matrix and is subjected to graft copolymerization with acrylic acid and acrylamide, modified coal slime is used as a filling material to form physical crosslinking with colloid, and the coal slurry-based gel is obtained through compounding. The coal slurry-based fire preventing and extinguishing material prepared by the invention realizes resource utilization of coal mine wastes while inhibiting spontaneous combustion of coal, and provides a new thought for the field of fire preventing and extinguishing of coal mines.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to underground fire prevention and control, and in particular to a coal slime-based fire prevention and extinguishing material for inhibiting coal spontaneous combustion and a preparation method thereof. Background Art

[0002] Coal mine fire is a common and serious safety hazard in the coal mining process. It not only threatens the lives of miners, but also seriously hinders the sustainable development of coal resources. Although many technologies have been used to prevent and control coal mine fires, due to the influence of complex factors such as the characteristics of coal, the geological conditions of coal mines, and the mine environment, coal mine fire prevention and extinguishing is still a very challenging problem. For this reason, it is particularly important to research and develop new and efficient coal mine fire prevention and extinguishing materials.

[0003] At the same time, the waste problem generated in the coal mining process is becoming increasingly serious. These wastes include abandoned ore, coal gangue, coal slime, etc., which have a serious impact on the environment and human health. How to effectively treat and utilize these wastes to achieve resource recycling and sustainable development of the environment is also an important topic of current research.

[0004] In recent years, due to the continuous increase in coal mining volume and the downturn in the coal market, the amount of byproduct coal slime has increased. At present, the research on coal slime resource utilization technology has been slow, resulting in coal slime being piled up on the surface for a long time, making it difficult to dispose of it efficiently, which has seriously affected the ecological environment around the mining area and the construction of green mines. Therefore, taking advantage of the strong water retention and high viscosity of coal slime itself, the coal slime slurry is compounded with the cementitious material, and the compounded product is poured into the underground goaf for fire extinguishing. This process can not only effectively dispose of a large amount of waste coal slime piled up around the mine, but also fill the goaf, realizing the resource utilization of coal mine waste and the suppression of coal spontaneous combustion. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a coal slime-based fire extinguishing material and a preparation method for inhibiting coal spontaneous combustion. The modified coal slime is compounded with a gel to form a gel and improve its mechanical properties, thereby realizing the resource utilization of coal mine waste and the inhibition of coal spontaneous combustion.

[0006] In order to solve the above technical problems, the solution of the present invention includes:

[0007] 1. A coal slime-based fire extinguishing material for inhibiting spontaneous combustion of coal and a preparation method thereof, which comprises, by mass percentage:

[0008] 0.6%-1% konjac glucomannan, 2%-5% coal slime, 5%-10% acrylic acid, 3%-5% polyacrylamide, 0.015%-0.04% potassium thiosulfate, 0.02%-0.05% ammonium persulfate, 0.2%-0.4% N,N-methylenebisacrylamide, and the balance is water.

[0009] 2. The fire-fighting material for resource utilization of coal mine waste and suppression of coal spontaneous combustion according to claim 1 is characterized in that the coal mine waste is coal slime, a waste product that is difficult to reuse and is produced after cleaning and screening in a coal washing plant. It is mainly composed of coal powder, water, and bone stone powder, has a large output, and has more water content and greater viscosity.

[0010] 3. The fire extinguishing material for resource utilization of coal mine waste and inhibition of coal spontaneous combustion according to claim 1, characterized in that the initiator is potassium thiosulfate and ammonium persulfate solution; and the cross-linking agent is N,N-methylenebisacrylamide solution.

[0011] 4. A method for preparing a coal slime-based fire extinguishing material for inhibiting spontaneous combustion of coal as claimed in claim 1, comprising the following steps:

[0012] Step 1: Dry the coal slime powder at 60°C for 4 hours, then grind it in a pulverizer, mix the ground coal slime and grinding balls in a certain proportion, add 2% (wt) stearic acid solution and an appropriate amount of deionized water, and grind it in a ball mill for a period of time, then perform ultrasonic dispersion, washing, suction filtration, drying and grinding to obtain modified coal slime.

[0013] Step 2, take an appropriate amount of konjac flour and place it in a 500ml beaker, and add a certain amount of deionized water to it, and make it completely gelatinized at 90°C and under the protection of a nitrogen atmosphere. Then, use 20% sodium hydroxide solution to neutralize acrylic acid under ice bath conditions, and then add the pre-prepared polyacrylamide solution to a beaker at 65°C and stir evenly. After that, add initiators potassium thiosulfate and ammonium persulfate to the mixture and react for 40 minutes. Slowly add the cross-linking agent N,N-methylenebisacrylamide, after 1 hour of cross-linking reaction, add different masses of modified coal slime, stir evenly, and obtain a black colloid after a period of time. Finally, use ethanol to precipitate the obtained product, filter it and vacuum dry it at 60°C until the mass is constant.

[0014] 5. The preparation method according to claim 1, characterized in that the ratio of coal slime to grinding balls in step 1 is 1:5.

[0015] 6. The preparation method according to claim 1, characterized in that the reaction temperature in step 2 is 65°C and the drying temperature is 60°C.

[0016] The present invention provides a coal slime-based fire prevention and extinguishing material for inhibiting coal spontaneous combustion and a preparation method. In the preparation process, konjac glucomannan is used as a matrix, and a graft copolymerization reaction is carried out with acrylic acid and acrylamide. The modified coal slime is used as a filling material to form a physical crosslink with the colloid to obtain a coal slime slurry-based gel. It not only maintains the high water retention and degradability of the biomass gel, but also has the adhesion and sealing properties of the coal slime. Using this for underground fire prevention and control can not only effectively dispose of a large amount of waste coal slime piled up around the mine, but also fill the goaf, realizing the resource utilization of coal mine waste and the suppression of coal mine fires. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The present invention is a schematic diagram of the process of the coal slime-based fire extinguishing material and the preparation method thereof for suppressing the spontaneous combustion of coal.

[0018] Figure 2 This is a scanning electron microscope image of the coal slime-based fire extinguishing material used to suppress coal spontaneous combustion in the present invention.

[0019] Figure 3 It is a schematic diagram of the reaction process of the coal slime-based fire extinguishing material and preparation method for inhibiting coal spontaneous combustion in the present invention.

[0020] The present invention provides a coal slime-based fire extinguishing material and a preparation method for inhibiting coal spontaneous combustion. In order to make the objectives, technical solutions and effects of the present invention clearer, the present invention will be described in more detail below. It should be understood that the specific embodiments described here are only for illustrating the present invention and are not intended to limit the present invention.

[0021] The invention provides a coal slime-based fire extinguishing material for inhibiting spontaneous combustion of coal and a preparation method thereof. The coal slime-based fire extinguishing material comprises, by mass percentage, 0.6%-1% of konjac glucomannan, 2%-5% of coal slime, 5%-10% of acrylic acid, 3%-5% of polyacrylamide, 0.015%-0.04% of potassium thiosulfate, 0.02%-0.05% of ammonium persulfate, 0.2%-0.4% of N,N-methylenebisacrylamide, and the balance is water.

[0022] The initiator is potassium thiosulfate and ammonium persulfate solution; the cross-linking agent is N,N-methylenebisacrylamide solution.

[0023] The present invention also provides a method for preparing the above-mentioned fire-proof and extinguishing material for resource utilization of coal mine waste and inhibition of coal spontaneous combustion, such as Figure 1 As shown, it includes the following steps:

[0024] Step 1: Dry the coal slime powder at 60°C for 4 hours, then grind it in a pulverizer, mix the ground coal slime and grinding balls in a certain proportion, add 2% (wt) stearic acid solution and an appropriate amount of deionized water, and grind it in a ball mill for a period of time, then perform ultrasonic dispersion, washing, suction filtration, drying and grinding to obtain modified coal slime.

[0025] Step 2, take an appropriate amount of konjac flour and place it in a 500ml beaker, and add a certain amount of deionized water to it, and make it completely gelatinized at 90°C and under the protection of a nitrogen atmosphere. Then, use 20% sodium hydroxide solution to neutralize acrylic acid under ice bath conditions, and then add the pre-prepared polyacrylamide solution to a beaker at 65°C and stir evenly. After that, add initiators potassium thiosulfate and ammonium persulfate to the mixture and react for 40 minutes. Slowly add the cross-linking agent N,N-methylenebisacrylamide, after 1 hour of cross-linking reaction, add different masses of modified coal slime, stir evenly, and obtain a black colloid after a period of time. Finally, use ethanol to precipitate the obtained product, filter it and vacuum dry it at 60°C until the mass is constant.

[0026] The present invention provides a coal slime-based fire prevention and extinguishing material for inhibiting coal spontaneous combustion and a preparation method, which uses konjac glucomannan as a matrix, undergoes graft copolymerization reaction with acrylic acid and acrylamide, and uses the modified coal slime as a filling material to form physical crosslinks with the colloid to obtain a coal slime slurry-based gel. It not only maintains the high water retention and degradability of the biomass gel, but also has the adhesion and sealing properties of the coal slime. Using this for underground fire prevention and control can not only effectively dispose of a large amount of waste coal slime piled up around the mine, but also fill the goaf, thereby realizing the resource utilization of coal mine waste and the suppression of coal mine fires. In order to further describe the present invention, more detailed embodiments are listed below.

[0027] Embodiment 1:

[0028] The coal slime powder was dried at 60°C for 4 hours and then ground in a pulverizer. The ground coal slime and grinding balls were mixed in a ratio of 1:5, 2% (wt) stearic acid solution and an appropriate amount of deionized water were added, and after ball milling for a period of time, ultrasonic dispersion, washing, suction filtration, drying and grinding were performed to obtain the modified coal slime.

[0029] Accurately weigh 1g of konjac flour and place it in a 500ml beaker, add 150ml of deionized water, and gelatinize at 90℃ for 30min until the konjac flour is fully swollen. Lower the temperature to 65℃, then add the prepared sodium acrylate solution and polyacrylamide solution to the beaker, then add initiator 0.025g potassium thiosulfate and 0.038g ammonium persulfate, stir evenly, and initiate at 65℃ for 30min, finally add 0.35g of crosslinking agent N,N-methylenebisacrylamide, after 1 hour of crosslinking reaction, add coal slurry made from 3g of modified coal slurry, stir evenly, and obtain black colloid after a period of time. Finally, use ethanol to precipitate the obtained product, filter it to obtain coal slurry-based gel, and test the relevant properties.

[0030] Embodiment 2:

[0031] The coal slime powder was dried at 60°C for 4 hours and then ground in a pulverizer. The ground coal slime and grinding balls were mixed in a ratio of 1:5, 2% (wt) stearic acid solution and an appropriate amount of deionized water were added, and after ball milling for a period of time, ultrasonic dispersion, washing, suction filtration, drying and grinding were performed to obtain the modified coal slime.

[0032] Accurately weigh 1g of konjac flour and place it in a 500ml beaker, add 150ml of deionized water, and gelatinize at 90℃ for 30min until the konjac flour is fully swollen. Lower the temperature to 65℃, then add the prepared sodium acrylate solution and polyacrylamide solution to the beaker, then add initiator 0.025g potassium thiosulfate and 0.038g ammonium persulfate, stir evenly, and initiate at 65℃ for 30min, finally add 0.35g of crosslinking agent N,N-methylenebisacrylamide, after 1 hour of crosslinking reaction, add coal slurry made from 5g of modified coal slurry, stir evenly, and obtain black colloid after a period of time. Finally, use ethanol to precipitate the obtained product, filter it to obtain coal slurry-based gel, and test the relevant properties.

[0033] Embodiment 3:

[0034] The coal slime powder was dried at 60°C for 4 hours and then ground in a pulverizer. The ground coal slime and grinding balls were mixed in a ratio of 1:5, 2% (wt) stearic acid solution and an appropriate amount of deionized water were added, and after ball milling for a period of time, ultrasonic dispersion, washing, suction filtration, drying and grinding were performed to obtain the modified coal slime.

[0035] Accurately weigh 1g of konjac flour and place it in a 500ml beaker, add 150ml of deionized water, and gelatinize at 90℃ for 30min until the konjac flour is fully swollen. Lower the temperature to 65℃, then add the prepared sodium acrylate solution and polyacrylamide solution to the beaker, then add initiator 0.025g potassium thiosulfate and 0.038g ammonium persulfate, stir evenly, and initiate at 65℃ for 30min, finally add 0.38g of crosslinking agent N,N-methylenebisacrylamide, after 1 hour of crosslinking reaction, add coal slurry made from 7g of modified coal slurry, stir evenly, and obtain black colloid after a period of time. Finally, use ethanol to precipitate the obtained product, filter it to obtain coal slurry-based gel, and test the relevant properties.

[0036] Table 1 Thermal stability of gel with 3g modified coal slime added

[0037]

[0038] Table 2 Thermal stability of gel with 5g modified coal slime added

[0039]

[0040] Table 3 Thermal stability of gel with 7g modified coal slime added

[0041]

[0042] Of course, the above description is only a preferred embodiment of the present invention, and the present invention is not limited to the above embodiments. It should be noted that all equivalent substitutions and obvious deformation forms made by any technician familiar with the field under the guidance of this specification fall within the essential scope of this specification and should be protected by the present invention.

Claims

1. A coal slime-based fire extinguishing material for inhibiting spontaneous combustion of coal and a preparation method thereof, comprising, by mass percentage: 0.6%-1% konjac glucomannan, 2%-5% modified coal slime, 5%-10% acrylic acid, 3%-5% polyacrylamide, 0.015%-0.04% potassium thiosulfate, 0.02%-0.05% ammonium persulfate, 0.2%-0.4% N,N-methylenebisacrylamide, and the balance is water.

2. The fire extinguishing material for resource utilization of coal mine waste and suppression of coal spontaneous combustion according to claim 1, characterized in that: The coal mine waste is coal slime, a waste product that is difficult to reuse and is produced after cleaning and screening in a coal washing plant. It is mainly composed of coal powder, water, and bone and stone powder, has a large output, and has a high moisture content and a high viscosity.

3. The fire extinguishing material for resource utilization of coal mine waste and suppression of coal spontaneous combustion according to claim 1, characterized in that: The initiator is potassium thiosulfate and ammonium persulfate solution; the cross-linking agent is N,N-methylenebisacrylamide solution.

4. A method for preparing a coal slime-based fire extinguishing material for inhibiting coal spontaneous combustion as claimed in claim 1, comprising the following steps: Step 1: Dry the coal slime powder at 60° C. for 4 hours, then grind it in a pulverizer, mix the ground coal slime and grinding balls in a certain proportion, add 2% (wt) stearic acid solution and an appropriate amount of deionized water, and grind it in a ball mill for a period of time, then perform ultrasonic dispersion, washing, suction filtration, drying and grinding to obtain modified coal slime; Step 2: Take an appropriate amount of konjac flour and place it in a 500ml beaker, add a certain amount of deionized water to it, and make it completely gelatinized at 90°C and under the protection of nitrogen atmosphere; then, use 20% sodium hydroxide solution to neutralize acrylic acid under ice bath conditions, and then add the pre-prepared polyacrylamide solution to a beaker at 65°C and stir evenly; then, add initiators potassium thiosulfate and ammonium persulfate to the mixture and react for 40 minutes. Slowly add the cross-linking agent N,N-methylenebisacrylamide, after 1 hour of cross-linking reaction, add different masses of modified coal slime, stir evenly, and obtain a black colloid after a period of time. Finally, use ethanol to precipitate the obtained product, filter it and vacuum dry it at 60°C until the mass is constant.

5. The preparation method according to claim 1, characterized in that: The ratio of coal slime to grinding balls in step 1 is 1:

5.

6. The preparation method according to claim 1, characterized in that: The reaction temperature in step 2 is 65°C and the drying temperature is 60°C.

Citation Information

Cited By

  • Technological process for preparing coal spontaneous combustion prevention and control material by recycling coal slime and application of technological process

    CN119222952A