High-performance filtering material for polymer cutting and preparation method of high-performance filtering material
By treating polyphenylene sulfide fibers with nano-SiO2 dispersion to form a composite fiber web, the problem of insufficient chemical and thermal stability of existing filter materials during polymer cutting is solved, thereby improving the strength and filtration efficiency of the material.
Patent Information
- Application Number
- CN202411257237.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-22
AI Technical Summary
Existing filter materials lack sufficient chemical and thermal stability during polymer cutting, and their strength, dust removal efficiency, and dust stripping performance need to be further enhanced.
A composite fiber web is formed by needle punching polyphenylene sulfide fibers and reinforcing fibers, combined with a treatment liquid containing nano-SiO2 dispersion and specific complexes. Through ring-opening addition reaction, a three-dimensional network structure is formed, which enhances the rigidity and flexibility of the material and improves filtration efficiency.
It significantly improves the material's mechanical strength, dust removal efficiency, and dust stripping rate, achieving a high-performance filtration effect.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of filter materials, in particular to a high-performance filter material for polymer cutting and a preparation method thereof. Background Art
[0002] High-performance filter materials can be widely used in the field of polymer cutting, such as the cutting process of plastics, rubber and other materials. It can effectively filter the tiny particles and impurities generated during the cutting process, protect the cutting equipment and the environment, and improve product quality and production efficiency.
[0003] Chinese patent CN118390309A: discloses a method for preparing a layered, gradient foam layer coated filter material. The present invention uses polytetrafluoroethylene (PTFE) as the main component of the foam coating finishing liquid, after forming a PTFE film layer on the surface of the filter substrate, introduces polyvinyl alcohol (PVA) to modify the PTFE, and innovates the finishing process after the foam film layer is coated.
[0004] Chinese patent CN118407252A: relates to an acid-resistant and alkali-resistant filter material for a filter press and a preparation method thereof, and relates to the field of filter materials. The acid-resistant and alkali-resistant fiber fabric is obtained by weaving acid-resistant and alkali-resistant fibers. The acid-resistant and alkali-resistant fibers include composite fibers and fluorine-modified reinforcing coatings. The fluorine-modified reinforcing coatings are obtained by coating the fluorine-modified reinforcing coatings on the surfaces of the composite fibers. The fluorine-modified reinforcing coatings include the following components by mass: 40-60 parts of fluorine-modified acrylic emulsion, 20-30 parts of fluorinated graphene styrene-acrylic emulsion, 10-30 parts of water, and 2-6 parts of a leveling agent. The raw materials for preparing the fluorine-modified acrylic emulsion include butyl acrylate, styrene, hydroxypropyl acrylate, acrylic acid, methacryloyloxypropyl cage-type silsesquioxane, and dodecafluoroheptyl methacrylate.
[0005] Chinese patent CN118105777A: discloses a modified PTFE fiber composite filter material and a preparation method thereof, including a filter material body, the filter material body including composite fibers, filter fibers and compression-resistant fibers, the composite fibers including the following components: 20 to 30 parts by weight of PTFE fibers, compression-resistant fibers, glass fibers, carbon fibers and polypropylene fibers are arranged in the filter material body of the present invention.
[0006] The filter materials currently prepared using patented technologies and existing methods have deficiencies in chemical stability and thermal stability. At the same time, their material strength, dust removal efficiency and dust stripping performance still need to be significantly enhanced and optimized. Summary of the invention
[0007] In view of the deficiencies of the prior art, the present invention provides a high-performance filter material for polymer cutting and a preparation method thereof, wherein the operation steps are as follows:
[0008] S1: 60-80 parts by weight of polyphenylene sulfide fiber and 1-5 parts of reinforcing fiber are needle-punched to obtain a composite fiber web;
[0009] S2: sintering 80-100 parts of polyphenylene sulfide resin at 300-360° C., stretching, adhering to a composite fiber web, and hot pressing to obtain a composite fiber filter material;
[0010] S3: 14-17 parts of the composite fiber filter material are immersed in 50-60 parts of the treatment liquid. After immersion for 60-90 minutes, the excess liquid is squeezed out, and the material is dried and heat-treated to obtain a high-performance filter material.
[0011] In some embodiments, the reinforcing fiber is one of stainless steel fiber, carbon fiber, aramid fiber, basalt fiber, and sepiolite fiber.
[0012] In some embodiments, the acupuncture density is 60-100 needles / cm 2 .
[0013] In some embodiments, the margin ratio is 60-70%.
[0014] In some embodiments, the heat treatment is performed at a temperature of 230-250° C. and for a time of 100-200 seconds.
[0015] In some embodiments, the method for preparing the treatment solution is:
[0016] A1: Add 100-125 parts of nano-SiO2 powder to 1000-1280 parts of deionized water, mix and ultrasonically disperse for 20-30 minutes; add 3-6 parts of silane coupling agent, and ultrasonically disperse for 30-50 minutes to obtain epoxy nano-SiO2 dispersion;
[0017] A2: 50-150 parts of epoxy nano-SiO2 dispersion, 0.005-0.02 parts of 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex, 10-20 parts of cardanol glycidyl ether, 30-50 parts of polytetrafluoroethylene emulsion, 150-200 parts of water, 2-5 parts of triethanolamine, continue ultrasonic treatment at 50-70°C for 60-80 minutes, mix and stir for 20-40 minutes to obtain a treated solution.
[0018] In some embodiments, the silane coupling agent is one of γ-(2,3-epoxypropoxy)propyltriethoxysilane, 3-[(2,3)-epoxypropoxy]propylmethyldimethoxysilane, and γ-glycidyloxypropyltrimethoxysilane.
[0019] In some embodiments, the preparation method of the 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex is:
[0020] According to weight, 3-6 parts of 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid, CAS: 1312703-28-8, 3-6 parts of cerium nitrate and 100-120 parts of toluene are mixed, reacted at 60-70° C. for 100-150 minutes, and toluene is removed by distillation to obtain a 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex.
[0021] Amino-epoxy ring-opening addition reaction mechanism:
[0022] In the process of preparing high-performance filter materials, the first thing that occurs is the ring-opening addition reaction between the amino group in the 2'-amino-[1,1':4',1″-terphenyl]-4,4″-dicarboxylic acid / cerium metal complex and the epoxy group in the epoxy nano-SiO2 dispersion and cardanolglycidyl ether; this is a typical reaction between amino groups and epoxy groups, in which the nucleophilic nitrogen atom of the amino group attacks the carbon atom on the epoxy ring, causing the epoxy ring to crack and form a longer chain structure; triethanolamine may play two roles here: one is to act as a catalyst to accelerate the reaction between the amino group and the epoxy group; the other is that it may participate in further cross-linking reactions through its own hydroxyl groups to enhance the mechanical strength and stability of the final material.
[0023] After the ring-opening addition reaction, the original linear or planar structure is transformed into a more complex three-dimensional network structure, which helps to improve the filtration efficiency and mechanical strength of the material.
[0024] Compared with the prior art, the beneficial technical effects of the present invention are:
[0025] 1. Terphenyl is a large aromatic system with a conjugated structure. Its introduction can significantly increase the structural rigidity of the material. In addition, the hydrophobicity of terphenyl also makes the modified polyphenylene sulfide fiber perform better in dust removal rate.
[0026] 2. Cardanol is extracted from natural cashew oil and has a structure of long-chain alkyl and phenol groups. This structure can increase the surface roughness of the material while providing good flexibility, improve the interaction between the material and the substance to be filtered, and thus improve the filtration efficiency. DETAILED DESCRIPTION
[0027] To better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be understood by those skilled in the art that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0028] Unless otherwise specified, the experimental methods used in the examples are all conventional methods; the materials, reagents, etc. used, unless otherwise specified, can be obtained from commercial channels.
[0029] 1. Mechanical strength test: Test according to GB / T17638-1998;
[0030] 2. Dust removal efficiency: refer to HJ / T324-2006, and test at constant pressure 30 times after aging;
[0031] 3. Dust stripping rate: Tested in accordance with HJ / T324-2006.
[0032] Example 1
[0033] A high-performance filter material for polymer cutting and a preparation method thereof, wherein the operation steps are as follows:
[0034] S1: 60g of polyphenylene sulfide fiber and 1g of reinforcing fiber are needle-punched to obtain a composite fiber web;
[0035] S2: 80 g of polyphenylene sulfide resin is sintered at 300° C., stretched, adhered to a composite fiber web, and hot-pressed to obtain a composite fiber filter material;
[0036] S3: 14 g of the composite fiber filter material is immersed in 50 g of the treatment liquid. After immersion for 60 minutes, the excess liquid is squeezed out, and the material is dried and heat-treated to obtain a high-performance filter material.
[0037] The reinforcing fiber is stainless steel fiber.
[0038] The acupuncture density is 60 needles / cm 2 .
[0039] The rolling margin is 60%.
[0040] The heat treatment temperature is 230° C. and the time is 100 s.
[0041] The preparation method of the treatment liquid is:
[0042] A1: Add 100g of nano-SiO2 powder into 1000g of deionized water, mix and disperse by ultrasonic for 20min; add 3g of silane coupling agent and disperse by ultrasonic for 30min; obtain epoxy nano-SiO2 dispersion;
[0043] A2: 50 g epoxy nano-SiO2 dispersion, 0.005 g 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex, 10 g cardanol glycidyl ether, 30 g polytetrafluoroethylene emulsion, 150 g water, 2 g triethanolamine, continue ultrasonic treatment at 50°C for 60 min, mix and stir for 20 min to obtain a treated solution.
[0044] The silane coupling agent is γ-(2,3-epoxypropoxy)propyltriethoxysilane.
[0045] The preparation method of the 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex is as follows:
[0046] 3 g of 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid, CAS: 1312703-28-8, 3 g of cerium nitrate, and 100 g of toluene were mixed, reacted at 60° C. for 100 minutes, and toluene was distilled off to obtain a 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex.
[0047] Example 2
[0048] A high-performance filter material for polymer cutting and a preparation method thereof, wherein the operation steps are as follows:
[0049] S1: 65g of polyphenylene sulfide fiber and 2g of reinforcing fiber are needle-punched to obtain a composite fiber web;
[0050] S2: 85 g of polyphenylene sulfide resin was sintered at 320° C., stretched, adhered to a composite fiber web, and hot-pressed to obtain a composite fiber filter material;
[0051] S3: 15 g of the composite fiber filter material was immersed in 53 g of the treatment liquid for 70 min, and then the excess liquid was squeezed out, dried, and heat-treated to obtain a high-performance filter material.
[0052] The reinforcing fiber is aramid fiber.
[0053] The acupuncture density is 70 needles / cm 2 .
[0054] The rolling margin is 65%.
[0055] The heat treatment temperature is 235° C. and the time is 140 seconds.
[0056] The preparation method of the treatment liquid is:
[0057] A1: Add 110g of nano-SiO2 powder into 1100g of deionized water, mix and disperse by ultrasonic for 25min; add 4g of silane coupling agent and disperse by ultrasonic for 35min; obtain epoxy nano-SiO2 dispersion;
[0058] A2: 80 g epoxy nano-SiO2 dispersion, 0.01 g 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex, 13 g cardanol glycidyl ether, 35 g polytetrafluoroethylene emulsion, 160 g water, 3 g triethanolamine, continue ultrasonic treatment at 55°C for 65 min, mix and stir for 25 min to obtain a treated solution.
[0059] The silane coupling agent is 3-[(2,3)-epoxypropoxy]propylmethyldimethoxysilane.
[0060] The preparation method of the 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex is as follows:
[0061] 4 g of 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid, CAS: 1312703-28-8, 4 g of cerium nitrate, and 105 g of toluene were mixed, reacted at 65° C. for 110 minutes, and toluene was distilled off to obtain 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex.
[0062] Example 3
[0063] A high-performance filter material for polymer cutting and a preparation method thereof, wherein the operation steps are as follows:
[0064] S1: 75g of polyphenylene sulfide fiber and 4g of reinforcing fiber are needle-punched to obtain a composite fiber web;
[0065] S2: 95 g of polyphenylene sulfide resin was sintered at 350° C., stretched, adhered to a composite fiber web, and hot-pressed to obtain a composite fiber filter material;
[0066] S3: 16 g of the composite fiber filter material is immersed in 58 g of the treatment liquid. After immersion for 80 minutes, the excess liquid is squeezed out, and the material is dried and heat-treated to obtain a high-performance filter material.
[0067] The reinforcing fiber is basalt fiber.
[0068] The acupuncture density is 90 needles / cm 2 .
[0069] The rolling margin is 65%.
[0070] The heat treatment temperature is 245° C. and the time is 180 seconds.
[0071] The preparation method of the treatment liquid is:
[0072] A1: Add 120g of nano-SiO2 powder into 1200g of deionized water, mix and disperse by ultrasonic for 25min; add 5g of silane coupling agent and disperse by ultrasonic for 45min; obtain epoxy nano-SiO2 dispersion;
[0073] A2: 130 g epoxy nano-SiO2 dispersion, 0.015 g 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex, 18 g cardanol glycidyl ether, 45 g polytetrafluoroethylene emulsion, 180 g water, 4 g triethanolamine, continue ultrasonic treatment at 65°C for 75 min, mix and stir for 35 min to obtain a treated solution.
[0074] The silane coupling agent is 3-[(2,3)-epoxypropoxy]propylmethyldimethoxysilane.
[0075] The preparation method of the 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex is as follows:
[0076] 5 g of 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid, CAS: 1312703-28-8, 5 g of cerium nitrate, and 115 g of toluene were mixed, reacted at 65° C. for 140 minutes, and toluene was distilled off to obtain 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex.
[0077] Example 4
[0078] A high-performance filter material for polymer cutting and a preparation method thereof, wherein the operation steps are as follows:
[0079] S1: 80g of polyphenylene sulfide fiber and 5g of reinforcing fiber are needle-punched to obtain a composite fiber web;
[0080] S2: 100 g of polyphenylene sulfide resin is sintered at 360° C., stretched, adhered to a composite fiber web, and hot-pressed to obtain a composite fiber filter material;
[0081] S3: 17 g of the composite fiber filter material was immersed in 60 g of the treatment liquid for 90 min, and then the excess liquid was squeezed out, dried, and heat-treated to obtain a high-performance filter material.
[0082] The reinforcing fiber is sepiolite fiber.
[0083] The acupuncture density is 100 needles / cm 2 .
[0084] The rolling margin is 70%.
[0085] The heat treatment temperature is 250° C. and the time is 200 s.
[0086] The preparation method of the treatment liquid is:
[0087] A1: Add 125g of nano-SiO2 powder to 1280g of deionized water, mix and disperse by ultrasonic for 30min; add 6g of silane coupling agent and disperse by ultrasonic for 50min; obtain epoxy nano-SiO2 dispersion;
[0088] A2: 150g epoxy nano-SiO2 dispersion, 0.02g 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex, 20g cardanol glycidyl ether, 50g polytetrafluoroethylene emulsion, 200g water, 5g triethanolamine, continue ultrasonic treatment at 70°C for 80min, mix and stir for 40min to obtain a treated solution.
[0089] The silane coupling agent is gamma-glycidyloxypropyltrimethoxysilane.
[0090] The preparation method of the 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex is as follows:
[0091] 6 g of 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid, CAS: 1312703-28-8, 6 g of cerium nitrate, and 120 g of toluene were mixed, reacted at 70° C. for 150 minutes, and toluene was distilled off to obtain 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex.
[0092] Comparative Example 1
[0093] In this example, 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex and cardanol glycidyl ether were not added, and the other steps were the same as in Example 1.
[0094] Comparative Example 2
[0095] In this example, 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex was not added, and the other steps were the same as in Example 1.
[0096] Comparative Example 3
[0097] In this example, no cardanol glycidyl ether was added, and the rest was the same as in Example 1.
[0098] Test results:
[0099] Longitudinal breaking strength / kN / m Transverse breaking strength / kN / m Dust removal efficiency% Dust removal rate / % Example 1 21.9 20.7 99.9993 99.89 Example 2 22.5 21.0 99.9996 99.92 Example 3 23.1 21.5 99.9998 99.96 Example 4 23.6 21.8 99.9999 99.98 Comparative Example 1 15.3 14.6 95.42 92.71 Comparative Example 2 18.4 17.9 98.61 96.25 Comparative Example 3 19.2 18.5 99.03 97.36
[0100] Through the data analysis of the above embodiments and comparative examples, the high-performance filter material prepared by the present invention has excellent mechanical strength, dust removal efficiency and dust stripping rate.
[0101] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A high-performance filter material for polymer cutting and a preparation method thereof, wherein the operation steps are: S1: 60-80 parts of polyphenylene sulfide fiber and 1-5 parts of reinforcing fiber are needle-punched by weight to obtain a composite fiber web; S2: sintering 80-100 parts of polyphenylene sulfide resin at 300-360° C., stretching, adhering to a composite fiber web, and hot pressing to obtain a composite fiber filter material; S3: immerse 14-17 parts of the composite fiber filter material in 50-60 parts of the treatment liquid for 60-90 minutes, squeeze out the excess liquid, dry, and heat-treat to obtain a high-performance filter material.
2. A high-performance filter material for polymer cutting and a preparation method thereof according to claim 1, characterized in that: The reinforcing fiber is one of stainless steel fiber, carbon fiber, aramid fiber, basalt fiber and sepiolite fiber.
3. The high-performance filter material for polymer cutting and the preparation method thereof according to claim 1, characterized in that: The acupuncture density is 60-100 needles / cm 2 .
4. The high-performance filter material for polymer cutting and the preparation method thereof according to claim 1, characterized in that: The rolling margin is 60-70%.
5. The high-performance filter material for polymer cutting and the preparation method thereof according to claim 1, characterized in that: The heat treatment temperature is 230-250° C., and the time is 100-200 seconds.
6. The high-performance filter material for polymer cutting and the preparation method thereof according to claim 1, characterized in that: The preparation method of the treatment liquid is: A1: Add 100-125 parts of nano-SiO2 powder to 1000-1280 parts of deionized water, mix and ultrasonically disperse for 20-30 minutes; add 3-6 parts of silane coupling agent, and ultrasonically disperse for 30-50 minutes to obtain epoxy nano-SiO2 dispersion; A2: 50-150 parts of epoxy nano-SiO2 dispersion, 0.005-0.02 parts of 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex, 10-20 parts of cardanol glycidyl ether, 30-50 parts of polytetrafluoroethylene emulsion, 150-200 parts of water, 2-5 parts of triethanolamine, continue ultrasonic treatment at 50-70°C for 60-80 minutes, mix and stir for 20-40 minutes to obtain a treated solution.
7. A high-performance filter material for polymer cutting and a preparation method thereof according to claim 6, characterized in that: The silane coupling agent is one of γ-(2,3-epoxypropoxy)propyltriethoxysilane, 3-[(2,3)-epoxypropoxy]propylmethyldimethoxysilane and γ-glycidyloxypropyltrimethoxysilane.
8. The high-performance filter material for polymer cutting and the preparation method thereof according to claim 6, characterized in that: The preparation method of the 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex is as follows: According to weight, 3-6 parts of 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid, CAS: 1312703-28-8, 3-6 parts of cerium nitrate and 100-120 parts of toluene are mixed, reacted at 60-70° C. for 100-150 minutes, and toluene is removed by distillation to obtain a 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / cerium metal complex.
Citation Information
Patent Citations
Composite type fiber filtering material and preparation method thereof as well as filtering bag
CN102512881A
Method for preparing modified basalt fiber / polyphenylene sulfide compound filter material through dip coating
CN104191738A
Dip coating preparation method of modified basalt fiber / polyphenylene sulfide composite filter material
CN104233803A
Back flushing filter element of gas turbine filtration system
CN110215775A
Fingerprint authentication device, display device including the same, and method for authenticatiing fingerprint of display device
KR1020220030474A