Hierarchical pore MOFs-on-SSN polymer composite membrane and preparation method thereof

By introducing MOFs seed crystals and metal mesh into the polymer, a multi-stage pore MOFs-on-SSN@polymer composite film is solved, and the problem of insufficient flexibility of MOFs film and difficult to amplify the carrier material is achieved, and efficient hydrogen separation and batch volume are achieved Chemical production.

CN118987990APending Publication Date: 2024-11-22INST OF LASER MFG HENAN ACAD OF SCI +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411024088.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing MOFs films have problems such as insufficient flexibility, difficulty in amplifying the carrier material and high cost in the process of separation and purification of hydrogen, which limits their wide application.

Method used

By introducing MOFs seed crystals and metal mesh (SSN) into the polymer, MOFs crystals are induced to grow on the surface, forming a multi-stage porous MOFs-on-SSN@polymer composite membrane, improving separation performance and avoiding fracture, and using an autoclave, etc. Equipment for preparation.

Benefits of technology

The high-efficiency gas separation performance of MOFs films is achieved, the strength and toughness of the film are improved, and the production potential is provided, reducing the preparation cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118987990A_ABST
    Figure CN118987990A_ABST
Patent Text Reader

Abstract

The invention discloses a hierarchical porous MOFs-on-SSN polymer composite membrane and a preparation method thereof. The method comprises the following steps: S1, preparing a seed crystal MOFs crystal solution; s2, adding a polymer into the seed crystal MOFs crystal solution to obtain a solution C, coating SSN with the solution C, and performing treatment to obtain an SSN-coated polymer; and S3, mixing a second metal salt, a second organic ligand and a second regulator to obtain a solution D, putting the SSN-coated polymer in the step S2 into the solution D, pouring the solution D into a high-pressure reaction kettle, and after the reaction is completed, obtaining the hierarchical porous MOFs-on-SSN-coated polymer composite membrane. According to the preparation method disclosed by the invention, the polymer mixed with the MOFs seed crystal is used as the middle layer, so that the nucleation growth position of the MOFs crystal on the surface of the polymer is greatly increased, the uniform MOFs film layer can grow on the substrate, and the MOFs crystal is prevented from falling off; the prepared MOFs crystal layer is an effective separation layer, and a satisfactory gas separation effect can be achieved through the combination of macropores of the polymer and micropores of the MOFs crystal layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of membrane separation materials, and in particular to a multi-level porous MOFs-on-SSN@polymer composite membrane and a preparation method thereof. Background Art

[0002] With the extensive use of traditional fossil energy, problems such as resource depletion, environmental pollution, and climate change are becoming increasingly serious. Hydrogen (H2) as a green, sustainable, clean energy has become the focus of global attention. However, large-scale production of H2 from industry requires a lot of cost and time in the separation and purification process, which hinders the actual scale of H2 use. Membrane separation technology is considered to be a promising separation and purification method due to its low energy consumption and cost as well as environmentally friendly process. However, there are still many problems to be solved in practical applications.

[0003] Metal-organic framework (MOFs) materials have attracted extensive attention in the field of gas adsorption and separation due to their highly diverse structures and pore sizes, as well as their specific adsorption affinity. Therefore, MOFs materials have become a popular material in the preparation of molecular sieve membranes. MOFs gas separation membranes, especially zeolitic imidazole framework (ZIF) membranes, such as ZIF-7, ZIF-8, ZIF-9, ZIF-37, ZIF-90 and ZIF-95, have been widely used in the purification of H2. However, since MOFs materials are not flexible and are easily broken by force, it is difficult to use them alone as membrane materials. Therefore, they are usually used as additives to prepare polymer mixed matrix membranes or to grow dense MOFs crystal layers on carriers as crystal membranes. Although MOFs-based membranes have excellent separation performance, polymer mixed matrix membranes are prone to the defect of not having sieving performance due to the interaction between MOFs and polymers, which greatly affects the separation performance; in addition, it is necessary to coat the surface with seeds or form a film on the surface of a chemically modified carrier to prepare MOFs crystal membranes with practical application value. The problem of difficult to scale up and high cost of support materials has been difficult to solve, thus limiting the widespread application of MOFs membranes.

[0004] CN202211664085.4 discloses a method for preparing a metal-MOFs-74 / PSF film, its products and applications. The method uses tetrahydrofuran as a common synthesis solvent for MOFs-74 and polysulfone, which reduces the particle agglomeration phenomenon of MOFs-74 between the polysulfone matrix during the preparation process, and directly adds polysulfone to the MOFs suspension to obtain the desired mixed matrix membrane after reaction. At the same time, a microwave-assisted method is used in the preparation process, which greatly shortens the synthesis time of MOFs and improves the preparation efficiency of the membrane.

[0005] CN202410252470.0 discloses a method for preparing a rigid MOFs-polymer hydrogen bond network mixed matrix membrane, and the preparation process includes: first, using a combination of hydrothermal and heat treatment to obtain activated MIL-53 crystals, and evenly dispersing them in a polyamic acid solution to form a casting liquid; then, evenly coating the casting liquid on a clean glass plate and letting it air dry naturally; finally, heat-treating the peeled film to cause a "breathing effect" in the MOFs crystals and an imidization reaction in the polyamic acid, and finally using the hydrogen bonds between the flexible MOFs and the polymer to prepare a self-supporting rigid MOFs mixed matrix membrane. The above invention proposes a strategy for hydrogen-bonded rigid flexible MOFs to prepare a self-supporting rigid MOFs mixed matrix membrane.

[0006] The above technical solutions have made improvements in different aspects, but the prepared MOFs membrane still has the problem that the carrier material is difficult to scale up. Therefore, it is urgent to develop a simple and feasible method for preparing MOFs membrane. Summary of the invention

[0007] The purpose of the present invention is to provide a multi-level porous MOFs-on-SSN@polymer composite membrane and a preparation method thereof. By introducing MOFs seeds and metal mesh (hereinafter referred to as SSN) into the polymer, firstly, the MOFs seeds blended in the polymer can induce the growth of MOFs crystals on its surface, and the outermost MOFs crystal layer is an effective separation layer, which can greatly improve the separation performance; secondly, the SSN in the polymer can serve as a skeleton to support the MOFs membrane and avoid breakage.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions: A method for preparing a multi-level porous MOFs-on-SSN@polymer composite membrane comprises the following steps: S1: preparing a seed MOFs crystal solution using a first metal salt, a first organic ligand and a first regulator; S2: adding the polymer to the seed MOFs crystal solution in step S1 to obtain solution C, coating solution C on SSN and treating to obtain SSN@polymer; S3: The second metal salt, the second organic ligand and the second regulator are mixed to obtain a solution D, the SSN@polymer in step S2 is placed in the solution D, and poured into a high-pressure reactor. After the reaction is completed, a multi-level porous MOFs-on-SSN@polymer composite membrane is obtained.

[0009] Furthermore, step S1 specifically includes: S101: fully dissolving a first metal salt in a first solvent to obtain a solution A; S102: fully dissolving the first organic ligand and the first regulator in the second solvent to obtain a solution B; S103: mixing solution A and solution B uniformly by stirring to precipitate crystal powder; Wherein, the first solvent and the second solvent are both mixed solutions of N,N-dimethylformamide, ethanol and water, and the volume ratio of N,N-dimethylformamide:ethanol:water is 6-9:1-3:1-3.

[0010] Furthermore, in steps S101-S103, the metal ions in the first metal salt are one or more of zinc, cobalt, iron and nickel; the first organic ligand is 2-methylimidazole, benzimidazole, imidazole, 2-aldehyde imidazole or 2-ethylimidazole; the first regulator is triethylamine, aniline or ethylenediamine, and the mass of the first regulator is 1%-5% of the total mass of solution A and solution B.

[0011] Further, step S2 specifically includes: S201: adding a polymer to the seed MOFs crystal solution of step S1 under stirring, stirring at a first set temperature for a first set time and standing for degassing to obtain a solution C; S202: coating solution C on SSN, standing in water and washing with clean water, and then drying in a vacuum freeze drying oven to obtain SSN@polymer; Wherein, the mass of the polymer is 3 g-5 g, the first set temperature is 50° C.-90° C., and the first set time is 2 h-6 h.

[0012] Further, step S3 specifically includes: S301: fully dissolving the second metal salt, the second organic ligand and the second regulator in a third solvent to obtain a solution D; S302: fix the SSN@polymer in step S2 in the solution D in step S301, perform ultrasonic degassing, and then let it stand to allow the solution to wet the SSN@polymer; S303: pouring the mixture of the SSN@polymer in step S302 and the solution D in step S301 into a high-pressure reactor containing a Teflon liner, and reacting at a third set temperature for a third set time to obtain a multi-level porous MOFs-on-SSN@polymer composite membrane; Among them, the metal ion in the second metal salt is the same as the metal ion in the first metal salt, the second organic ligand is the same as the first organic ligand, the third solvent is methanol, ethanol, a mixture of methanol and ethanol, or a mixture of methanol and water, the second regulator is sodium formate, sodium acetate or sodium benzoate, the mass of the second regulator is 1%-5% of the total mass of solution D, the third set temperature is 120℃-150℃, and the third set time is 6 h-12 h.

[0013] Furthermore, in step S302, the SSN@polymer is fixed in a vertical manner in the solution D, so that both sides or one side of the SSN@polymer contacts the solution.

[0014] Furthermore, step S3 also includes: S304: washing the multi-level porous MOFs-on-SSN@polymer composite membrane obtained in step S303, and vacuum drying it at room temperature for a fourth set time to obtain a dried multi-level porous MOFs-on-SSN@polymer composite membrane; Among them, the fourth setting time is 12 h-24 h.

[0015] The present invention also relates to a multi-level porous MOFs-on-SSN@polymer composite membrane, comprising an inner core, an intermediate layer and an outer shell, wherein the inner core is SSN, the intermediate layer is a polymer layer mixed with MOFs crystal seeds, and the outer shell is a MOFs membrane layer.

[0016] The present invention has the following beneficial effects: 1. According to the preparation method of the present invention, by using a polymer mixed with MOFs crystal seeds as an intermediate layer, the nucleation growth positions of MOFs crystals on the polymer surface are greatly increased, so that a uniform MOFs film layer can be grown on the substrate, avoiding the shedding of MOFs crystals; the prepared MOFs crystal layer is an effective separation layer, which can greatly improve the separation performance.

[0017] 2. The MOFs-on-SSN@ polymer composite membrane of the present invention includes submicron-scale macropores formed by polymers for rapid gas passage; and subnanoscale micropores of the surface MOFs membrane layer for gas separation; through the combination of polymer macropores and MOFs material micropores, a satisfactory gas separation effect can be achieved.

[0018] 3. The MOFs-on-SSN@polymer composite membrane of the present invention uses SSN as the core, which greatly improves the strength and toughness of the composite membrane, thereby increasing the application range of the MOFs-on-SSN@polymer composite membrane.

[0019] 4. Since the SSN@polymer substrate can be prepared on a large scale, the hierarchical MOFs-on-SSN@polymer composite membrane of the present invention has the potential for mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic diagram of the structure of the MOFs-on-SSN@polymer composite membrane of the present invention; Figure 2 This is the structural diagram of MOFs materials; Figure 3 is a schematic diagram of an uncoated SSN; Figure 4 is a schematic diagram of a SSN coated with a polymer, wherein the polymer does not completely cover the SSN; Figure 5 is a schematic diagram of a SSN coated with a polymer, wherein the polymer completely covers the SSN; Figure 6 This is a SEM image of the ZIF-8-on-SSN@polysulfone composite membrane of Example 1 of the present invention.

[0021] In the figure, 1. MOFs membrane layer; 2. SSN; 3. Polymer DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0023] As described herein, the experimental methods used in the following examples are conventional methods unless otherwise specified.

[0024] In addition, the materials, reagents, and devices used in the following examples can be obtained from commercial sources unless otherwise specified.

[0025] As used herein, the abbreviation "SSN" means metal mesh.

[0026] As used herein, unless otherwise specified, numerical ranges include both the starting and ending values ​​of the range. For example, when describing the mass of a polymer as "3 g-5 g", this means that both 3 g and 5 g are valid values ​​of the mass.

[0027] It is well known that although MOFs crystal membranes have excellent separation performance, they must be coated with seeds on the surface or formed on a chemically modified carrier surface to prepare membranes with practical application value. Various substrates such as SSN substrates are conventionally used, but due to the poor heterogeneous nucleation points on the SSN substrate, it is usually difficult to obtain high-quality MOFs membranes using in-situ growth methods, especially for unmodified carriers. Therefore, it is necessary to chemically modify the substrate or introduce an intermediate layer before MOFs membrane formation.

[0028] Based on this, Figures 1 to 6 As shown, the method for preparing a multi-level porous MOFs-on-SSN@polymer composite membrane of the present invention comprises the following steps: S1: preparing a seed MOFs crystal solution using a first metal salt, a first organic ligand and a first regulator; S2: adding the polymer to the seed MOFs crystal solution in step S1 to obtain solution C, coating solution C on SSN and treating to obtain SSN@polymer; S3: The second metal salt, the second organic ligand and the second regulator are mixed to obtain a solution D, the SSN@polymer in step S2 is placed in the solution D, and poured into a high-pressure reactor. After the reaction is completed, a multi-level porous MOFs-on-SSN@polymer composite membrane is obtained.

[0029] Step S1 is a step of synthesizing a MOFs material as a seed, and there is no particular limitation on the method for synthesizing the MOFs material. In the preparation method of the present invention, a suitable first metal salt, a first organic ligand and a first regulator are selected according to the type and properties of the MOFs material to be synthesized, such as the size and shape of the pores. In one embodiment of the present invention, a seed MOFs material is synthesized using a solvothermal method.

[0030] Specifically, step S1 includes the following steps: S101: fully dissolving a first metal salt in a first solvent to obtain a solution A; S102: fully dissolving the first organic ligand and the first regulator in the second solvent to obtain a solution B; S103: Mix solution A and solution B evenly by stirring to precipitate crystal powder.

[0031] In the present invention, there is no particular restriction on the type of the first metal salt, as long as it can react with the organic ligand to obtain the MOFs material, but the present invention preferably uses nitrates or sulfates, and more preferably uses nitrates. In addition, the metal ions in the first metal salt are one or more of zinc, cobalt, iron and nickel. In the process of synthesizing the seed MOFs crystal, the mass of the first metal salt is generally 0.8 g-1.2 g.

[0032] The first organic ligand is an organic ligand commonly used in the synthesis of MOFs materials in the art. For example, the first organic ligand can be 2-methylimidazole, benzimidazole, imidazole, 2-formylimidazole or 2-ethylimidazole. In the process of synthesizing the seed MOFs crystal, the mass of the first organic ligand is 0.9 g-1.1 g.

[0033] It is known that in the synthesis process of MOFs materials, the main function of the regulator is to regulate the growth rate of MOFs crystals. In step S1 of the present invention, in order to achieve rapid crystallization of MOFs materials and precipitate MOFs crystals, the first regulator is specifically triethylamine, aniline or ethylenediamine, and its mass is 1%-5% of the total mass of solution A and solution B.

[0034] As known to those skilled in the art, the stability of MOFs materials prepared in different solvents in the solvent is relatively high. In order to improve the stability of the prepared MOFs material, during the synthesis process, the first solvent and the second solvent used in the present invention are a mixed solution of N, N-dimethylformamide, ethanol and water, wherein the volume ratio of N, N-dimethylformamide: ethanol: water is 6-9: 1-3: 1-3. At the same time, the use of a mixed solvent enables step S2 to be performed directly after obtaining the MOFs crystal material powder in step S1, without the need to dry and redissolve the MOFs crystals, and ensure that the polymer in step S2 can be well dissolved therein. Preferably, the volume of the first solvent is 30 mL-70 mL, and the volume of the second solvent is 30 mL-70 mL.

[0035] As described above, after obtaining the seed MOFs crystal solution in step S1, the polymer is directly added to the solution to obtain a polymer solution mixed with MOFs crystals as seeds and the SSN is coated with the polymer solution to obtain SSN@polymer.

[0036] Specifically, step S2 includes the following steps: S201: adding a polymer to the seed MOFs crystal solution of step S1 under stirring, stirring at a first set temperature for a first set time and standing for degassing to obtain a solution C; S202: coating solution C on SSN, allowing it to stand in water and washing it with clean water, and then drying it in a vacuum freeze drying oven to obtain SSN@polymer.

[0037] Due to the use of the first solvent and the second solvent in the present invention, the polymer can be directly added to the seed MOFs crystal solution after step S1, and due to the use of a mixed solution of different substances, the polymer can be well dissolved therein. In the present invention, the polymer is a polymer conventionally used in the art, for example, the polymer can be a mixture of one or more of polysulfone, polyethersulfone, polyimide or polyvinylidene fluoride. In addition, the amount of the polymer should be sufficient to completely cover the SSN. Therefore, in the present invention, the amount of the polymer used is 3 g-5 g. In the case of this amount, complete coverage of the SSN can be achieved, such as Figure 5 When the polymer is less than 3 g, as shown Figure 4 As shown, when coating SSN, the mesh of SSN cannot be completely covered, which affects the subsequent growth of MOFs crystals on the surface. Some MOFs crystals grow in the mesh of SSN instead of on the surface, resulting in an uneven MOFs crystal film. In the present invention, there is no particular restriction on the thickness of the polymer film, which is mainly affected by the thickness of SSN, and the thickness of the polymer film has little effect on the separation performance, and only serves to support the MOFs film.

[0038] After the polymer and the seed MOFs crystal solution are mixed, they need to be reacted under certain conditions for a period of time to obtain solution C. Specifically, the polymer and the seed MOFs crystal solution are stirred at a temperature of 50°C-90°C, and then allowed to stand for degassing for about 2 h-6 h. That is, in the present invention, the first set temperature is 50°C-90°C, and the first set time is 2 h-6 h.

[0039] In the present invention, there is no particular limitation on the metal mesh SSN as long as it can achieve a supporting function. For example, examples of the metal mesh include stainless steel mesh, copper mesh, and the like.

[0040] In addition, there is no particular restriction on the coating method, as long as the polymer solution mixed with MOFs crystals as seeds can be coated on the SSN, for example, a doctor blade film method can be used. In step S2, the SSN is completely covered by coating the polymer blended with MOFs crystal seeds, and the MOFs crystal seeds serve as nucleation sites for subsequent MOFs film layers, promoting the uniform growth of the MOFs film layers, wherein the SSN is similar to the bones of the human body and plays a supporting role.

[0041] Afterwards, step S3 is performed. Step S3 is a step of growing a MOFs crystal film layer on the SSN coated with a polymer. Therefore, step S3 specifically includes: S301: fully dissolving the second metal salt, the second organic ligand and the second regulator in a third solvent to obtain a solution D; S302: fix the SSN@polymer in step S2 in the solution D in step S301, perform ultrasonic degassing, and then let it stand to allow the solution to wet the SSN@polymer; S303: Pour the mixture of the SSN@polymer in step S302 and the solution D in step S301 into a high-pressure reactor containing a Teflon liner, and react at a third set temperature for a third set time to obtain a multi-level porous MOFs-on-SSN@polymer composite membrane.

[0042] In step S3, there is no particular restriction on the second metal salt, as long as it can provide the same metal ions as those in the first metal salt. That is, the metal ions in the second metal salt are the same as those in the first metal salt, and are one or more of zinc, cobalt, iron and nickel. In addition, the second metal salt is preferably a nitrate or a chloride, more preferably a chloride. The reason is that, relative to nitrates or sulfates, MOFs synthesized by chlorides are more conducive to growing into defect-free MOFs films. In addition, the mass of the second metal salt is 0.2 g-0.8 g.

[0043] In the present invention, the second organic ligand is the same as the first organic ligand, and can be 2-methylimidazole, benzimidazole, imidazole, 2-formylimidazole or 2-ethylimidazole. The mass of the second organic ligand is usually 0.4 g -0.6 g.

[0044] When performing step S3, that is, when growing a MOFs layer on the SSN@ polymer, if the MOFs crystallization speed is too fast, defects such as uneven grains will be generated, thereby affecting the separation performance of the final membrane. Therefore, in order to make the crystal growth more uniform, in step S301 of the present invention, a second regulator different from the above-mentioned first regulator is used. The second regulator is sodium formate, sodium acetate or sodium benzoate. Compared with the first regulator, the second regulator makes the MOFs crystallization relatively slow to ensure that the crystal growth is more uniform, thereby obtaining a uniform MOFs film layer. In order to achieve the desired effect, the mass of the second regulator is 1%-5% of the total mass of solution D.

[0045] In step S302, the SSN@ polymer is placed in the solution D in step S301, preferably vertically fixed in the solution D in step S301. This is mainly because the vertical fixing method can prevent the crystal particles from growing too large during the growth of MOFs, and the excess MOFs from settling on the surface of the MOFs membrane, affecting the subsequent cleaning.

[0046] In the present invention, in order to grow suitable MOFs crystals on the surface and regulate the MOFs crystal morphology, the third set temperature is controlled to 120°C-150°C, and the third set time is set to 6 h-12 h. Under the reaction conditions, the MOFs crystal film grown on the surface has a crystal size (i.e., film thickness) suitable for gas separation, providing a relatively short separation path, thereby improving the gas separation performance. The crystal size is substantially equal to the film thickness of MOFs, which is about 1 μm-5 μm.

[0047] After step S303, a MOFs-on-SSN@ polymer composite membrane is obtained. If the surface MOFs layer of the obtained MOFs-on-SSN@ polymer composite membrane is too thick, the path of gas permeation through the membrane becomes longer, the resistance becomes larger, and the gas separation performance is reduced. Therefore, the main separation layer of the MOFs-on-SSN@ polymer composite membrane is a MOFs layer with a thickness of 1 μm-5 μm.

[0048] After step S303, in order to effectively remove the residual substances on the surface of the MOFs-on-SSN@polymer composite membrane and further improve the gas separation performance of the obtained MOFs-on-SSN@polymer composite membrane, the preparation method of the present invention further includes: S304: The hierarchical MOFs-on-SSN@polymer composite membrane obtained in step S303 is rinsed and vacuum dried at room temperature for a fourth set time to obtain a dried hierarchical MOFs-on-SSN@polymer composite membrane.

[0049] In the present invention, the fourth set time is 12 h-24 h.

[0050] In the present invention, there is no particular limitation on the number of flushing and the solution used for flushing, as long as the MOFs particles deposited on the surface can be washed away. Conventional non-toxic and volatile reagents are generally used, for example, methanol or ethanol can be used for flushing multiple times to wash away the MOFs particles deposited on the surface and reduce contamination to subsequent tests.

[0051] The principle of the present invention is as follows: MOFs are a type of stable crystalline material formed by metal ions or metal clusters and organic ligands through coordination bonds. Figure 2The general structure of the MOFs material shown has a porous structure, and the pore size is related to the type of organic ligands. Usually, the MOFs materials with the same organic ligands have the same pore size. For example, the pore size of ZIF-8 is about 0.34 nm. The structure of MOFs can be regulated by selecting different metal ions and organic ligands to achieve selective adsorption and separation of gas molecules. The porous structure of MOFs provides a large number of adsorption sites, and the separation of gas molecules of different sizes and properties can be achieved by adjusting the pore size or pore structure. For example, ZIF-8 has high thermal and chemical stability, good screening performance for gas molecules, especially excellent separation performance for the separation of hydrogen (0.285 nm) and methane (0.376 nm).

[0052] The preparation method of the present invention is based on the principle of "like attracts like". First, a casting solution is prepared from MOFs crystals and a film-forming polymer, and then the casting solution is coated on the SSN. After molding, the polymer containing MOFs seeds is firmly adhered to the SSN, and finally it is placed in a MOFs precursor solution to induce the growth of a thin MOFs film layer to prepare a MOFs-on-SSN@polymer composite film. During the formation of the MOFs film layer, due to the presence of MOFs seeds on the surface of the polymer, according to the principle of "like attracts like", the MOFs ligands in the solution will gather near the seeds and nucleate and grow on the surface to form a MOFs film layer.

[0053] In addition, the present invention also provides a multi-level porous MOFs-on-SSN@polymer composite membrane, including an inner core, an intermediate layer and an outer shell, wherein the inner core is SSN, the intermediate layer is a polymer layer mixed with MOFs crystal seeds, and the outer shell is a MOFs membrane layer.

[0054] The pores of the multi-level porous MOFs-on-SSN@ polymer composite membrane include macropores formed by the polymer, which are usually submicron-sized, and micropores of the surface MOFs membrane layer, which are usually subnano-sized. During the preparation process, the polymer forms a three-dimensional network structure, thereby forming submicron-sized macropores, which do not have gas separation performance and only serve as gas circulation channels for rapid gas passage. The micropores of the MOFs membrane layer are subnano-sized pores that are essentially used for gas separation. Through the combination of the macropores of the polymer and the micropores of the MOFs membrane layer, a satisfactory gas separation effect can be achieved.

[0055] Figure 6 The composite membrane according to Example 1 of the present invention is shown. On the SSN coated with a polymer, due to the MOFs seeds blended in the polymer, based on the principle of "like attracts like", a high-quality MOFs crystal film grows on the surface, and the MOFs film layer has a uniform thickness.

[0056] In the multi-level porous MOFs-on-SSN@ polymer composite membrane prepared by the preparation method of the present invention, the SSN as the core mainly plays the role of a supporting layer, supporting the MOFs membrane, improving the strength of the membrane, and avoiding fracture; the polymer as the middle layer mainly provides a large number of MOFs seeds on the surface of the SSN to induce the growth of the MOFs membrane layer; the MOFs membrane layer as the outer layer mainly plays a role of separation. This preparation method is simple and can be prepared on a large scale, which is conducive to expanding the application range of MOFs membranes.

[0057] The preparation method of the present invention is further described below by way of examples.

[0058] The sources of the reagents used in the examples are as follows, and the materials or reagents not mentioned are also commercially available products: Zinc nitrate hexahydrate, Brand: Greagent, CAS No.: 10196-18-6, Parameter: ≥99.0% N,N-dimethylformamide, Brand: Greagent, CAS No.: 68-12-2, Parameter: ≥99.5% Ethanol, Brand: Adamas, CAS No.: 64-17-5, Parameter: 99.5% Triethylamine, Brand: Greagent, CAS No.: 121-44-8, Parameter: ≥99.0% 2-Methylimidazole, Brand: Adamas, CAS No.: 696-98-1, Parameter: 98% Zinc chloride, Brand: Greagent, CAS No.: 7646-85-7, Parameter: ≥98% Sodium formate, Brand: Adamas, CAS No.: 141-53-7, Parameter: >98% Methanol, Brand: Greagent, CAS No.: 67-56-1, Parameter: ≥99.7% Cobalt nitrate hexahydrate, Brand: Adamas, CAS No.: 10026-22-9, Parameter: 99% Polysulfone, Brand: BASF, CAS No.: 25135-51-7, Parameter: S6010.

[0059] Embodiment 1 S101. Dissolve 1.02 g of zinc nitrate hexahydrate in 50 mL of a mixed solution of N,N-dimethylformamide, ethanol, and water (the volume ratio of N,N-dimethylformamide, ethanol, and water is 8:1:1, and the density of the mixed solution is 0.948 g / cm 3 ), to obtain solution A; S102. Dissolve 1.1 g of 2-methylimidazole and 1.39 g of triethylamine in 50 mL of a mixed solution of N,N-dimethylformamide, ethanol, and water (the volume ratio of N,N-dimethylformamide, ethanol, and water is 8:1:1, and the density of the mixed solution is 0.948 g / cm 3 ) to obtain solution B; S103. Under vigorous stirring, solution A and solution B were thoroughly mixed to precipitate white crystalline powder ZIF-8; S201. 5.00 g of polysulfone was added to the mixed solution in step S103 under stirring, stirred at 50 ° C for 6 hours and allowed to stand for 2 hours to degas, to obtain a solution C; S202. Solution C was coated on a clean SSN to a thickness of 100 μm, and placed in water for 2 hours to displace the solvent, and washed with water several times, and then dried in a vacuum freeze dryer for 2 hours to obtain SSN@polysulfone; S301. 0.43 g of zinc chloride hexahydrate, 0.52 g of 2-methylimidazole and 0.22 g of sodium formate were fully dissolved in 40 mL of methanol solution to obtain solution D; S302. The SSN@polysulfone of step S202 is fixed vertically in solution D and ultrasonically degassed for 10 minutes, and then allowed to stand for half an hour to allow solution D to fully wet the SSN@polysulfone; S303. Pour the solution D and SSN@polysulfone in step S301 into a high pressure reactor containing a Teflon liner and react at 120° C. for 6 hours to obtain a hierarchical porous ZIF-8-on-SSN@polysulfone composite membrane; S304. The ZIF-8-on-SSN@polysulfone composite membrane obtained in step S303 is rinsed with ethanol several times, and vacuum dried at room temperature for 12 hours to obtain a dry ZIF-8-on-SSN@polysulfone composite membrane.

[0060] Embodiment 2 S101. Dissolve 1.02 g of cobalt nitrate hexahydrate in 50 mL of a mixed solution of N,N-dimethylformamide, ethanol, and water (the volume ratio of N,N-dimethylformamide, ethanol, and water is 8:1:1, and the density of the mixed solution is 0.948 g / cm 3 ), to obtain solution A; S102. Dissolve 1.1 g of 2-methylimidazole and 1.39 g of triethylamine in 50 mL of a mixed solution of N,N-dimethylformamide, ethanol, and water (the volume ratio of N,N-dimethylformamide, ethanol, and water is 8:1:1, and the density of the mixed solution is 0.948 g / cm 3 ) to obtain solution B; S103. Under vigorous stirring, solution A and solution B were thoroughly mixed to precipitate purple-red crystalline powder ZIF-67; S201. 5.00 g of polysulfone was added to the mixed solution in step S103 under stirring, stirred at 90 ° C for 12 hours and then allowed to stand for degassing for 2 hours to obtain a solution C; S202. Solution C was coated on a clean SSN to a thickness of 100 μm, and placed in water for 2 hours to displace the solvent, and washed with water several times, and then dried in a vacuum freeze dryer for 2 hours to obtain SSN@polysulfone; S301. 0.43 g of cobalt chloride hexahydrate, 0.52 g of 2-methylimidazole and 0.22 g of sodium benzoate were fully dissolved in 40 mL of methanol solution to obtain solution D; S302. The SSN@polysulfone of step S202 is fixed vertically in solution D and ultrasonically degassed for 10 minutes, and then allowed to stand for half an hour to allow solution D to fully wet the SSN@polysulfone; S303. The solution D and SSN@polysulfone in step S301 are poured into a high pressure reactor containing a Teflon liner, and reacted at 150° C. for 6 hours to obtain a ZIF-67-on-SSN@polysulfone composite membrane; S304. The ZIF-67-on-SSN@polysulfone composite membrane obtained in step S303 is rinsed with ethanol several times, and vacuum dried at room temperature for 12 hours to obtain a dry ZIF-67-on-SSN@polysulfone composite membrane.

[0061] Figure 6 The SEM image of the ZIF-8-on-SSN@polysulfone composite membrane of Example 1 is shown. It can be seen from the figure that a high-quality ZIF-8 crystal film is grown on the surface of the SSN coated with polysulfone (ie, SSN@polysulfone), and the thickness of the ZIF-8 film layer is substantially uniform, about 5 μm.

[0062] Gas separation performance test The gas separation performance of the MOFs-on-SSN@ polymer composite membrane prepared in the above embodiments was tested, specifically including: Gas permeation rate and separation factor test: Taking hydrogen as the research object, the MOFs-on-SSN@polymer composite membrane prepared in each example was tested using a laboratory-made gas separation test device.

[0063] The specific process is as follows: the MOFs-on-SSN@ polymer composite membrane prepared in each example is placed in a separation mold, and a mixture of hydrogen and methane (volume ratio of 1:1) is separated at 0.1 MPa and room temperature, and the hydrogen permeation and methane permeation are recorded. The membrane separation factor α is calculated by the following formula i / j : Where x and y represent the permeate gas and retained gas components, respectively, and i and j represent the front and back of the membrane, respectively. Composite film number <![CDATA[Permeation rate (mol·m -2 s -1 Pa -1 ).]]> Separation Factor Embodiment 1 <![CDATA[3.06×10 -6 ]]> 18.56 Embodiment 2 <![CDATA[2.34×10 -6 ]]> 16.84

[0064] The above results show that the gas separation performance of the MOFs-on-SSN@ polymer composite membrane prepared in each embodiment of the present invention is relatively good. The combination of the macropores of the polymer and the small pores of the MOFs material allows the gas to pass quickly, which is beneficial to the separation and purification of hydrogen.

[0065] The preferred specific embodiments of the present invention are described in detail above. It should be understood that ordinary technicians in this field can make many modifications and changes based on the concept of the present invention without creative work. Therefore, all technical solutions that can be obtained by technicians in this technical field through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the existing technology should be within the scope of protection determined by the claims.

Claims

1. A method for preparing a multi-level porous MOFs-on-SSN@polymer composite membrane, characterized in that: The following steps are involved: S1: preparing a seed MOFs crystal solution using a first metal salt, a first organic ligand and a first regulator; S2: adding the polymer to the seed MOFs crystal solution in step S1 to obtain solution C, coating solution C on SSN and treating to obtain SSN@polymer; S3: The second metal salt, the second organic ligand and the second regulator are mixed to obtain a solution D, the SSN@polymer in step S2 is placed in the solution D, and poured into a high-pressure reactor. After the reaction is completed, a multi-level porous MOFs-on-SSN@polymer composite membrane is obtained.

2. The method for preparing a multi-level porous MOFs-on-SSN@polymer composite membrane according to claim 1, characterized in that: Step S1 specifically includes: S101: dissolving a first metal salt in a first solvent to obtain a solution A; S102: dissolving the first organic ligand and the first regulator in a second solvent to obtain a solution B; S103: mixing solution A and solution B uniformly by stirring to precipitate crystal powder; Wherein, the first solvent and the second solvent are both mixed solutions of N,N-dimethylformamide, ethanol and water, and the volume ratio of N,N-dimethylformamide:ethanol:water is 6-9:1-3:1-3.

3. The method for preparing a multi-level porous MOFs-on-SSN@polymer composite membrane according to claim 2, characterized in that: In steps S101-S103, the metal ions in the first metal salt are one or more of zinc, cobalt, iron and nickel; the first organic ligand is 2-methylimidazole, benzimidazole, imidazole, 2-aldehyde imidazole or 2-ethylimidazole; the first regulator is triethylamine, aniline or ethylenediamine, and the mass of the first regulator is 1%-5% of the total mass of solution A and solution B.

4. The method for preparing a multi-level porous MOFs-on-SSN@polymer composite membrane according to claim 1, characterized in that: Step S2 specifically includes: S201: adding a polymer to the seed MOFs crystal solution of step S1 under stirring, stirring at a first set temperature for a first set time and standing for degassing to obtain a solution C; S202: coating solution C on SSN, standing in water and washing with clean water, and then drying in a vacuum freeze drying oven to obtain SSN@polymer; Wherein, the mass of the polymer is 3 g-5 g, the first set temperature is 50° C.-90° C., and the first set time is 2 h-6 h.

5. The method for preparing a multi-level porous MOFs-on-SSN@polymer composite membrane according to claim 1, characterized in that: Step S3 specifically includes: S301: dissolving a second metal salt, a second organic ligand and a second regulator in a third solvent to obtain a solution D; S302: fix the SSN@polymer in step S2 in the solution D in step S301, perform ultrasonic degassing, and then let it stand to allow the solution to wet the SSN@polymer; S303: pouring the mixture of the SSN@polymer in step S302 and the solution D in step S301 into a high-pressure reactor containing a Teflon liner, and reacting at a third set temperature for a third set time to obtain a multi-level porous MOFs-on-SSN@polymer composite membrane; Wherein, the metal ion in the second metal salt is the same as the metal ion in the first metal salt, the second organic ligand is the same as the first organic ligand, the third solvent is methanol, ethanol, a mixture of methanol and ethanol, or a mixture of methanol and water, the second regulator is sodium formate, sodium acetate or sodium benzoate, and the mass of the second regulator is 1%-5% of the total mass of solution D.

6. The method for preparing a multi-level porous MOFs-on-SSN@polymer composite membrane according to claim 5, characterized in that: The third set temperature is 120° C.-150° C., and the third set time is 6 h-12 h.

7. The method for preparing a multi-level porous MOFs-on-SSN@polymer composite membrane according to claim 5, characterized in that: Step S3 further comprises: S304: washing the multi-level porous MOFs-on-SSN@polymer composite membrane obtained in step S303, and vacuum drying it at room temperature for a fourth set time to obtain a dried multi-level porous MOFs-on-SSN@polymer composite membrane; Among them, the fourth setting time is 12 h-24 h.

8. The method for preparing a multi-level porous MOFs-on-SSN@polymer composite membrane according to claim 5, characterized in that: In step S302, the SSN@polymer is fixed in solution D in a vertical manner.

9. A hierarchical MOFs-on-SSN@ polymer composite membrane prepared by the preparation method according to any one of claims 1 to 8, characterized in that: It comprises a core, an intermediate layer and an outer shell, wherein the core is SSN, the intermediate layer is a polymer layer mixed with MOFs crystal seeds, and the outer shell is a MOFs film layer.

Citation Information

Cited By

  • Carbon dioxide gas selective separation composite membrane and preparation method thereof

    CN117732276A

  • Carbon dioxide gas selective separation composite membrane and preparation method thereof

    CN117732276B