Preparation method and application of CNTs (at) SiO2 (at) CeO2 composite membrane
Through the preparation method of CNTs@SiO2@CeO2 composite membrane, the problems of low efficiency and poor anti-pollution performance in the prior art are solved, and efficient oil-water separation and membrane stability are achieved, and suitable for treating oil-containing wastewater.
Patent Information
- Application Number
- CN202411213330.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-30
AI Technical Summary
When treating oil-containing wastewater, existing separation membranes have problems such as low separation efficiency, poor anti-pollution performance, high viscosity crude oil can easily cause channel blockage, and membrane flux decay too quickly, and cannot effectively deal with oil-containing wastewater with increased emissions.
Using the preparation method of CNTs@SiO2@CeO2 composite film, the CNTs, SiO2 and CeO2 nanoparticles are ultrasonicly mixed in an organic solvent to form composite particles, and combined with PVDF powder and pore-making agent. After heating, stirring and defoaming, The final obtained diaphragm is cleaned by deionized water to produce an anti-contamination composite membrane.
The filtering effect of oil-water separation and the recycling performance of the membrane are improved, the durability and separation performance of the membrane are enhanced, the channel is blocked, and more efficient oil-water separation and stable membrane performance are achieved.
Smart Images

Figure CN118987995A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of membrane separation, and specifically relates to a preparation method of a CNTs@SiO2@CeO2 composite membrane and application thereof. Background Art
[0002] With the development of industrial production, the increasing amount of oily wastewater and oil spills has caused serious water pollution and threatened the human ecological environment. Traditional oil removal technologies, namely gravity sedimentation, flotation, coagulation, adsorption, biological treatment and advanced oxidation processes, have problems such as low efficiency, high cost, complex process and secondary pollution, and cannot cope with the increasing amount of oily wastewater. In contrast, membrane filtration is regarded as the most effective method due to its advantages such as low energy cost, high efficiency, simple operation and environmental friendliness.
[0003] In recent decades, membrane separation technology has been widely used in the treatment of oily wastewater due to its advantages of low energy consumption, high efficiency and simple operation. Membrane separation technology removes pollutants of a certain particle size from water through specially made porous materials.
[0004] However, existing separation membranes generally have problems such as low separation efficiency, poor anti-pollution performance, high-viscosity crude oil easily causing pore blockage, and rapid membrane flux attenuation. Summary of the invention
[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0007] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a CNTs@SiO2@CeO2 composite film.
[0008] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing a CNTs@SiO2@CeO2 composite film, comprising:
[0009] Dispersing CNTs in deionized water and stirring to form a uniform CNTs dispersion solution;
[0010] SiO2 and CeO2 nanoparticles are added to the CNTs dispersion solution, ultrasonically mixed, and the composite particles are dried and ground to obtain composite particles;
[0011] The composite particles are added into an organic solvent and dispersed uniformly by ultrasonication to obtain a dispersion;
[0012] Adding PVDF powder and pore-forming agent into the dispersion, heating and stirring to obtain a casting solution, degassing, scraping the film, and obtaining a membrane sheet;
[0013] The obtained membrane piece is repeatedly washed in deionized water to remove the organic solvent remaining in the membrane, thereby obtaining the CNTs@SiO2@CeO2 composite membrane.
[0014] As a preferred embodiment of the preparation method of the present invention, the ratio of CNTs, SiO2 and CeO2 is 50-100 mg: 100-150 mg: 100-150 mg.
[0015] As a preferred embodiment of the preparation method of the present invention, the particle size of the composite particles is
[0016] As a preferred embodiment of the preparation method of the present invention, the organic solvent comprises a DMF solution.
[0017] As a preferred embodiment of the preparation method of the present invention, the ratio of the organic solvent to CNTs is 40-80 mL: 5-10 mg.
[0018] As a preferred embodiment of the preparation method of the present invention, the pore-forming agent comprises polyethylene glycol and polyvinyl pyrrolidone.
[0019] As a preferred solution of the preparation method of the present invention, the ratio of the PVDF powder to the pore-forming agent is 3-5 g: 0.1-0.3 g.
[0020] As a preferred embodiment of the preparation method of the present invention, the heating and stirring to obtain the casting liquid has a heating and stirring temperature of 50 to 70° C. and a stirring time of 6 to 8 hours.
[0021] Another object of the present invention is to overcome the deficiencies in the prior art and provide a CNTs@SiO2@CeO2 composite film prepared by a preparation method.
[0022] Another object of the present invention is to overcome the deficiencies in the prior art and provide a CNTs@SiO2@CeO2 composite membrane for use in separation of oil-water mixtures.
[0023] Beneficial effects of the present invention:
[0024] (1) The CNTs@SiO2@CeO2 composite membrane prepared by the method of the present invention is aimed at the problem that the composite membrane may be blocked and the membrane durability is poor in practical applications of membrane separation technology. A method for preparing an oil-water separation anti-pollution membrane is proposed. The prepared membrane has good oil filtering effect, good recycling performance, and is economical and practical.
[0025] (2) The present invention proposes a method for preparing a CNTs@SiO2@CeO2 composite membrane, wherein a CNTs@SiO2@CeO2 composite material is prepared and dispersed in an organic solvent. The composite effect of the two improves the filtration performance of the membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0027] Figure 1 This is a physical picture of the composite membrane obtained in the embodiment of the present invention.
[0028] Figure 2 The figure is a diagram showing the filtering effect of the composite membrane prepared in the embodiment of the present invention on different types of oil. DETAILED DESCRIPTION
[0029] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0030] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0031] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0032] The SiO2 nanoparticles in the present invention were purchased from Bisley New Materials; dimethylacetamide was purchased from Sinopharm Group; high-grade pure polyvinyl pyrrolidone (PVP-K30) was purchased from Sinopharm Group; CNTs were purchased from Chengdu Organic Chemistry Co., Ltd.; and CeO2 nanoparticles were purchased from Suzhou Yuante New Materials.
[0033] The composite separation membrane of the present invention is used to test the separation performance of oil-water mixture:
[0034] (1) Water flux test method: The water flux of the membrane is determined by the time it takes for 100 ml of pure water to pass through the composite membrane using a vacuum filtration device. The specific formula is:
[0035] In the formula, V(L), A(m 2 ), Δt(h) are the filtrate volume, effective membrane permeation area and filtration time respectively.
[0036] (2) Oil flux test method: The water flux of the membrane is determined by the time it takes for 100 ml of water-in-oil emulsion (kerosene emulsion, which is prepared by adding 990 ml of deionized water to a container and taking 30 mg of SDS as an emulsifier; then, adding 10 ml of kerosene to the above solution, ultrasonically stirring for 30 min, and then vigorously stirring for 6 h to obtain a surfactant-stabilized emulsion) to pass through the composite membrane using a vacuum filtration device. The specific formula is
[0037] Where V(L), A(m2), Δt(h), and ΔP(bar) are the filtrate volume, effective membrane permeation area, filtration time, and transmembrane pressure, respectively.
[0038] (3) Retention rate test method: Use a vacuum filtration device to pass 100 ml of water-in-oil emulsion (kerosene emulsion, prepared as above) through the composite membrane, and then use an infrared oil meter to measure the concentration of the solution before and after filtration. The specific formula is:
[0039] Among them C i (mg / L) and C0 (mg / L) are the oil contents in the filtered and original feed emulsions, respectively.
[0040] (4) Flux recovery rate test method: After filtering 100 ml of kerosene using a vacuum filtration device, the membrane was simply cleaned and the water flux was measured again. The formula is:
[0041] Among them, J W1 and J W2 are the pure water fluxes before and after filtering the emulsion, respectively.
[0042] Example 1
[0043] (1) Disperse 50 mg of CNTs into 50 ml of deionized water and stir at 25 °C for 100 min to form a uniform CNTs dispersion.
[0044] (2) Then, 100 mg of SiO2 and 100 mg of CeO2 nanoparticles were added to the CNTs dispersion solution and mixed uniformly by ultrasound. Subsequently, the composite particles were dry-ground to prevent particle agglomeration.
[0045] (3) The composite particles CNTs@SiO2@CeO2 were added into 40 ml of organic solvent DMF and then dispersed evenly under 60 W ultrasound for 60 min.
[0046] (4) Then, 3 g of PVDF powder and 0.1 g of PVP were added to the dispersion, heated and stirred for 6 h to obtain a casting solution, which was then allowed to stand for 12 h for degassing.
[0047] (5) After the casting solution is scraped with a scraper, the obtained membrane is immediately placed in deionized water for phase inversion. The membrane needs to be soaked in deionized water for more than 24 hours, and the water is changed every 2 hours to allow the solvent and non-solvent to be fully exchanged. Finally, a composite separation membrane with a thickness of 100 um is obtained. The actual picture of the composite membrane can be seen in Figure 1 .
[0048] Example 2
[0049] (1) Disperse 80 mg of CNTs into 50 ml of deionized water and stir at 25 °C for 120 min to form a uniform CNTs dispersion.
[0050] (2) Then, 120 mg of SiO2 nanoparticles and 120 mg of CeO2 were added to the CNTs dispersion solution and mixed uniformly by ultrasound. Subsequently, the composite particles were dry-ground to prevent particle agglomeration.
[0051] (3) The composite particles CNTs@SiO2@CeO2 were added into 50 ml of organic solvent DMF and then ultrasonicated at 60 W for 60 min to make them evenly dispersed.
[0052] (4) Then, 3 g of PVDF powder and 0.1 g of PVP were added to the dispersion, heated and stirred for 6 h to obtain a casting solution, which was then allowed to stand for 12 h for degassing.
[0053] (5) After the casting liquid is scraped with a scraper, the obtained membrane is immediately placed in deionized water for phase inversion. The membrane needs to be soaked in deionized water for more than 24 hours, and the water is changed every 2 hours to allow the solvent and non-solvent to be fully exchanged. Finally, the composite separation membrane thickness is 100um.
[0054] Example 3
[0055] (1) Disperse 100 mg of CNTs in 50 ml of deionized water and stir at 25 °C for 130 min to form a uniform CNTs dispersion.
[0056] (2) Then, 130 mg of SiO2 and 130 mg of CeO2 nanoparticles were added to the CNTs dispersion solution and mixed uniformly by 60 W ultrasound. Subsequently, the composite particles were dry-ground to prevent particle agglomeration.
[0057] (3) The obtained yellow crystals and SiO2 nanoparticles were added to 60 ml of ethanol solution, and then ultrasonic treatment was carried out for 90 minutes. The mixed solution after ultrasonication was baked at 90°C for 12 hours to obtain a composite material, and then ground into 1300 mesh in a mortar to reduce its agglomeration phenomenon, and then collected to obtain CNTs@SiO2@CeO2 material.
[0058] (4) Then, 3 g of PVDF powder and 0.1 g of PVP were added to the dispersion, heated and stirred for 6 h to obtain a casting solution, which was then allowed to stand for 12 h for degassing.
[0059] (5) After the casting liquid is scraped with a scraper, the obtained membrane is immediately placed in deionized water for phase inversion. The membrane needs to be soaked in deionized water for more than 24 hours, and the water is changed every 2 hours to allow the solvent and non-solvent to be fully exchanged. Finally, the composite separation membrane thickness is 100um.
[0060] The CNTs@SiO2@CeO2 composite separation membrane prepared in Example 1 was used to test the separation performance of oil-water mixture. Edible oil, n-hexane, kerosene, petroleum ether, and 1,2-dichloroethane were used as water-in-oil emulsions (990 mL of deionized water was added to the container, and 30 mg of SDS was taken as an emulsifier; then, 10 mL of the corresponding oil was added to the above solution, ultrasonically stirred for 30 minutes, and then vigorously stirred for 6 hours to obtain a surfactant-stabilized emulsion). The results are shown in Figure 2 ;
[0061] The CNTs@SiO2@CeO2 composite separation membrane prepared in the example was taken to test its water flux. The oil filtration effect and flux recovery rate are shown in Table 1 below.
[0062] Table 1
[0063] <![CDATA[Water flux (L / m 2 ·h)]]> <![CDATA[Oil flux (L / m 2 ·h)]]> Retention rate (%) Flux recovery rate (%) Example 1 2355 650.2 99.5 99.2 Example 2 2201 586.2 99.4 98.7 Example 3 2050 535.4 99.2 98.6
[0064] Comparative Example 1
[0065] (1) Disperse 50 mg of CNTs into 50 ml of deionized water and stir at 25 °C for 100 min to form a uniform CNTs dispersion.
[0066] (2) Then, 3 g of PVDF powder and 0.1 g of PVP were added to the dispersion, heated and stirred for 6 h to obtain a casting solution, which was then allowed to stand for 12 h for degassing.
[0067] (3) After the casting liquid is scraped with a scraper, the obtained membrane is immediately placed in deionized water for phase inversion. The membrane needs to be soaked in deionized water for more than 24 hours, and the water is changed every 2 hours to allow the solvent and non-solvent to be fully exchanged. Finally, the composite separation membrane thickness is 100um.
[0068] Comparative Example 2
[0069] (1) 100 mg of SiO2 and 100 mg of CeO2 nanoparticles were added to 50 ml of deionized water, and the mixture was uniformly mixed by ultrasound. The composite particles were dry-ground to prevent particle agglomeration.
[0070] (2) The composite particles SiO2@CeO2 were added into 40 ml of organic solvent DMF and then dispersed evenly under 60 W ultrasonic wave for 60 min.
[0071] (3) Then, 3 g of PVDF powder and 0.1 g of PVP were added to the dispersion, heated and stirred for 6 h to obtain a casting solution, which was then allowed to stand for 12 h for degassing.
[0072] (4) After the casting liquid is scraped with a scraper, the obtained membrane is immediately placed in deionized water for phase inversion. The membrane needs to be soaked in deionized water for more than 24 hours, and the water is changed every 2 hours to allow the solvent and non-solvent to be fully exchanged. Finally, the composite separation membrane thickness is 100um.
[0073] Comparative Example 3
[0074] (1) Disperse 50 mg of CNTs into 50 ml of deionized water and stir at 25 °C for 100 min to form a uniform CNTs dispersion.
[0075] (2) Then, 100 mg of SiO2 and 100 mg of CeO2 nanoparticles were added to the CNTs dispersion solution and mixed uniformly by ultrasound. Subsequently, the composite particles were dry-ground to prevent particle agglomeration.
[0076] (3) Add the composite particles CNTs@SiO2@CeO2 into 40 ml of organic solvent DMF and then disperse them evenly under 60W ultrasound for 60 min.
[0077] (4) Then, 3 g of PVDF powder was added to the dispersion, heated and stirred for 6 h to obtain a casting solution, and then allowed to stand for 12 h for degassing.
[0078] (5) After the casting liquid is scraped with a scraper, the obtained membrane is immediately placed in deionized water for phase inversion. The membrane needs to be soaked in deionized water for more than 24 hours, and the water is changed every 2 hours to allow the solvent and non-solvent to be fully exchanged. Finally, the composite separation membrane thickness is 100um.
[0079] The water flux was tested, and the filtering effect on oil and the flux recovery rate are shown in Table 2.
[0080] Table 2
[0081]
[0082] As can be seen from Table 2, the CNTs@SiO2@CeO2 composite separation membrane prepared in Example 1 was tested for oil-water mixture separation performance together with Comparative Examples 1, 2 and 3, and kerosene was used as the water-in-oil emulsion. As shown in Table 2, CNTs@SiO2@CeO2 has a continuous, uniform two-dimensional porous network, and nanoparticles can be loaded inside the network, which greatly improves the oil-water separation performance of the composite membrane and the stability of the membrane.
[0083] Carbon nanotubes (CNTs) have unique nanoscale pore structure and adjustable surface chemical properties. After SiO2@CeO2 is compounded, the potential points on the surface will match each other, making the composite particles very strong and durable.
[0084] Comparative Example 4
[0085] (1) Disperse 100 mg of CNTs into 50 ml of deionized water and stir at 25 °C for 100 min to form a uniform CNTs dispersion.
[0086] (2) Then, 100 mg of SiO2 and 100 mg of CeO2 nanoparticles were added to the CNTs dispersion solution and mixed uniformly by ultrasound. Subsequently, the composite particles were dry-ground to prevent particle agglomeration.
[0087] (3) Add the composite particles CNTs@SiO2@CeO2 into 40 ml of organic solvent DMF and then disperse them evenly by ultrasonication at 60 W for 60 min;
[0088] (4) Then, 3 g of PVDF powder and 0.1 g of PVP were added to the dispersion, heated and stirred for 6 h to obtain a casting solution, which was then allowed to stand for 12 h for degassing.
[0089] (5) After the casting liquid is scraped with a scraper, the obtained membrane is immediately placed in deionized water for phase inversion. The membrane needs to be soaked in deionized water for more than 24 hours, and the water is changed every 2 hours to allow the solvent and non-solvent to be fully exchanged. Finally, the composite separation membrane thickness is 100um.
[0090] Comparative Example 5
[0091] (1) Disperse 25 mg of CNTs into 50 ml of deionized water and stir at 25 °C for 100 min to form a uniform CNTs dispersion.
[0092] (2) Then, 100 mg of SiO2 and 100 mg of CeO2 nanoparticles were added to the CNTs dispersion solution and mixed uniformly by ultrasound. Subsequently, the composite particles were dry-ground to prevent particle agglomeration.
[0093] (3) The composite particles CNTs@SiO2@CeO2 were added into 40 ml of organic solvent DMF and then dispersed evenly under 60 W ultrasound for 60 min.
[0094] (4) Then, 3 g of PVDF powder and 0.1 g of PVP were added to the dispersion, heated and stirred for 6 h to obtain a casting solution, which was then allowed to stand for 12 h for degassing.
[0095] (5) After the casting liquid is scraped with a scraper, the obtained membrane is immediately placed in deionized water for phase inversion. The membrane needs to be soaked in deionized water for more than 24 hours, and the water is changed every 2 hours to allow the solvent and non-solvent to be fully exchanged. Finally, the composite separation membrane thickness is 100um.
[0096] Comparative Example 6 (200 mg CNTs)
[0097] (1) Disperse 200 mg of CNTs into 50 ml of deionized water and stir at 25 °C for 100 min to form a uniform CNTs dispersion.
[0098] (2) Then, 100 mg of SiO2 and 100 mg of CeO2 nanoparticles were added to the CNTs dispersion solution and mixed uniformly by ultrasound. Subsequently, the composite particles were dry-ground to prevent particle agglomeration.
[0099] (3) Add the composite particles CNTs@SiO2@CeO2 into 40 ml of organic solvent DMF and then disperse them evenly under 60W ultrasound for 60 min.
[0100] (4) Then, 3 g of PVDF powder and 0.1 g of PVP were added to the dispersion, heated and stirred for 6 h to obtain a casting solution, which was then allowed to stand for 12 h for degassing.
[0101] (5) After the casting liquid is scraped with a scraper, the obtained membrane is immediately placed in deionized water for phase inversion. The membrane needs to be soaked in deionized water for more than 24 hours, and the water is changed every 2 hours to allow the solvent and non-solvent to be fully exchanged. Finally, the composite separation membrane thickness is 100um.
[0102] The performance test results are shown in Table 3.
[0103] Table 3
[0104]
[0105] From Table 3, it can be concluded that adding too much or too little CNTs will affect the separation effect and water flux of the composite membrane. When too little CNTs is added, the water flux of the membrane will increase because there are fewer particles and the water channel of the membrane is not blocked. However, the separation effect of oily wastewater will deteriorate. This is because the oil contact angle of the membrane becomes smaller due to the low content of composite particles, and the resistance to oil will become weaker. However, adding too many particles will cause the particles to block the membrane and the water flux will decrease. Although the separation efficiency will be improved, on the whole, moderate addition of CNTs will give the best comprehensive separation effect.
[0106] The preparation method of the CNTs@SiO2@CeO2 separation membrane provided by the present invention has the following main principles: in the pore-forming method, pores are formed by using a pore-forming agent, polyvinyl pyrrolidone, to embed particles into the pores of the membrane. Since the zeta potential of silicon dioxide particles is negative and the zeta potential of cerium dioxide particles is positive, there is an attraction between SiO2 and CeO2. Since the CNTs material is a continuous and uniform two-dimensional porous network, SiO2 nanoparticles and CeO2 can be loaded on the CNTs grid to make the coating firm and stable, so the prepared composite membrane can achieve a good effect in oil-water separation.
[0107] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.
Claims
1. A method for preparing a CNTs@SiO2@CeO2 composite film, characterized in that: include, Dispersing CNTs in deionized water and stirring to form a uniform CNTs dispersion solution; SiO2 and CeO2 nanoparticles are added to the CNTs dispersion solution, ultrasonically mixed, and the composite particles are dried and ground to obtain composite particles; The composite particles are added into an organic solvent and dispersed uniformly by ultrasonication to obtain a dispersion; Adding PVDF powder and pore-forming agent into the dispersion, heating and stirring to obtain a casting solution, degassing, scraping the film, and obtaining a membrane sheet; The obtained membrane piece is repeatedly washed in deionized water to remove the organic solvent remaining in the membrane, thereby obtaining the CNTs@SiO2@CeO2 composite membrane.
2. The preparation method according to claim 1, characterized in that: The ratio of CNTs, SiO2 and CeO2 is 50-100mg:100-150mg:100-150mg.
3. The preparation method according to claim 1 or 2, characterized in that: The composite particles have a particle size of 2nm to 6nm.
4. The preparation method according to claim 1, characterized in that: The organic solvent includes a DMF solution.
5. The preparation method according to claim 4, characterized in that: The ratio of the organic solvent to CNTs is 40-80 mL: 5-10 mg.
6. The preparation method according to claim 1, characterized in that: The pore formers include polyethylene glycol and polyvinyl pyrrolidone.
7. The preparation method according to claim 1 or 6, characterized in that: The ratio of the PVDF powder to the pore-forming agent is 3-5 g: 0.1-0.3 g.
8. The preparation method according to claim 1, characterized in that: The heating and stirring process obtains a casting solution, wherein the heating and stirring temperature is 50 to 70° C. and the stirring time is 6 to 8 hours.
9. The CNTs@SiO2@CeO2 composite film obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the CNTs@SiO2@CeO2 composite membrane according to claim 9 in separation of oil-water mixture.
Citation Information
Patent Citations
Silicon-carbon composite, a method for preparing said composite, and an electrode material and a battery comprising said composite
CN107112504A
Polysulfate flat ultrafiltration membrane and preparation method thereof
CN111330452A
Method for preparing of polymer-carbon nanotube composite particles
KR1020120124611A
Manufacturing process for porous material
US20120034391A1
Method of forming self-assembled nanostructures
US20220347597A1