Preparation method of porous methanol synthesis catalyst

The porous methanol synthesis catalyst was prepared by the calcination-free method, which solved the problem of catalyst sintering and low porosity, achieved the combination of high catalytic performance and porous structure, and improved the diffusion of reaction raw materials and catalyst activity.

CN118988352APending Publication Date: 2024-11-22ANHUI CONCH IND TECHNOLOGY RESEARCH INSTITUTE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411098468.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing methanol synthesis catalysts are prone to sintering after the calcination step, resulting in a degradation of catalytic performance and forming a solid cylinder with low porosity and slow diffusion of reaction raw materials, making it difficult to contact the active sites of the catalyst.

Method used

The catalyst is prepared by the calcination-free method, and is pressed and molded by co-precipitation, aging, crushing and mixing with binder and lubricant, forming a porous structure, avoiding sintering, and suppressing the generation of hot spots through endothermic decomposition reaction during use.

Benefits of technology

The specific surface area and pore volume of the catalyst are improved, the catalytic performance is enhanced, the sintering situation is avoided, and the porous structure and strength of the catalyst are maintained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988352A_ABST
    Figure CN118988352A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a porous methanol synthesis catalyst. The preparation method comprises the following steps: mixing an aqueous solution containing a copper salt, a zinc salt and an aluminum salt with an alkali solution, and carrying out a co-precipitation reaction; aging a product of the co-precipitation reaction, and filtering to obtain a filter cake; and drying and crushing the filter cake, mixing the crushed filter cake with a binder and a lubricant, carrying out compression molding, and drying to obtain the methanol synthesis catalyst. The roasting step is omitted, and the preparation process is simple and easy to control; the prepared catalyst forms a porous structure in the hydrogen reduction process, that is, the hydrogenation reduction reaction of the metal oxide and the decomposition reaction of the basic carbonate are carried out in a linkage manner, so that the sintering condition of the catalyst is avoided, the specific surface area and the pore volume of the catalyst are effectively improved, and the catalytic performance of the catalyst is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a methanol synthesis catalyst, in particular to a method for preparing a porous methanol synthesis catalyst. Background Art

[0002] At present, the widely used methanol synthesis catalyst is a copper-based catalyst prepared by coprecipitation, and its main production process includes coprecipitation, aging, filtration, washing, drying, roasting, and molding. In order to solve the problem that the roasting step easily causes catalyst sintering and reduces catalytic performance, Chinese patent CN114073990A discloses a method for preparing a copper-based hydrogenation catalyst without roasting, in which the coprecipitation product is directly treated with hydrogen reduction, and then passivated in a mixed gas containing oxygen, and finally molded to obtain a catalyst. Although the invention omits the roasting step, the copper in the catalyst exists in the form of an oxidized state and needs to be reduced in situ before use. Since copper oxide hydrogenation reduction is a strong exothermic reaction, the concentration of hydrogen and the heating rate need to be strictly controlled during the process, otherwise it is very easy to run away and burn the reactor. Even if the overall temperature of the hydrogenation reduction reactor can be accurately controlled, the reduction process will still produce local hot spots on the catalyst, which will still cause the local microscopic particles of the catalyst to sinter and grow, resulting in a decrease in catalyst activity.

[0003] In addition, since the catalyst is usually pressed into a solid cylinder with a diameter and height of about 5 mm after calcination, its overall porosity is low, and the diffusion rate of the reaction raw materials into the interior of the catalyst is slow, making it difficult for the active sites inside the catalyst to contact the reaction raw materials, and only the outer layer of the catalyst is efficiently utilized. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide a method for preparing a methanol synthesis catalyst, so as to solve the problem of how to prepare a methanol synthesis catalyst with high catalytic performance. Another purpose of the present invention is to propose an application of the catalyst prepared by the above method in catalytic preparation of methanol, so as to solve the problem of how to catalytic preparation of methanol.

[0005] Technical solution: The method for preparing a methanol synthesis catalyst according to the present invention comprises the following steps:

[0006] (1) mixing an aqueous solution containing a copper salt, a zinc salt and an aluminum salt with an alkaline solution to carry out a coprecipitation reaction;

[0007] (2) aging the product of the coprecipitation reaction and filtering to obtain a filter cake;

[0008] (3) The filter cake is dried and crushed, mixed with a binder and a lubricant, and then pressed into a mold, and dried to obtain a methanol synthesis catalyst.

[0009] In the present invention, since there is no high-temperature roasting, the catalyst exists in the form of basic carbonate. In the subsequent use of the catalyst, an endothermic decomposition reaction occurs while the catalyst is reduced, offsetting the heat generated by partial reduction, thereby inhibiting the generation of local hot spots of the catalyst, preventing the catalyst from sintering, and improving the catalyst activity. In addition, the process of basic carbonate decomposition releases carbon dioxide and water, so that the catalyst becomes a porous structure, which is conducive to the diffusion of the reaction raw materials in the catalyst, so that the internal active sites of the catalyst can also be effectively utilized.

[0010] Preferably, in step (1), the copper salt includes one or more of copper nitrate, copper acetate, and copper acetylacetonate; the zinc salt includes one or more of zinc nitrate, zinc acetate, and zinc acetylacetonate; and the aluminum salt includes one or more of aluminum nitrate, aluminum acetate, and aluminum acetylacetonate.

[0011] Preferably, in step (1), the molar ratio of copper:zinc:aluminum in the aqueous solution containing copper salt, zinc salt and aluminum salt is 0.48-10:0.6-4.0:1.

[0012] Preferably, in step (1), the solute in the alkaline solution is one or more of sodium carbonate, potassium carbonate, ammonium carbonate, sodium bicarbonate, potassium bicarbonate, ammonium bicarbonate, sodium hydroxide, potassium hydroxide, and aqueous ammonia.

[0013] Preferably, in step (1), the concentration of the alkaline solution is 0.5-1.5 mol / L.

[0014] Preferably, in step (1), the coprecipitation reaction conditions are: controlling the pH at 6.0-8.0 and the temperature at 60-90°C during the precipitation process or at the end point.

[0015] Preferably, in step (2), the aging condition is aging at 60-90° C. for 0-3 h.

[0016] Preferably, in step (3), the binder includes one or more of calcium sulfate, magnesium sulfate, calcium nitrate, magnesium nitrate, calcium carbonate, magnesium carbonate, calcium oxide, magnesium oxide, calcium hydroxide, magnesium hydroxide, aluminum sol, and silica sol; the lubricant includes water, methanol, ethanol, isopropanol, graphite, C 6-12 One or more of the hydrocarbons.

[0017] In some embodiments, the amount of the binder is 3%-25%, and the amount of the lubricant is 1%-20%.

[0018] Due to the porous structure produced by decomposition, the catalyst strength decreases and is easy to break, so a binder needs to be added to increase the catalyst strength and maintain the catalyst structure. Traditional catalyst binders such as natural rubber, synthetic resin, stearic acid, asphalt, etc. are organic substances that cannot withstand the high temperature conditions of methanol synthesis, while inorganic binders such as cement and aluminum phosphate contain harmful components such as iron and phosphorus, which will greatly affect the catalyst activity and promote side reactions. Therefore, the role of the binder is mainly to improve the strength of the porous catalyst while ensuring that the catalytic performance is not affected.

[0019] Preferably, in step (3), the filter cake is dried at a temperature of 60-150°C, and the drying temperature after molding is 100-210°C.

[0020] The present invention further applies the catalyst prepared by the above preparation method to the preparation of methanol using CO2 and H2 as raw materials.

[0021] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:

[0022] 1. The present invention omits the roasting step, and the preparation process is simple and easy to control;

[0023] 2. The catalyst prepared by the present invention forms a porous structure during the hydrogen reduction process, which is equivalent to linking the hydrogenation reduction reaction of the metal oxide with the decomposition reaction of the basic carbonate, thereby avoiding the occurrence of catalyst sintering, effectively increasing the specific surface area and pore volume of the catalyst, and thus improving the catalytic performance of the catalyst.

[0024] 3. The present invention also utilizes a binder to maintain the porous structure of the catalyst without affecting the catalytic performance of the catalyst, thereby successfully making up for the defect that the strength decreases and affects the catalytic performance due to molding before high-temperature treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a microstructure diagram of the porous catalyst prepared in Example 1. DETAILED DESCRIPTION

[0026] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0027] Example 1: A method for preparing a methanol synthesis catalyst is as follows:

[0028] Weigh 0.15 mol of copper nitrate trihydrate, 0.09 mol of zinc acetate dihydrate, and 0.025 mol of aluminum nitrate nonahydrate, add 150 g of deionized water, stir and dissolve, and obtain a salt solution.

[0029] Weigh 0.25 mol of sodium carbonate, add 200 g of deionized water, stir and dissolve to obtain an alkaline solution.

[0030] The alkaline solution was heated to 70° C., and the salt solution was added to the alkaline solution under stirring, and the reaction temperature was maintained at 70° C. When the pH dropped to 6.5, the addition of the salt solution was stopped, and the temperature was maintained at 70° C. for aging for 1 hour.

[0031] The aged product was filtered and the filter cake was washed with deionized water until no Na + The filter cake was dried at 110°C for 12 hours and then crushed, mixed with 2g of magnesium sulfate and 1g of graphite, and pressed into a cylinder with a diameter of 5mm and a height of 5mm. After drying at 150°C for 7h, catalyst sample 1 was obtained. Figure 1 shown.

[0032] Example 2: A method for preparing a methanol synthesis catalyst is as follows:

[0033] Weigh 0.012 mol of copper nitrate trihydrate, 0.015 mol of zinc acetate dihydrate, and 0.025 mol of aluminum nitrate nonahydrate, add 150 g of deionized water, stir and dissolve to obtain a salt solution.

[0034] Weigh 0.1 mol of ammonium carbonate, add 200 g of deionized water, stir and dissolve to obtain an alkaline solution.

[0035] Heat the alkaline solution to 70° C., add the salt solution to the alkaline solution while stirring, and maintain the reaction temperature at 70° C. When the pH drops to 6.5, stop adding the salt solution.

[0036] The coprecipitated product was filtered and the filter cake was washed with deionized water until no NH4 was detected. + The filter cake was dried at 100°C for 6 hours, crushed, mixed with 2g of magnesium sulfate and 5g of water, and pressed into a cylinder with a diameter of 5mm and a height of 5mm. Catalyst sample 2 was obtained after drying at 100°C for 10 hours.

[0037] Example 3: A method for preparing a methanol synthesis catalyst is as follows:

[0038] Weigh 0.25 mol of copper acetate, 0.1 mol of zinc acetate dihydrate, and 0.025 mol of aluminum nitrate nonahydrate, add 150 g of deionized water, stir and dissolve to obtain a salt solution.

[0039] Weigh 0.3 mol of potassium carbonate, add it into 200 g of deionized water, stir and dissolve to obtain an alkaline solution.

[0040] The alkaline solution was heated to 80° C., and the salt solution was added to the alkaline solution under stirring, and the reaction temperature was maintained at 80° C. When the pH dropped to 8.0, the addition of the salt solution was stopped, and the aging was maintained at 80° C. for 1.5 hours.

[0041] The aged product was filtered and the filter cake was washed with deionized water until no K was detected. +The filter cake was dried at 180°C for 3 hours and then crushed, mixed with 3g of magnesium hydroxide and 4g of ethanol, and pressed into a cylinder with a diameter of 5mm and a height of 5mm. Catalyst sample 3 was obtained after drying at 210°C for 3h.

[0042] Example 4: A method for preparing a methanol synthesis catalyst is as follows:

[0043] Weigh 0.012 mol of copper acetate, 0.1 mol of zinc acetylacetonate, and 0.025 mol of aluminum acetylacetonate, add 150 g of deionized water, stir and dissolve to obtain a salt solution.

[0044] Weigh 0.2 mol of sodium bicarbonate, add 200 g of deionized water, stir and dissolve to obtain an alkaline solution.

[0045] The alkaline solution was heated to 60° C., and the salt solution was added to the alkaline solution under stirring, and the reaction temperature was maintained at 60° C. When the pH dropped to 6.0, the addition of the salt solution was stopped, and the aging was maintained at 60° C. for 2 hours.

[0046] The aged product was filtered and the filter cake was washed with deionized water until no Na + The filter cake was dried at 70°C for 12 hours and then crushed, mixed with 2g of calcium hydroxide and 5g of methanol, and pressed into a cylinder with a diameter of 5mm and a height of 5mm. Catalyst sample 4 was obtained after drying at 140°C for 5h.

[0047] Example 5: A method for preparing a methanol synthesis catalyst is as follows:

[0048] Weigh 0.25 mol of copper acetylacetonate, 0.015 mol of zinc nitrate hexahydrate, and 0.025 mol of aluminum acetate, add 150 g of deionized water, stir and dissolve to obtain a salt solution.

[0049] Weigh 0.2 mol of ammonium bicarbonate, add 200 g of deionized water, stir and dissolve to obtain an alkaline solution.

[0050] The alkaline solution was heated to 90° C., and the salt solution was added to the alkaline solution under stirring, and the reaction temperature was maintained at 90° C. When the pH dropped to 7.5, the addition of the salt solution was stopped, and the aging was maintained at 90° C. for 0.1 hour.

[0051] The aged product was filtered and the filter cake was washed with deionized water until no NH4 was detected. + The filter cake was dried at 150°C for 10 hours and then crushed, mixed with 2g of magnesium sulfate and 3g of n-hexane, and pressed into a cylinder with a diameter of 5mm and a height of 5mm. The catalyst sample 5 was obtained after drying at 170°C for 8h.

[0052] Comparative Example 1: The rest is the same as Example 1, except that:

[0053] No magnesium sulfate was added.

[0054] Comparative Example 2: The rest is the same as Example 1, except that:

[0055] After drying the filter cake at 110°C for 12 hours, it was reduced at 230°C for 10 minutes in a hydrogen-nitrogen mixed gas atmosphere containing 15% hydrogen. After cooling, it was reacted in an oxygen-nitrogen mixed gas atmosphere containing 2.0% oxygen for 5 minutes at a mixed gas space velocity of 2000 h -1 After the reaction, it is mixed with magnesium sulfate and graphite and pressed into a cylinder with a diameter of 5 mm and a height of 5 mm.

[0056] Comparative Example 3: The rest is the same as Example 1, except that:

[0057] The filter cake was dried at 110°C for 12 hours, calcined at 350°C for 3 hours in a nitrogen atmosphere, and after cooling, mixed with magnesium sulfate and graphite and pressed into a cylinder with a diameter of 5 mm and a height of 5 mm.

[0058] The samples prepared in Examples 1-5 and Comparative Examples 1-3 were tested for porous structure and catalytic performance as follows:

[0059] Catalytic performance test: The catalyst was tested for activity using a fixed bed high pressure microreactor, and the product composition was analyzed by gas chromatograph to calculate the selectivity of the reaction and the space-time yield of methanol. The catalyst samples of the embodiment and comparative example were crushed, passed through a 40-80 mesh sieve, and then 0.1 g was weighed and mixed with 0.4 g of quartz sand and loaded into a fixed bed reactor. Before the activity test, the catalyst was subjected to in-situ temperature reduction in an atmosphere of 20% H2-80% Ar by volume, and reduced at 250°C for 1 hour.

[0060] Reaction conditions for methanol synthesis: reaction pressure 2.0 MPa, reaction temperature 220°C, space velocity 24000 h -1 ;

[0061] The volume composition of the raw gas is: CO2=24%, Ar=4%, and the rest is H2.

[0062] The specific surface area and pore volume of the same catalyst before and after catalytic methanol synthesis were measured respectively.

[0063] The test results are as follows:

[0064] Table 1 Catalytic performance and porous structure test results of catalysts prepared by different preparation processes

[0065]

[0066] As can be seen from the results in Table 1, the catalytic performance of samples 1-5 is better than that of the comparative example. In comparative example 1, no binder was added. Under high temperature reaction, although the catalyst formed a porous structure, it collapsed and broke, resulting in that although the specific surface area of ​​the catalyst after the reaction was not significantly reduced compared with Example 1, the pore volume was significantly reduced.

[0067] The metal elements in the catalyst prepared in Comparative Example 2 are all in the form of oxides. In the early stage of the reaction, they are inevitably reduced by H2, resulting in local sintering of the catalyst. This can be seen from the fact that the specific surface area and pore volume of the catalyst after the reaction are significantly reduced compared with those in Example 1.

[0068] In Comparative Example 3, a calcination step was added, resulting in no decomposition of the basic carbonate during the reduction process, causing sintering of the catalyst, resulting in a smaller specific surface area and pore volume of the catalyst, and further resulting in poor catalytic performance.

[0069] Embodiment 6: All other aspects are the same as those of Embodiment 1, except that:

[0070] Using different binder types as variables, we observed the effect of binder on catalyst structure and performance. The test method was the same as above. The results are as follows:

[0071] Table 2 Effects of different binders on the catalytic performance and porous structure of catalysts

[0072]

[0073]

[0074] As can be seen from the results in Table 2, as binders for maintaining the porous structure, although magnesium sulfate, magnesium hydroxide, magnesium carbonate, magnesium hydroxide, and calcium oxide do not have a prominent maintenance effect, they do not significantly inhibit the activity of the catalyst. Although binders such as aluminum sol and silica sol can maintain the porous structure well, silicon and aluminum sol cover the active sites of the catalyst and produce acidic sites, resulting in a significant reduction in the catalytic performance of the catalyst. Therefore, the selection of the binder in the present invention is more important for the performance release of the catalyst.

Claims

1. A method for preparing a methanol synthesis catalyst, characterized in that: The steps include: (1) mixing an aqueous solution containing a copper salt, a zinc salt and an aluminum salt with an alkaline solution to carry out a coprecipitation reaction; (2) aging the product of the coprecipitation reaction and filtering to obtain a filter cake; (3) The filter cake is dried and crushed, mixed with a binder and a lubricant, and then pressed into a mold, and dried to obtain a methanol synthesis catalyst.

2. The method for preparing the methanol synthesis catalyst according to claim 1, characterized in that: In step (1), the copper salt includes one or more of copper nitrate, copper acetate, and copper acetylacetonate; the zinc salt includes one or more of zinc nitrate, zinc acetate, and zinc acetylacetonate; and the aluminum salt includes one or more of aluminum nitrate, aluminum acetate, and aluminum acetylacetonate.

3. The method for preparing the methanol synthesis catalyst according to claim 1, characterized in that: In step (1), the molar ratio of copper:zinc:aluminum in the aqueous solution containing copper salt, zinc salt and aluminum salt is 0.48-10:0.6-4.0:

1.

4. The method for preparing the methanol synthesis catalyst according to claim 1, characterized in that: In step (1), the solute in the alkaline solution is one or more of sodium carbonate, potassium carbonate, ammonium carbonate, sodium bicarbonate, potassium bicarbonate, ammonium bicarbonate, sodium hydroxide, potassium hydroxide, and aqueous ammonia.

5. The method for preparing the methanol synthesis catalyst according to claim 1, characterized in that: In step (1), the concentration of the alkaline solution is 0.5-1.5 mol / L.

6. The method for preparing the methanol synthesis catalyst according to claim 1, characterized in that: In step (1), the coprecipitation reaction conditions are: controlling the pH at 6.0-8.0 and the temperature at 60-90°C during the precipitation process or at the end point.

7. The method for preparing the methanol synthesis catalyst according to claim 1, characterized in that: In step (2), the aging condition is aging at 60-90° C. for 0-3 h.

8. The method for preparing the methanol synthesis catalyst according to claim 1, characterized in that: In step (3), the binder includes one or more of calcium sulfate, magnesium sulfate, calcium nitrate, magnesium nitrate, calcium carbonate, magnesium carbonate, calcium oxide, magnesium oxide, calcium hydroxide, magnesium hydroxide, aluminum sol, and silica sol; the lubricant includes water, methanol, ethanol, isopropanol, graphite, C 6-12 One or more of the hydrocarbons.

9. The method for preparing the methanol synthesis catalyst according to claim 1, characterized in that: In step (3), the filter cake is dried at a temperature of 60-150°C, and the drying temperature after molding is 100-210°C.

10. Use of the catalyst prepared according to the preparation method according to any one of claims 1 to 9 in preparing methanol using CO2 and H2 as raw materials.

Citation Information

Patent Citations

  • Method for preparing catalyst precursor for methanol synthesis

    CA2006758A1

  • Protective agent for methanol synthesis catalyst and preparation method and application of protective agent

    CN108854476A

  • Catalyst for preparing methanol through hydrogenation of carbon dioxide and preparation method and application thereof

    CN110327933A

  • Modified copper-based catalyst for acetylene hydrochlorination reaction and preparation method thereof

    CN111389423A

  • Preparation method of high-activity methanol synthesis catalyst

    CN112237916A