Preparation method of heterogeneous formic acid dehydrogenation catalyst and catalyst
Patent Information
- Application Number
- CN202410986688.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-23
AI Technical Summary
[0003]现有甲酸脱氢非均相催化剂存在以下不足:主要以贵金属钯、金为主,成本高昂,限制了甲酸储氢方法的应用;而非贵金属异相单原子催化剂在制备时需要高温煅烧,金属容易团聚,难以实现金属原子级分散
[0016]本发明具有如下有益效果:(1)本发明采用具有锌钴金属节点的ZIF-67前驱体吸附糠醇,然后使糠醇在框架材料内发生聚合形成聚糠醇,而聚糠醇作为新的支撑骨架有利于防止碳化导致的结构坍塌和催化活性成分钴的团聚,从而提升了催化剂中钴单原子的负载量,进而提升了单位质量的催化剂的催化性能。(2)本发明所制备的催化剂,在以丙烯碳酸脂(PC)为溶剂,反应温度为100℃下催化甲酸脱氢时可达778mL/gcat·h的产氢速率,即使在纯HCOOH条件下,仍有268mL/gcat·h的产氢速率,并展现出了良好的循环稳定性。
Smart Images

Figure CN118988368A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of formic acid dehydrogenation catalysis, and in particular to a preparation method and application of a heterogeneous formic acid dehydrogenation catalyst. Background Art
[0002] Formic acid (HCOOH) is a good hydrogen storage medium with high hydrogen storage capacity, non-toxicity, and a stable liquid compound at room temperature, which is convenient for storage and transportation. Formic acid can be synthesized through sustainable pathways such as carbon dioxide hydrogenation or partial oxidation of biomass, and can produce hydrogen under catalysis.
[0003] Existing heterogeneous catalysts for formic acid dehydrogenation have the following shortcomings: they are mainly based on precious metals palladium and gold, which are expensive and limit the application of formic acid hydrogen storage methods; and non-precious metal heterogeneous single-atom catalysts require high-temperature calcination during preparation, the metals are easy to agglomerate, and it is difficult to achieve metal atomic-level dispersion. The Co-NC catalyst reported by Beller et al. in 2017 has high selectivity for formic acid dehydrogenation, but its hydrogen production rate is still far behind that of precious metals palladium and gold. In 2020, they subsequently reported that ZIF-67 with a certain cobalt-zinc ratio was used as a precursor to prepare a Co single-atom catalyst. Compared with Co-NC, the performance is significantly improved, but the loading of single-atom cobalt is still low, which limits the improvement of catalytic performance. Therefore, how to prepare a formic acid dehydrogenation catalyst with a higher single-atom metal loading is a problem that needs to be further solved. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a heterogeneous formic acid dehydrogenation catalyst. The catalyst prepared by the method has a higher metal loading, higher catalytic selectivity and higher hydrogen production rate in a formic acid dehydrogenation reaction, and good cycle stability.
[0005] In order to achieve the above object, the present invention adopts the following technical scheme:
[0006] A method for preparing a heterogeneous formic acid dehydrogenation catalyst comprises the following steps:
[0007] Step S1: preparing a ZIF-67 precursor having zinc and cobalt metal nodes, wherein the molar ratio of zinc to cobalt elements is 5 to 15:1;
[0008] Step S2: using a ZIF-67 precursor to adsorb furfuryl alcohol in a furfuryl alcohol solution to obtain a precursor adsorbing furfuryl alcohol, wherein the mass fraction of furfuryl alcohol in the furfuryl alcohol solution is 10 to 100%;
[0009] Step S3: heating the precursor adsorbing furfuryl alcohol under an inert atmosphere to polymerize the furfuryl alcohol, and then heating to 800° C. under vacuum conditions with a circulating water pump to carbonize and volatilize zinc, thereby obtaining a heterogeneous formic acid dehydrogenation catalyst.
[0010] Preferably, in the step S1, a mixed solution of zinc salt and cobalt salt is first prepared, and the molar ratio of zinc to cobalt is 5 to 15:1; then a 2-methylimidazole solution is added to the mixed solution of zinc salt and cobalt salt, and stirred to generate a precipitate to obtain a ZIF-67 precursor having zinc and cobalt metal nodes; in the step S2, the ZIF-67 precursor is first heated to 300°C under an inert atmosphere for activation, and then the activated ZIF-67 precursor is immersed in a furfuryl alcohol solution to adsorb furfuryl alcohol to obtain a precursor adsorbing furfuryl alcohol; in the step S3, the precursor adsorbing furfuryl alcohol is first heated to 80°C under an inert gas atmosphere and maintained for 2 to 14 hours, and then heated to 150°C and maintained for 1 to 8 hours to polymerize furfuryl alcohol, and then heated to 800°C under vacuum conditions and maintained for 1 to 5 hours for carbonization.
[0011] Further preferably, in the step S1, the zinc salt and the cobalt salt are dissolved in methanol to prepare the mixed solution, and the mass ratio of the zinc salt to the volume of methanol is 1 g: 30-50 mL; then, a methanol solution of 2-methylimidazole is added to the mixed solution of the zinc salt and the cobalt salt, and the mass ratio of the 2-methylimidazole to the volume of methanol is 1 g: 10-15 mL, and the volume ratio of the mixed solution to the volume of the 2-methylimidazole methanol solution is 2: 1; in the step S2, the ZI The F-67 precursor is heated to 300° C. in an inert atmosphere and maintained for 1 to 3 hours for activation, and then the activated ZIF-67 precursor is immersed in a furfuryl alcohol solution to adsorb furfuryl alcohol to obtain a precursor adsorbing furfuryl alcohol; in the step S3, the precursor adsorbing furfuryl alcohol is first heated to 80° C. in an inert gas atmosphere and maintained for 2 to 14 hours, then heated to 150° C. and maintained for 1 to 8 hours to polymerize furfuryl alcohol, and then heated to 800° C. under vacuum conditions and maintained for 1 to 5 hours for carbonization.
[0012] Preferably, the zinc salt is zinc nitrate, zinc carbonate or zinc acetate, and the cobalt salt is cobalt nitrate, cobalt carbonate or cobalt acetate.
[0013] Preferably, in step S2, the activated ZIF-67 precursor is immersed in a furfuryl alcohol solution and subjected to room temperature ultrasound to adsorb the furfuryl alcohol.
[0014] Preferably, in step S1, the molar ratio of zinc to cobalt is 10:1; in step S2, the mass fraction of furfuryl alcohol in the furfuryl alcohol solution is 60%.
[0015] The present invention also provides a heterogeneous formic acid dehydrogenation catalyst, which is prepared by adopting the above preparation method.
[0016] The present invention has the following beneficial effects: (1) The present invention uses a ZIF-67 precursor with zinc-cobalt metal nodes to adsorb furfuryl alcohol, and then polymerizes furfuryl alcohol in the framework material to form polyfurfuryl alcohol. Polyfurfuryl alcohol as a new supporting skeleton is beneficial to prevent structural collapse caused by carbonization and agglomeration of the catalytic active ingredient cobalt, thereby increasing the loading amount of cobalt single atoms in the catalyst, and further improving the catalytic performance of the catalyst per unit mass. (2) The catalyst prepared by the present invention can reach 778 mL / g when catalyzing formic acid dehydrogenation at a reaction temperature of 100°C using propylene carbonate (PC) as a solvent. cat The hydrogen production rate is 268 mL / g even under pure HCOOH conditions. cat The hydrogen production rate was as high as 1.1 h and it exhibited good cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 Transmission electron microscope scanning images of the materials prepared in Examples 1-3 and Comparative Example 1;
[0018] Figure 2 XRD images of the materials prepared in Examples 1-3 and Comparative Example 1;
[0019] Figure 3 N of the materials prepared in Examples 1-3 and Comparative Example 1 2 Adsorption-desorption isotherms;
[0020] Figure 4 XPS images of the materials prepared in Example 1 and Comparative Example 1;
[0021] Figure 5 This is the X-ray absorption near edge structure spectrum (XANES) of CoNC-300-60% PFA;
[0022] Figure 6 a) Thermal gravimetric (TG) curves of 1:10ZIF-67, 1:10ZIF-67-300, 1:10ZIF-67-300-60% FA, and 1:10ZIF-67-300-60% PFA; b) Derivative thermogravimetric (DTG) curves; c) Infrared spectra of 1:10ZIF-67, 1:10ZIF-67-300, 1:10ZIF-67-300-60% FA, 1:10ZIF-67-300-60% PFA and 2-methylimidazole.
[0023] Figure 7 This is a diagram for analyzing the catalytic stability of CoNC-300-60% PFA single atom catalyst. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below in conjunction with embodiments:
[0025] Example 1 Preparation of Heterogeneous Formic Acid Dehydrogenation Catalyst CoNC-300-60% PFA
[0026] Step S1: Weigh 2.02 g (6.8 mmol) of Zn(NO 3 ) 2 6H 2 O and 197mg(0.68mmol)Co(NO 3 ) 2 6H 2 O (zinc-cobalt molar ratio of 10:1) was added to 80 ml of methanol solution and stirred to completely dissolve to prepare a zinc-cobalt mixed solution; 3.0 g (36.5 mmol) of 2-methylimidazole was weighed and dissolved in 40 ml of methanol to prepare a solution, and then the solution was slowly poured into the zinc-cobalt mixed solution, stirred for 24 hours, centrifuged, washed with methanol, and vacuum dried to obtain a metal framework compound ZIF-67 precursor with zinc and cobalt as metal nodes;
[0027] Step S2: The ZIF-67 precursor was transferred to a ceramic boat and placed in a tube furnace under N 2 The reaction mixture was heated to 300°C at a heating rate of 2°C / min under an aqueous atmosphere, maintained for 2 hours, and then naturally cooled to room temperature to obtain an activated precursor, recorded as ZIF-67-300; 5.11 mL of furfuryl alcohol and 4.89 mL of methanol were mixed to obtain a methanol solution of furfuryl alcohol (the mass fraction of furfuryl alcohol was 60%), and ZIF-67-300 was immersed in the methanol solution of furfuryl alcohol to adsorb furfuryl alcohol, ultrasonicated for 40 minutes, and allowed to stand at room temperature overnight. The methanol was then removed by reduced pressure distillation to obtain the precursor ZIF-67-300-60% adsorbed with furfuryl alcohol.
[0028] Step S3: The precursor ZIF-67-300-60% adsorbed with furfuryl alcohol was heated to 40 ℃ and then heated to 30 ℃ and then heated to 40 ℃ and then heated to 30 ℃ and then heated to 50 ℃ and then heated to 8 ... 2 The temperature was raised to 80°C at a heating rate of 2°C / min under atmosphere and maintained for 14 hours, then raised to 150°C and maintained for 6 hours to polymerize furfuryl alcohol into polyfurfuryl alcohol, and the obtained sample was recorded as ZIF-67-300-60% PFA; then, ZIF-67-300-60% PFA was heated to 800°C under vacuum conditions of a circulating water vacuum pump for carbonization and volatilization of zinc, the heating rate was 5°C / min, maintained for 3 hours, and naturally cooled to room temperature to obtain a heterogeneous formic acid dehydrogenation catalyst, recorded as CoNC-300-60% PFA.
[0029] Example 2 Preparation of Heterogeneous Formic Acid Dehydrogenation Catalyst CoNC-300-10% PFA
[0030] Step S1: Weigh 2.02 g (6.8 mmol) of Zn(NO 3 )2 6H 2 O and 197mg(0.68mmol)Co(NO 3 ) 2 6H 2 O (zinc-cobalt molar ratio of 10:1) was added to 80 ml of methanol solution and stirred to completely dissolve to prepare a zinc-cobalt mixed solution; 3.0 g (36.5 mmol) of 2-methylimidazole was weighed and dissolved in 40 ml of methanol to prepare a solution, and then the solution was slowly poured into the zinc-cobalt mixed solution, stirred for 24 hours, centrifuged, washed with methanol, and vacuum dried to obtain a metal framework compound ZIF-67 precursor with zinc and cobalt as metal nodes;
[0031] Step S2: The ZIF-67 precursor was transferred to a ceramic boat and placed in a tube furnace under N 2 The reaction mixture was heated to 300°C at a heating rate of 2°C / min under an aqueous atmosphere, maintained for 2 hours, and then naturally cooled to room temperature to obtain an activated precursor, recorded as ZIF-67-300; 0.72 mL of furfuryl alcohol and 9.28 mL of methanol were mixed to obtain a methanol solution of furfuryl alcohol (the mass fraction of furfuryl alcohol was 10%), and ZIF-67-300 was immersed in the methanol solution of furfuryl alcohol to adsorb furfuryl alcohol, ultrasonicated for 40 minutes, and allowed to stand at room temperature overnight. The methanol was then removed by reduced pressure distillation to obtain the precursor ZIF-67-300-10% adsorbed with furfuryl alcohol.
[0032] Step S3: The precursor ZIF-67-300-10% adsorbed with furfuryl alcohol was heated to 400 °C in N 2 The temperature was raised to 80°C at a heating rate of 2°C / min under an atmosphere and maintained for 14 hours, and then raised to 150°C and maintained for 6 hours to polymerize furfuryl alcohol into polyfurfuryl alcohol. The obtained sample was recorded as ZIF-67-300-10% PFA. Then, ZIF-67-300-10% PFA was heated to 800°C under vacuum conditions of a circulating water vacuum pump for carbonization and volatilization of zinc. The heating rate was 5°C / min and maintained for 3 hours. The catalyst was naturally cooled to room temperature to obtain a heterogeneous formic acid dehydrogenation catalyst, which was recorded as CoNC-300-10% PFA.
[0033] Example 3 Preparation of heterogeneous formic acid dehydrogenation catalyst ZIF-67-300-100%
[0034] Step S1: Weigh 2.02 g (6.8 mmol) of Zn(NO 3 ) 2 6H 2 O and 197mg(0.68mmol)Co(NO 3 ) 2 6H 2O (zinc-cobalt molar ratio of 10:1) was added to 80 ml of methanol solution and stirred to completely dissolve to prepare a zinc-cobalt mixed solution; 3.0 g (36.5 mmol) of 2-methylimidazole was weighed and dissolved in 40 ml of methanol to prepare a solution, and then the solution was slowly poured into the zinc-cobalt mixed solution, stirred for 24 hours, centrifuged, washed with methanol, and vacuum dried to obtain a metal framework compound ZIF-67 precursor with zinc and cobalt as metal nodes;
[0035] Step S2: The ZIF-67 precursor was transferred to a ceramic boat and placed in a tube furnace under N 2 The reaction mixture was heated to 300°C at a heating rate of 2°C / min under an aqueous atmosphere, maintained for 2 hours, and then naturally cooled to room temperature to obtain an activated precursor, recorded as ZIF-67-300; 10 mL of furfuryl alcohol (the mass fraction of furfuryl alcohol is 100%) was measured, and ZIF-67-300 was immersed in furfuryl alcohol to adsorb furfuryl alcohol, and ultrasonicated for 40 minutes to obtain the precursor ZIF-67-300-100% adsorbed furfuryl alcohol.
[0036] Step S3: The precursor ZIF-67-300-100% adsorbed with furfuryl alcohol was heated to 400 °C in N 2 The temperature was raised to 80°C at a heating rate of 2°C / min under an atmosphere and maintained for 14 hours, and then raised to 150°C and maintained for 6 hours to polymerize furfuryl alcohol into polyfurfuryl alcohol. The obtained sample was recorded as ZIF-67-300-100% PFA. Then, ZIF-67-300-100% PFA was heated to 800°C under vacuum conditions of a circulating water vacuum pump for carbonization and volatilization of zinc. The heating rate was 5°C / min and maintained for 3 hours. The catalyst was naturally cooled to room temperature to obtain a heterogeneous formic acid dehydrogenation catalyst, which was recorded as CoNC-300-100% PFA.
[0037] Example 4 Preparation of Heterogeneous Formic Acid Dehydrogenation Catalyst CoNC-300-60% FA Step S1: Weigh 2.02 g (6.8 mmol) of Zn(NO 3 ) 2 6H 2 O and 197mg(0.68mmol)Co(NO 3 ) 2 6H 2 O (zinc-cobalt molar ratio of 10:1) was added to 80 ml of methanol solution and stirred to completely dissolve to prepare a zinc-cobalt mixed solution; 3.0 g (36.5 mmol) of 2-methylimidazole was weighed and dissolved in 40 ml of methanol to prepare a solution, and then the solution was slowly poured into the zinc-cobalt mixed solution, stirred for 24 hours, centrifuged, washed with methanol, and vacuum dried to obtain a metal framework compound ZIF-67 precursor with zinc and cobalt as metal nodes;
[0038] Step S2: The ZIF-67 precursor was transferred to a ceramic boat and placed in a tube furnace under N 2 The reaction mixture was heated to 300°C at a heating rate of 2°C / min under an aqueous atmosphere, maintained for 2 hours, and then naturally cooled to room temperature to obtain an activated precursor, recorded as ZIF-67-300; 5.11 mL of furfuryl alcohol and 4.89 mL of methanol were mixed to obtain a methanol solution of furfuryl alcohol (the mass fraction of furfuryl alcohol was 60%), and ZIF-67-300 was immersed in the methanol solution of furfuryl alcohol to adsorb furfuryl alcohol, ultrasonicated for 40 minutes, and allowed to stand at room temperature overnight. The methanol was then removed by reduced pressure distillation to obtain the precursor ZIF-67-300-60% adsorbed with furfuryl alcohol.
[0039] Step S3: The precursor ZIF-67-300-60% adsorbing furfuryl alcohol is heated to 800°C under vacuum conditions of a circulating water vacuum pump for carbonization and volatilization of zinc, with a heating rate of 5°C / min, maintained for 3 hours, and naturally cooled to room temperature to obtain a heterogeneous formic acid dehydrogenation catalyst, recorded as CoNC-300-60% FA.
[0040] In this embodiment, in step S3, no heating steps are set at 80°C and 150°C to polymerize furfuryl alcohol, but furfuryl alcohol may still polymerize during the process of heating to 800°C.
[0041] Comparative Example 1 Preparation of CoNC-300 without impregnation with furfuryl alcohol
[0042] Step S1: Weigh 2.02 g (6.8 mmol) of Zn(NO 3 ) 2 6H 2 O and 197mg(0.68mmol)Co(NO 3 ) 2 6H 2 O (zinc-cobalt molar ratio of 10:1) was added to 80 ml of methanol solution and stirred to completely dissolve to prepare a zinc-cobalt mixed solution; 3.0 g (36.5 mmol) of 2-methylimidazole was weighed and dissolved in 40 ml of methanol to prepare a solution, and then the solution was slowly poured into the zinc-cobalt mixed solution, stirred for 24 hours, centrifuged, washed with methanol, and vacuum dried to obtain a metal framework compound ZIF-67 precursor with zinc and cobalt as metal nodes;
[0043] Step S2: The ZIF-67 precursor was transferred to a ceramic boat and placed in a tube furnace under N 2 The reaction mixture was heated to 300°C at a heating rate of 2°C / min under an atmosphere, maintained for 2 h, and then naturally cooled to room temperature to obtain an activated precursor, which was designated as ZIF-67-300.
[0044] Step S3: ZIF-67-300 is heated to 800°C under vacuum conditions of a circulating water vacuum pump to carbonize and volatilize zinc. The heating rate is 5°C / min and maintained for 3 hours. The mixture is naturally cooled to room temperature. The obtained material is recorded as CoNC-300.
[0045] Comparative Example 2 Preparation of CoNC without activation and furfuryl alcohol impregnation
[0046] Step S1: Weigh 2.02 g (6.8 mmol) of Zn(NO 3 ) 2 6H 2 O and 197mg(0.68mmol)Co(NO 3 ) 2 6H 2 O (zinc-cobalt molar ratio of 10:1) was added to 80 ml of methanol solution and stirred to completely dissolve to prepare a zinc-cobalt mixed solution; 3.0 g (36.5 mmol) of 2-methylimidazole was weighed and dissolved in 40 ml of methanol to prepare a solution, and then the solution was slowly poured into the zinc-cobalt mixed solution, stirred for 24 hours, centrifuged, washed with methanol, and vacuum dried to obtain a metal framework compound ZIF-67 precursor with zinc and cobalt as metal nodes;
[0047] Step S2: ZIF-67 was heated to 800°C under vacuum conditions of a circulating water vacuum pump for carbonization and volatilization of zinc. The heating rate was 5°C / min and maintained for 3 hours. The mixture was naturally cooled to room temperature. The obtained material was recorded as CoNC.
[0048] Characterization analysis
[0049] The materials prepared in Examples 1-4 and Comparative Examples 1-2 were characterized and analyzed.
[0050] (1) Transmission electron microscopy (TEM)
[0051] like Figure 1 As shown in a, b, and c, CoNC-300-60% PFA, CoNC-300-10% PFA, and CoNC-300-100% PFA prepared from ZIF-67 impregnated with furfuryl alcohol maintain their structural stability. As the furfuryl alcohol content increases, the metal content decreases and can be identified as metallic Co elemental substance (0.206 nm) by the lattice (0.206 nm). When the furfuryl alcohol content increases to 60% w / w, no Co metal nanoparticles with a crystalline structure are observed in the material ( Figure 1 a), indicating that Co is highly dispersed in the form of single atoms; when the furfuryl alcohol content is 10% or 100%, Co nanoparticles ( Figure 1 b. Figure 1c), indicating that the cobalt is not all present in the form of single atoms. Figure 1 As shown in (d), the Co / NC-300 prepared from ZIF-67 without furfuryl alcohol impregnation did not maintain the rhombic dodecahedral structure of ZIF-67.
[0052] (2) X-ray diffraction (XRD)
[0053] like Figure 2 As shown, in the XRD characterization of CoNC-300-60% PFA, CoNC-300-10% PFA, CoNC-300-100% PFA, and Co / NC-300, there is only the characteristic (002) plane of amorphous carbon at around 20°, so no diffraction peaks of Co-based compounds were found in the samples, indicating that the Co species are highly dispersed in the carbon matrix.
[0054] (3)N 2 Adsorption-desorption isotherms
[0055] CoNC-300-10% PFA, CoNC-300-60% PFA, CoNC-300-100% PFA, and Co / NC-300 all exhibit similar pore structures. Figure 3 It can be seen that the specific surface area of Co / NC-300 prepared without furfuryl alcohol impregnation is 225 m 2 ·g -1 The macropores are significantly reduced, which is because the sample does not maintain the morphology of ZIF-67. The specific surface areas of CoNC-300-10% PFA, CoNC-300-60% PFA, and CoNC-300-100% PFA are 378, 539, and 587 m 2 ·g -1 The nitrogen adsorption and desorption isotherms of CoNC-300-60% PFA have H4-type hysteresis loops and have a high specific surface area of 539m 2 ·g -1 , which helps to improve the catalytic performance of HCOOH dehydrogenation. (4) X-ray electron spectroscopy (XPS)
[0056] X-ray electron spectroscopy (XPS) was used to characterize the elemental composition and element valence state of CoNC-300-60%PFA and Co / NC-300 materials. Figure 4 As shown in a, the material mainly includes five elements: Co, Zn, C, N, and O. The peaks of 1021eV, 781eV, 531eV, 398eV, and 284eV belong to Zn 2p, Co 2p, O 1s, N 1s, and C1s, respectively. Figure 4 As shown in b, the fitting peak at 779.6 eV in the high-resolution Co 2p spectrum belongs to Co 0, the four fitting peaks at 780.8 / 796.5eV and 785.2 / 802.3eV belong to Co-N and the corresponding satellite signals, respectively. However, there is no Co in the XPS results of CoNC-300-60%PFA. 0 , this result is further confirmed by HRTEM images.
[0057] (5) X-ray absorption near-edge structure spectroscopy (XANES)
[0058] X-ray absorption near-edge structure (XANES) spectroscopy, such as Figure 5 As shown in a, the absorption edge of CoNC-300-60%PFA is located between the Co foil and Co 3 O 4 , indicating that the Co species in CoNC-300-60%PFA may be covalently bonded with N. Figure 5 b and 5c, the corresponding R space is obtained from the FEK3 weighted Fourier transform (FT), showing the bond lengths of the Co species. The curve of CoNC-300-60%PFA shows that There is a typical peak at , which may be attributed to the Co-N bond in the first shell. No Co-Co signal and Co-O signal were detected at the 30°C region. The results showed that the Co in CoNC-300-60%PFA was atomically dispersed and stable.
[0059] (6) Thermogravimetric analysis and infrared spectra
[0060] Figure 6 a, b are the thermogravimetric (TG) curves of 1:10ZIF-67, 1:10ZIF-67-300, 1:10ZIF-67-300-60%FA, and 1:10ZIF-67-300-60%PFA, respectively. Figure 6 a); b Derivative thermogravimetric (DTG) curve ( Figure 6 b) (1:10 is the molar ratio of cobalt to zinc).
[0061] Figure 6 a, b show that at 200 °C, due to the decomposition of dimethylimidazole, NH 3, 1:10ZIF-67 shows a more obvious weight loss than other materials. All materials experience significant weight loss at 650°C due to the carbonization and nitridation process of ZIF-67. At 850°C, most materials lose weight because Zn evaporates mainly in the form of Zn vapor. Comparing the total thermal analysis results of 1:10ZIF-67, 1:10ZIF-67-300, 1:10ZIF-67-300-60% FA, and 1:10ZIF-67-300-60% PFA, it can be seen that the introduction of polyfurfuryl alcohol has a significant effect on the calcination process of ZIF-67 precursor. The formation of polyfurfuryl alcohol in the body effectively reduces the loss of carbon and nitrogen elements during calcination and promotes the formation of high-density single-atom active sites.
[0062] Figure 6 c Infrared spectra of 1:10ZIF-67, 1:10ZIF-67-300, 1:10ZIF-67-300-60%FA, 1:10ZIF-67-300-60%PFA and 2-methylimidazole, respectively. Infrared image ( Figure 6 c) shows that 1:10ZIF-67-300-60%FA and 1:10ZIF-67-300-60%PFA are -1 There is a peak at , which proves that furfuryl alcohol and polyfurfuryl alcohol are successfully incorporated into the internal pore structure of the precursor.
[0063] Catalytic performance analysis
[0064] (1) The catalytic performance of the materials prepared in Examples 1-4 and Comparative Examples 1-2 was analyzed respectively.
[0065] First, check the air tightness of the gas measuring tube connected to the reaction device, then add 10 mL of propylene carbonate into the reaction bottle, add 562 μL of formic acid, start stirring and heating, wait until the temperature stabilizes at 100 °C, and after the device stabilizes, add 50 mg of catalyst, start reading, read once every 10 minutes, and record for a total of 2 hours. The results are shown in Table 1.
[0066] Table 1 Catalyst hydrogen production efficiency
[0067]
[0068] As can be seen from Table 1, the CoNC-300-60% PFA prepared by the present invention exhibits a kinetic energy of 778 mL / g at a reaction temperature of 100°C using propylene carbonate (PC) as solvent. cat·h hydrogen production rate; when the ratio of furfuryl alcohol to methanol was changed, the catalytic hydrogen production efficiency of CoNC-300-10% PFA and CoNC-100% PFA prepared was reduced; when furfuryl alcohol impregnation was not performed, the catalytic hydrogen production efficiency of CoNC-300 prepared was only 451mL / g cat h, the catalytic hydrogen production efficiency is significantly lower than that of CoNC-300-60% PFA. For CoNC-300-60% FA prepared in Example 4, its catalytic hydrogen production efficiency is 665 mL / g cat h, slightly lower than 778 mL / g of CoNC-300-60% PFA cat ·h, which indicates that the polymerization of furfuryl alcohol by heating at 80℃ and 150℃ contributes to the improvement of catalytic performance. When activation and furfuryl alcohol impregnation are not performed, the catalytic hydrogen production efficiency of the prepared CoNC is only 226mL / g cat ·h, the catalytic hydrogen production efficiency is significantly lower than that of CoNC-300-60%PFA.
[0069] (2) CoNC-300-60% PFA catalyst stability test
[0070] like Figure 7 As shown, the CoNC-300-60% PFA catalyst was repeatedly used in PC at 100°C. After three uses, washing and drying, the catalyst still showed high activity and stability.
Claims
1. A method for preparing a heterogeneous formic acid dehydrogenation catalyst, Features The steps include: Step S1: preparing a ZIF-67 precursor having zinc and cobalt metal nodes, wherein the molar ratio of zinc to cobalt elements is 5 to 15:1; Step S2: using a ZIF-67 precursor to adsorb furfuryl alcohol in a furfuryl alcohol solution to obtain a precursor adsorbing furfuryl alcohol, wherein the mass fraction of furfuryl alcohol in the furfuryl alcohol solution is 10 to 100%; Step S3: heating the precursor adsorbing furfuryl alcohol under an inert atmosphere to polymerize furfuryl alcohol, and then heating to 800° C. under vacuum conditions to carbonize and volatilize zinc to obtain a heterogeneous formic acid dehydrogenation catalyst; or directly heating the precursor adsorbing furfuryl alcohol to 800° C. under vacuum conditions to carbonize and volatilize zinc to obtain a heterogeneous formic acid dehydrogenation catalyst.
2. The method for preparing the heterogeneous formic acid dehydrogenation catalyst according to claim 1, Features: In the step S1, a mixed solution of zinc salt and cobalt salt is first prepared, wherein the molar ratio of zinc to cobalt is 5 to 15:1; then a 2-methylimidazole solution is added to the mixed solution of zinc salt and cobalt salt, and the mixture is stirred to generate a precipitate to obtain a ZIF-67 precursor having zinc and cobalt metal nodes; In the step S2, the ZIF-67 precursor is firstly heated to 300° C. in an inert atmosphere for activation, and then the activated ZIF-67 precursor is immersed in a furfuryl alcohol solution to adsorb furfuryl alcohol, thereby obtaining a precursor adsorbing furfuryl alcohol; In step S3, the precursor for adsorbing furfuryl alcohol is first heated to 80° C. in an inert gas atmosphere and maintained for 2 to 14 hours, then heated to 150° C. and maintained for 1 to 8 hours to polymerize furfuryl alcohol, and then heated to 800° C. under vacuum conditions and maintained for 1 to 5 hours for carbonization.
3. The method for preparing the heterogeneous formic acid dehydrogenation catalyst according to claim 2, Features: In the step S1, zinc salt and cobalt salt are dissolved in methanol to prepare the mixed solution, and the mass ratio of the zinc salt to the volume ratio of methanol is 1 g:30-50 mL; then a methanol solution of 2-methylimidazole is added to the mixed solution of the zinc salt and the cobalt salt, and the mass ratio of the 2-methylimidazole to the volume ratio of methanol is 1 g:10-15 mL, and the volume ratio of the mixed solution to the volume of the 2-methylimidazole methanol solution is 2:1; In the step S2, the ZIF-67 precursor is firstly heated to 300° C. in an inert atmosphere and maintained for 1 to 3 hours for activation, and then the activated ZIF-67 precursor is immersed in a furfuryl alcohol solution to adsorb furfuryl alcohol to obtain a precursor adsorbing furfuryl alcohol; In step S3, the precursor for adsorbing furfuryl alcohol is first heated to 80° C. in an inert gas atmosphere and maintained for 2 to 14 hours, then heated to 150° C. and maintained for 1 to 8 hours to polymerize furfuryl alcohol, and then heated to 800° C. under vacuum conditions and maintained for 1 to 5 hours for carbonization.
4. The method for preparing the heterogeneous formic acid dehydrogenation catalyst according to claim 1, 2 or 3, Features: The zinc salt is zinc nitrate, zinc carbonate or zinc acetate, and the cobalt salt is cobalt nitrate, cobalt carbonate or cobalt acetate.
5. The method for preparing the heterogeneous formic acid dehydrogenation catalyst according to claim 3, Features: In the step S2, the activated ZIF-67 precursor is immersed in a furfuryl alcohol solution and subjected to room temperature ultrasound to adsorb the furfuryl alcohol.
6. A method for preparing a heterogeneous formic acid dehydrogenation catalyst as claimed in claim 1, 2 or 3, Features: In the step S1, the molar ratio of zinc to cobalt is 10:1; in the step S2, the mass fraction of furfuryl alcohol in the furfuryl alcohol solution is 60%.
7. A heterogeneous formic acid dehydrogenation catalyst, Features The preparation method is described in any one of claims 1 to 6.
Citation Information
Patent Citations
Porous carbon loaded nano metal oxide catalyst, preparation method of catalyst, and hydrogen storage material
CN104069842A
Preparation method of porous nitrogen-doped carbon material supported cobalt-based catalyst and application of porous nitrogen-doped carbon material supported cobalt-based catalyst in reaction for preparing high-carbon alcohol through CO hydrogenation
CN114522708A
Heterogeneous nano-catalyst as well as preparation method and application thereof
CN115970767A
Dehydrogenation catalysts
GB2044121A
Process for synthesizing iron carbide fischer-tropsch catalysts
US20170173565A1
Cited By
Preparation method of heterogeneous formic acid dehydrogenation catalyst with low cobalt content and catalyst