Preparation method of CO catalyst for sintering machine
Through the preparation method of CO catalyst for sintering machine, coated catalysts are prepared using cordierite honeycomb ceramics and other materials, which solves the problems of insufficient activity and high cost of existing CO catalysts, achieves performance optimization and cost savings, and significantly improves material utilization rate and catalytic performance.
Patent Information
- Application Number
- CN202411085524.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
The existing CO catalysts are insufficient in actual applications and are costly, making it difficult to effectively treat the harmful gas carbon monoxide emitted by steel mills.
The CO oxidation catalyst preparation method is adopted for sintering machines, and the coating CO oxidation catalyst is made by carrier pretreatment and slurry preparation, and the coating CO oxidation catalyst is made using materials such as cordierite honeycomb ceramics, TiO2 powder, zeolite molecular sieve powder, etc. The effective calculation of unit area is calculated by combining the material weighing method. Coating amount, optimize catalyst performance.
Significantly save production costs, improve material utilization, and optimize CO catalyst performance, which can produce more catalyst support, reduce raw material waste, and achieve the expected catalytic performance.
Smart Images

Figure CN118988382A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst preparation, and in particular relates to a method for preparing a CO catalyst for a sintering machine. Background Art
[0002] In current steel production, carbon monoxide (CO) is a common harmful gas, and its effective treatment is the key to achieving clean production and meeting environmental protection standards. Although traditional CO treatment methods, such as thermal combustion and adsorption, can remove CO to a certain extent, these methods have some limitations that are difficult to overcome. Most of the existing CO treatments use catalysts. Although catalytic oxidation is a relatively economical and efficient CO treatment method, the existing CO catalysts still have the problems of insufficient activity and high cost in practical applications. Summary of the invention
[0003] (I) Purpose of the invention
[0004] In order to overcome the above shortcomings, the purpose of the present invention is to provide a method for preparing a CO catalyst for a sintering machine to solve the above technical problems.
[0005] (II) Technical solution
[0006] To achieve the above objectives, the technical solutions provided by this application are as follows:
[0007] A method for preparing a CO catalyst for a sintering machine comprises the following steps:
[0008] S1, carrier pretreatment, the carrier is cordierite honeycomb ceramic, the cordierite honeycomb ceramic is placed in a 20% concentration oxalic acid solution, boiled for 2 hours to remove surface impurities, washed with deionized water several times, dried, and calcined at 300°C for 3 hours to remove attached oxalic acid;
[0009] S2, slurry preparation, TiO 2 Powder or TiO 2 The powder is added with one or more of zeolite molecular sieve powder, ammonium metatungstate, ammonium metavanadate oxalic acid solution, ammonium heptamolybdate, cerium nitrate, palladium salt solution or platinum salt solution or platinum palladium salt mixed solution, binder, polyvinyl alcohol, ammonia water, and pure water to make a slurry with a solid-liquid ratio of 30%;
[0010] S3, catalyst preparation, soak the pretreated cordierite honeycomb ceramic in the slurry for 30-60 minutes, take it out and blow the surface with compressed air, calculate the coating amount by weighing the material, if the set coating amount is not reached, repeat the soaking and blowing, and the number of repeated soaking shall not exceed 3 times. After the coating amount reaches the set value, put it into the drying room for drying, and after drying, put it into the kiln for calcination at 500°C, and the calcination time is controlled at 20-30h to obtain a coated CO oxidation catalyst.
[0011] Preferably, the zeolite molecular sieve powder in S2 is mixed with TiO 2 The mass ratio is 2-10:100; WO 3 With TiO 2 The mass ratio of V is 2-8:100; 2 O 5 With TiO 2 The mass ratio of MoO is 0.5-3:100; 3 With TiO 2 The mass ratio is 2-8:100; CeO 2 With TiO 2 The mass ratio of the binder to TiO is 1-5:100; the concentration of the palladium salt solution or the platinum salt solution or the platinum-palladium salt mixed solution is 0.05-1%; 2 The mass ratio is 0.3-5:100; the concentration of polyvinyl alcohol is 0.5-2%.
[0012] Preferably, the pH of the slurry in S2 is controlled at 7.0-8.0.
[0013] Preferably, the drying temperature in S3 is controlled at 55-120° C., and the drying period is 2-3 days.
[0014] Preferably, a mixing unit is used to mix the raw materials in the slurry preparation in S2, and the mixing unit includes a mixing cylinder, a feed port is provided on the side of the mixing cylinder, a mixing shaft is rotatably provided on the central axis of the mixing cylinder, a plurality of stirring components are evenly arranged on the mixing shaft, the upper end of the mixing shaft passes through the mixing cylinder and is connected to a driving motor, and a discharge port is provided at the bottom of the mixing cylinder.
[0015] Preferably, each stirring assembly comprises a plurality of stirring rods radially arranged on the mixing shaft, and the stirring rods on each stirring assembly are on the same horizontal plane.
[0016] Preferably, the method of calculating the effective coating amount per unit area by material weighing comprises the following steps:
[0017] Step 1: Define additional variables:
[0018] W 载体 : The weight of the carrier itself;
[0019] W 干涂覆 : Weight of the coating material after drying on the carrier;
[0020] W 湿涂覆 : The weight of the undried coating material on the carrier;
[0021] Step 2, calculate the wet coating amount:
[0022] First calculate the incremental weight under the wet coated pile: ΔW 湿 =W 湿涂覆 -W 载体 ;
[0023] Step 3: Calculate the coating volume:
[0024] Calculate the volume V of the coating using the density formula: Where ρ is the density of the coating material;
[0025] Step 4: Calculate the effective coating volume:
[0026] Effective coating volume V 有效 :V 有效 =V×(1-φ), φ is the porosity;
[0027] Step 5: Calculate the effective coating amount per unit area:
[0028] The effective coating volume is divided by the carrier surface area A to obtain the effective coating volume per unit area C 有效 :
[0029] Beneficial effects:
[0030] The present invention uses a coating method to prepare the catalyst, which can reduce the amount of raw materials used, and the performance is similar to that of a conventional catalyst preparation method. This preparation method can significantly save production costs while ensuring performance. At the same time, the present invention can accurately 2 The mass ratio of can realize the optimization of CO catalyst performance, and the effective coating amount per unit area is calculated by material weighing method, which helps to achieve the expected catalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is a flow chart of the present invention;
[0032] Figure 2 It is a schematic structural diagram of the mixing unit of the present invention. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solutions and advantages of the present invention more clear, the following is a detailed description of the present invention in conjunction with the specific implementation methods and with reference to the attached drawings. Figure 1-2 , the present invention is further described in detail. It should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In addition, in the following description, descriptions of well-known structures and technologies are omitted to avoid unnecessary confusion of the concept of the present invention.
[0034] The present invention provides a method for preparing a CO catalyst for a sintering machine, characterized in that it comprises the following steps:
[0035] S1, carrier pretreatment, the carrier is cordierite honeycomb ceramic, the cordierite honeycomb ceramic is placed in a 20% concentration oxalic acid solution, boiled for 2 hours to remove surface impurities, washed with deionized water several times, dried, and calcined at 300°C for 3 hours to remove attached oxalic acid;
[0036] S2, slurry preparation, TiO 2 Powder or TiO 2 The powder is added with one or more of zeolite molecular sieve powder, ammonium metatungstate, ammonium metavanadate oxalic acid solution, ammonium heptamolybdate, cerium nitrate, palladium salt solution or platinum salt solution or platinum palladium salt mixed solution, binder, polyvinyl alcohol, ammonia water, and pure water raw materials to make a slurry with a solid-liquid ratio of 30%, and the pH is controlled at 7.0-8.0.
[0037] In the preparation of slurry, a mixing unit is used to mix the raw materials. The mixing unit includes a mixing cylinder 100. A feed port 101 is provided on the side of the mixing cylinder 100. A mixing shaft 200 is rotatably provided on the central axis of the mixing cylinder 101. A plurality of stirring components are evenly provided on the mixing shaft 200. The upper end of the mixing shaft 200 passes through the mixing cylinder 100 and is connected to the driving motor 400. A discharge port is provided at the bottom of the mixing cylinder 100. Each stirring component includes a plurality of stirring rods 300 radially arranged on the mixing shaft 200. A vertical stirring head is provided at the end of the stirring rod 300. The stirring rods 300 on each stirring component are on the same horizontal plane. When the raw materials need to be mixed, the raw materials are added to the mixing unit according to the proportion. The driving motor drives the stirring rod and the stirring head to rotate by driving the mixing shaft, thereby achieving rapid mixing of the raw materials and improving work efficiency.
[0038] The zeolite molecular sieve powder and TiO 2 The mass ratio is 2-10:100; WO 3 With TiO 2 The mass ratio of V is 2-8:100; 2 O 5 With TiO 2 The mass ratio of MoO is 0.5-3:100; 3 With TiO 2 The mass ratio is 2-8:100; CeO 2 With TiO 2 The mass ratio of the binder to TiO is 1-5:100; the concentration of the palladium salt solution or the platinum salt solution or the platinum-palladium salt mixed solution is 0.05-1%; 2 The mass ratio is 0.3-5:100; the concentration of polyvinyl alcohol is 0.5-2%.
[0039] S3, catalyst preparation, soak the pretreated cordierite honeycomb ceramic in the slurry for 30-60 minutes, take it out and blow the surface with compressed air, calculate the coating amount by weighing the material, if the set coating amount is not reached, repeat the soaking and blowing, and the number of repeated soaking shall not exceed 3 times. After the coating amount reaches the set value, put it into the drying room for drying, the drying temperature is controlled at 55-120°C, the drying cycle is 2-3 days, and after drying, it is placed in a kiln for calcination at 500°C, and the calcination time is controlled at 20-30h to obtain a coated CO oxidation catalyst.
[0040] The material weighing method to calculate the effective coating amount per unit area includes the following steps:
[0041] Step 1: Define additional variables:
[0042] W 载体 : The weight of the carrier itself;
[0043] W 干涂覆 : Weight of the coating material after drying on the carrier;
[0044] W 湿涂覆 : The weight of the undried coating material on the carrier;
[0045] Step 2, calculate the wet coating amount:
[0046] First calculate the incremental weight under the wet coated pile: ΔW 湿 =W 湿涂覆 -W 载体 ;
[0047] Step 3: Calculate the coating volume:
[0048] Calculate the volume V of the coating using the density formula: Where ρ is the density of the coating material;
[0049] Step 4: Calculate the effective coating volume:
[0050] Effective coating volume V 有效 :V 有效 =V×(1-φ), φ is the porosity;
[0051] Step 5: Calculate the effective coating amount per unit area:
[0052] The effective coating volume is divided by the carrier surface area A to obtain the effective coating volume per unit area C 有效 :
[0053] Example 1
[0054] Example 1
[0055] S1, placing the cordierite honeycomb ceramic in a 20% concentration oxalic acid solution, boiling it for 2 hours to remove surface impurities, washing it with deionized water for several times, drying it, and calcining it at 300° C. for 3 hours to remove the attached oxalic acid.
[0056] S2, weigh TiO 2 Powder 10kg or TiO 2 The powder is added with one or more of zeolite molecular sieve powder, ammonium metatungstate, ammonium metavanadate oxalic acid solution, ammonium heptamolybdate, cerium nitrate, palladium salt solution or platinum salt solution or platinum palladium salt mixed solution, binder, polyvinyl alcohol, ammonia water, pure water and other raw materials to make a slurry with a solid-liquid ratio of 30%, and the pH is controlled at 7.0-8.0.
[0057] Among them, zeolite molecular sieve powder and TiO 2 The mass ratio is 2:100; WO 3 With TiO 2 The mass ratio of V is 2:100; 2 O 5 With TiO 2 The mass ratio of MoO is 0.5:100; 3 With TiO 2 The mass ratio is 2:100; CeO 2 With TiO 2 The mass ratio of the binder to TiO is 1:100; the concentration of the palladium salt solution or the platinum salt solution or the platinum-palladium salt mixed solution is 0.05%; 2 The mass ratio is 0.3:100; the concentration of polyvinyl alcohol is 0.5%.
[0058] S3, soak the pretreated cordierite honeycomb ceramic in the slurry for 30-60 minutes, take it out and blow the surface with compressed air, calculate the coating amount by weighing the material, if the set coating amount is not reached, repeat the soaking and blowing, and the number of repeated soaking shall not exceed 3 times. After the coating amount reaches the set value, put it into the drying room for drying, the drying temperature is controlled at 55-120°C, the drying cycle is 2-3 days, and after drying, it is placed in a kiln for calcination at 500°C, and the calcination time is controlled at 20-30h to obtain a coated CO oxidation catalyst.
[0059] The equipment used for the test is a catalyst performance evaluation reaction device.
[0060] Table 1 Design flue gas conditions
[0061] name unit Design parameters Volumetric space velocity <![CDATA[h -1 ]]> 20000 <![CDATA[O 2 Concentration]]> % 4 CO concentration <![CDATA[mg / Nm 3 ]]> 2000 <![CDATA[H 2 O content]]> % 10 <![CDATA[SO 2 Concentration]]> <![CDATA[mg / Nm 3 ]]> 30 <![CDATA[NH 3 Concentration]]> <![CDATA[mg / Nm 3 ]]> 10 NOx concentration <![CDATA[mg / Nm 3 ]]> 60 Run time h 3
[0062] Table 2CO oxidation efficiency
[0063]
[0064] Example 2
[0065] S1, placing the cordierite honeycomb ceramic in a 20% concentration oxalic acid solution, boiling it for 2 hours to remove surface impurities, washing it with deionized water for several times, drying it, and calcining it at 300° C. for 3 hours to remove the attached oxalic acid.
[0066] S2, weigh TiO 2 Powder 10kg or TiO 2 The powder is added with one or more of zeolite molecular sieve powder, ammonium metatungstate, ammonium metavanadate oxalic acid solution, ammonium heptamolybdate, cerium nitrate, palladium salt solution or platinum salt solution or platinum palladium salt mixed solution, binder, polyvinyl alcohol, ammonia water, pure water and other raw materials to make a slurry with a solid-liquid ratio of 30%, and the pH is controlled at 7.0-8.0.
[0067] Among them, zeolite molecular sieve powder and TiO 2 The mass ratio is 6:100; WO 3 With TiO 2 The mass ratio of V is 5:100; 2 O 5 With TiO 2 The mass ratio of MoO is 1.5:100; 3 With TiO 2 The mass ratio is 5:100; CeO 2 With TiO 2 The mass ratio of the palladium salt solution or the platinum salt solution or the platinum-palladium salt mixed solution is 3:100; the concentration of the binder and the TiO 2 The mass ratio is 2.5:100; the concentration of polyvinyl alcohol is 1.2%.
[0068] S3, soak the pretreated cordierite honeycomb ceramic in the slurry for 30-60 minutes, take it out and blow the surface with compressed air, calculate the coating amount by weighing the material, if the set coating amount is not reached, repeat the soaking and blowing, and the number of repeated soaking shall not exceed 3 times. After the coating amount reaches the set value, put it into the drying room for drying, the drying temperature is controlled at 55-120°C, the drying cycle is 2-3 days, and after drying, it is placed in a kiln for calcination at 500°C, and the calcination time is controlled at 20-30h to obtain a coated CO oxidation catalyst.
[0069] The equipment used for the test is a catalyst performance evaluation reaction device.
[0070] Table 3 Design flue gas conditions
[0071] name unit Design parameters Volumetric space velocity <![CDATA[h -1 ]]> 20000 <![CDATA[O 2 Concentration]]> % 4 CO concentration <![CDATA[mg / Nm 3 ]]> 2000 <![CDATA[H 2 O content]]> % 10 <![CDATA[SO 2 Concentration]]> <![CDATA[mg / Nm 3 ]]> 30 <![CDATA[NH 3 Concentration]]> <![CDATA[mg / Nm 3 ]]> 10 NOx concentration <![CDATA[mg / Nm 3 ]]> 60 Run time h 3
[0072] Table 4CO oxidation efficiency
[0073]
[0074] Example 3
[0075] S1, placing the cordierite honeycomb ceramic in a 20% concentration oxalic acid solution, boiling it for 2 hours to remove surface impurities, washing it with deionized water for several times, drying it, and calcining it at 300° C. for 3 hours to remove the attached oxalic acid.
[0076] S2, weigh TiO 2 Powder 10kg or TiO 2 The powder is added with one or more of zeolite molecular sieve powder, ammonium metatungstate, ammonium metavanadate oxalic acid solution, ammonium heptamolybdate, cerium nitrate, palladium salt solution or platinum salt solution or platinum palladium salt mixed solution, binder, polyvinyl alcohol, ammonia water, pure water and other raw materials to make a slurry with a solid-liquid ratio of 30%, and the pH is controlled at 7.0-8.0.
[0077] Among them, zeolite molecular sieve powder and TiO 2 The mass ratio is 10:100; WO 3 With TiO 2 The mass ratio of V is 8:100; 2 O 5 With TiO 2 The mass ratio of MoO is 3:100; 3 With TiO 2 The mass ratio is 8:100; CeO 2 With TiO 2 The mass ratio of the binder to TiO is 5:100; the concentration of the palladium salt solution or the platinum salt solution or the platinum-palladium salt mixed solution is 1%; 2 The mass ratio is 5:100; the concentration of polyvinyl alcohol is 2%.
[0078] S3, soak the pretreated cordierite honeycomb ceramic in the slurry for 30-60 minutes, take it out and blow the surface with compressed air, calculate the coating amount by weighing the material, if the set coating amount is not reached, repeat the soaking and blowing, and the number of repeated soaking shall not exceed 3 times. After the coating amount reaches the set value, put it into the drying room for drying, the drying temperature is controlled at 55-120°C, the drying cycle is 2-3 days, and after drying, it is placed in a kiln for calcination at 500°C, and the calcination time is controlled at 20-30h to obtain a coated CO oxidation catalyst.
[0079] The equipment used for the test is a catalyst performance evaluation reaction device.
[0080] Table 5 Design flue gas conditions
[0081]
[0082]
[0083] Table 6 CO oxidation efficiency
[0084]
[0085] The present invention uses a coating method to prepare the catalyst, which can reduce the amount of raw materials used, and the performance is similar to that of a conventional catalyst preparation method. This preparation method can significantly save production costs while ensuring performance. In traditional production, using the same amount of mud, about 90 to 110 catalyst carriers are produced. However, through the preparation method of the present invention, at least 150 to 170 catalyst carriers can be produced, which is almost twice the number of the traditional method. This significant increase is not only reflected in the quantity, but also means that we can use raw materials more effectively and reduce waste in the production process.
[0086] This method not only improves the utilization rate of materials, but also reduces waste in the production process. 2 The mass ratio of can realize the optimization of CO catalyst performance, and the effective coating amount per unit area is calculated by material weighing method, which helps to achieve the expected catalytic performance.
[0087] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a CO catalyst for a sintering machine, characterized in that: The following steps are involved: S1, carrier pretreatment, the carrier is cordierite honeycomb ceramic, the cordierite honeycomb ceramic is placed in a 20% concentration oxalic acid solution, boiled for 2 hours to remove surface impurities, washed with deionized water several times, dried, and calcined at 300°C for 3 hours to remove attached oxalic acid; S2, slurry preparation, TiO2 powder or TiO2 powder is added with one or more of zeolite molecular sieve powder, ammonium metatungstate, ammonium metavanadate oxalic acid solution, ammonium heptamolybdate, cerium nitrate, palladium salt solution or platinum salt solution or platinum palladium salt mixed solution, binder, polyvinyl alcohol, ammonia water, and pure water raw materials to prepare a slurry with a solid-liquid ratio of 30%; S3, catalyst preparation, soak the pretreated cordierite honeycomb ceramic in the slurry for 30-60 minutes, take it out and blow the surface with compressed air, calculate the coating amount by weighing the material, if the set coating amount is not reached, repeat the soaking and blowing, and the number of repeated soaking shall not exceed 3 times. After the coating amount reaches the set value, put it into the drying room for drying, and after drying, put it into the kiln for calcination at 500°C, and the calcination time is controlled at 20-30h to obtain a coated CO oxidation catalyst.
2. The method for preparing a CO catalyst for a sintering machine according to claim 1, characterized in that: The mass ratio of zeolite molecular sieve powder to TiO2 in S2 is 2-10:100; the mass ratio of WO3 to TiO2 is 2-8:100; the mass ratio of V2O5 to TiO2 is 0.5-3:100; the mass ratio of MoO3 to TiO2 is 2-8:100; the mass ratio of CeO2 to TiO2 is 1-5:100; the concentration of palladium salt solution or platinum salt solution or platinum-palladium salt mixed solution is 0.05-1%; the mass ratio of binder to TiO2 is 0.3-5:100; and the concentration of polyvinyl alcohol is 0.5-2%.
3. The method for preparing a CO catalyst for a sintering machine according to claim 1, characterized in that: The pH of the slurry in S2 was controlled at 7.0-8.
0.
4. The method for preparing a CO catalyst for a sintering machine according to claim 1, characterized in that: In S3, the drying temperature is controlled at 55-120°C, and the drying cycle is 2-3 days.
5. The method for preparing a CO catalyst for a sintering machine according to claim 1, characterized in that: In the slurry preparation in S2, a mixing unit is used to mix the raw materials, and the mixing unit includes a mixing cylinder, a feeding port is provided on the side of the mixing cylinder, a mixing shaft is rotatably provided on the central axis of the mixing cylinder, a plurality of stirring components are evenly provided on the mixing shaft, the upper end of the mixing shaft passes through the mixing cylinder and is connected to a driving motor, and a discharge port is provided at the bottom of the mixing cylinder.
6. The method for preparing a CO catalyst for a sintering machine according to claim 5, characterized in that: Each stirring assembly includes a plurality of stirring rods radially arranged on the mixing shaft, and the stirring rods on each stirring assembly are on the same horizontal plane.
7. The method for preparing a CO catalyst for a sintering machine according to claim 1, characterized in that: The material weighing method to calculate the effective coating amount per unit area includes the following steps: Step 1: Define additional variables: W 载体 : The weight of the carrier itself; W 干涂覆 : Weight of the coating material after drying on the carrier; W 湿涂覆 : The weight of the undried coating material on the carrier; Step 2, calculate the wet coating amount: First calculate the incremental weight under the wet coated pile: ΔW 湿 =W 湿涂覆 -W 载体 ; Step 3: Calculate the coating volume: Calculate the volume V of the coating using the density formula: Where ρ is the density of the coating material; Step 4: Calculate the effective coating volume: Effective coating volume V 有效 :V 有效 =V×(1-φ), φ is the porosity; Step 5: Calculate the effective coating amount per unit area: The effective coating volume is divided by the carrier surface area A to obtain the effective coating volume per unit area C 有效 :
Citation Information
Patent Citations
Noble metal composite vanadium-titanium catalyst for purifying coal-fired flue organic waste gas as well as preparation method and application of the noble metal composite vanadium-titanium catalyst
CN111420660A
Preparation method and application of monolithic CO selective oxidation catalyst
CN115608377A
CO catalytic oxidation catalyst as well as preparation method and application thereof
CN116037202A
Production process of online quantitative coating type high-performance polyolefin greenhouse film
CN116277910A
Preparation method of catalyst suitable for CO catalytic combustion treatment of steel sintering flue gas