Efficient and stable catalyst as well as preparation method and application thereof

By connecting proton-type heteropolyacids and active metal components with covalent bonds on the metal oxide support to form a porous structure, the problem that existing catalysts only survive under high temperature and high pressure is solved, and high efficiency under mild conditions is achieved Catalysis and stability.

CN118988400APending Publication Date: 2024-11-22ZHEJIANG UNIV +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411096313.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing metal oxide-supported heteropolyacid catalysts have high catalytic activity only at high temperature or high pressure, and the stability and loss of heteropolyacids on the support are difficult to solve, resulting in high costs and insufficient activity.

Method used

A metal oxide support with a three-dimensional porous structure is used to support proton-type heteropoly acids, and is connected to the support through covalent bonds, and combines active metal components to form heteropoly acids in a single molecule state and metal dispersion catalysts in a single atom state to enhance catalysis. Activity and stability.

Benefits of technology

A catalytic effect with high catalytic activity and stability under mild conditions is achieved, reducing costs and simplifying the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988400A_ABST
    Figure CN118988400A_ABST
Patent Text Reader

Abstract

The invention discloses an efficient and stable catalyst and a preparation method and application thereof.The catalyst comprises a metal oxide carrier of a three-dimensional porous structure and heteropoly acid dispersed in a single molecule state and connected to the metal oxide carrier, the heteropoly acid is proton-type heteropoly acid capable of providing hydrogen ions, and further, the heteropoly acid can be used as a proton-type heteropoly acid capable of providing hydrogen ions; the catalyst also includes an active metal component dispersed in a monatomic state and linked to one or both of the heteropolyacid and the metal oxide carrier; the problem that active sites of heteropoly acid and metal cannot be fully utilized in the prior art is solved, and the catalyst has excellent catalytic activity and good stability and is suitable for being used in alkylation, esterification, hydrogenation, amination and other reactions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and in particular to a highly efficient and stable catalyst and a preparation method and application thereof. Background Art

[0002] Heteropolyacids (POMs) are formed by heteroatoms (such as P, Si, Fe, Co, etc.) and polyatoms (such as Mo, W, V, Nb, Ta, etc.) bridged by oxygen atoms. Heteropolyacids are not only acidic but also redox-sensitive, and are a new type of multifunctional catalyst. However, since heteropolyacids are non-porous solid substances (with a specific surface area of ​​less than 10m 2 / g), when heteropolyacids are directly used as catalysts, due to their small specific surface area, the exposed acid active sites are limited, and non-polar reactants cannot enter their bulk phase, resulting in insufficient catalytic activity and difficulty in separating homogeneous reaction catalysts.

[0003] It is known that immobilizing heteropolyacids on a carrier helps to achieve homogeneous heterogeneity, making the catalyst easy to recover, reducing corrosion and increasing the specific surface area, thereby enhancing the mechanical strength of the catalyst. Alumina is one of the commonly used catalyst carriers, and heteropolyacids have been reported in many papers. However, the catalytic activity of heteropolyacids supported on metal oxides reported is still unsatisfactory. For example, it still needs to be carried out at a higher temperature or under pressure. In addition, it is still a challenge to stabilize the heteropolyacid on alumina and minimize its loss.

[0004] Chinese patent document CN117138812A discloses a composite nano catalyst and a preparation method thereof, which can catalyze the hydrolysis of aluminum precursors and promote the generation of five-coordinated aluminum sites by in-situ introduction of polyoxometalates during the synthesis of porous nano alumina carriers, so that polyoxometalates can be in-situ anchored in the process of generating five-coordinated aluminum sites, thereby enabling polyoxometalates to stably exist on porous nano alumina carriers. However, the reaction catalyzed by the composite nano catalyst, such as the selective oxidation reaction of 2-methylbutyraldehyde, still needs to be carried out at 80°C and under pressure. In addition, it can be seen from the multiple schemes disclosed in the document that when the polyoxometalates used are in the form of salts such as ammonium phosphomolybdate and sodium phosphotungstate, the prepared catalyst has higher activity and selectivity than the acid form such as phosphomolybdic acid and phosphotungstic acid. Since the polyoxometalates in the form of salts usually have higher costs than the acid form, this also means that the pursuit of higher activity and selectivity will have to pay higher costs accordingly. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome one or more deficiencies in the prior art and provide a new catalyst with excellent performance.

[0006] The invention also provides a method for preparing the catalyst.

[0007] The present invention also provides the use of the novel catalyst in an acid catalytic system or a selective catalytic reaction, especially in esterification, oxidation, dehydrogenation and hydrogenation reactions, which has a significantly better catalytic effect.

[0008] Based on this, a technical solution adopted by the present invention is: a catalyst, which includes a metal oxide carrier with a three-dimensional porous structure and a heteropolyacid dispersed in a single molecule state and connected to the metal oxide carrier, and the heteropolyacid is a proton-type heteropolyacid that can provide hydrogen ions.

[0009] Another technical solution provided by the present invention is: a catalyst, which includes a metal oxide carrier with a three-dimensional porous structure, a heteropolyacid dispersed in a single molecule state and connected to the metal oxide carrier, and an active metal component dispersed in a single atom state and connected to one or both of the heteropolyacid and the metal oxide carrier, wherein the heteropolyacid is a proton-type heteropolyacid capable of providing hydrogen ions.

[0010] In some embodiments of the present invention, in the proton-type heteropolyacid, the heteroatoms and polyatoms are coordinated and bridged by oxygen atoms, the heteroatoms include at least one selected from P, Si, Fe, and Co, and the polyatoms include at least one selected from Mo, W, V, Nb, and Ta.

[0011] Furthermore, the proton-type heteropolyacid is connected to the metal oxide support at least through a covalent bond.

[0012] Furthermore, the covalent bond is formed between the polyatoms in the proton-type heteropolyacid, the terminal oxygen in the proton-type heteropolyacid and the metal atom in the metal oxide support.

[0013] According to some preferred aspects of the present invention, the active metal component is connected to the proton-type heteropolyacid via a chemical bond, wherein the chemical bond comprises a coordination bond, and the active metal component is also selectively adsorbed on the metal oxide support.

[0014] In some embodiments of the present invention, the metal oxide support is a hollow structure.

[0015] In some embodiments of the present invention, the hollow structure has a single hollow chamber or a cavity combination formed by a plurality of hollow chambers gathered in a connected state or a partially connected state.

[0016] In some embodiments of the present invention, the average diameter of the hollow chamber or cavity combination is 1-90 nm.

[0017] In some embodiments of the present invention, the ratio of the average diameter of the hollow chamber or cavity combination to the average particle size of the catalyst is 0.3-0.9:1.

[0018] In some embodiments of the present invention, the catalyst comprises a hollow spherical porous alumina carrier formed by self-assembly of two-dimensional nanosheets, and the proton-type heteropolyacid is dispersed in the skeleton, inside the pores and on the surface of the porous alumina carrier in a single molecule state.

[0019] According to the present invention, the proton-type heteropoly acid in a single-molecule state is distributed in the skeleton, inside the pores and on the surface of the metal oxide carrier.

[0020] In some embodiments of the present invention, the active metal component is a combination of one or more selected from transition metals.

[0021] Furthermore, the active metal component is a combination of one or more selected from Group IB-IIB and Group VB-VIIIB.

[0022] Furthermore, the active metal component is a combination of one or more selected from Pd, Pt, Ru, Au, Ag, Rh, Ni, Cu, Fe and Co.

[0023] In some embodiments of the present invention, the mass content of the active metal component in the catalyst is 0.01%-15% by mass percentage.

[0024] Furthermore, in the catalyst, the mass content of the active metal component is 0.04%-15% in terms of mass percentage.

[0025] In some embodiments of the present invention, the proton-type heteropolyacid includes a combination of one or more selected from phosphomolybdic acid, phosphotungstic acid, silicotungstic acid, silicomolybdic acid, phosphovanadium heteropolyacid, phosphoniobial heteropolyacid, phosphotantalum heteropolyacid, ferromolybdic heteropolyacid, ferrotungsten heteropolyacid, ferrovanadium heteropolyacid, cobaltmolybdic heteropolyacid, cobalttungsten heteropolyacid, and cobaltvanadium heteropolyacid.

[0026] In some embodiments of the present invention, the mass content of the proton-type heteropoly acid in the catalyst is 1%-68% by mass percentage.

[0027] Furthermore, in the catalyst, the mass content of the proton-type heteropoly acid is 7%-45% in terms of mass percentage.

[0028] Furthermore, in the catalyst, the mass content of the proton-type heteropoly acid is 7%-25% by mass percentage.

[0029] In some embodiments of the present invention, the catalyst has an average pore size of 2-30 nm, an average pore volume of 0.4-1.5 cc / g, and an average density of 0.5-4.0 g / cm 3 .

[0030] In some embodiments of the present invention, the average particle size of the catalyst is 10-350 nm. Further, the average particle size of the catalyst is 80-250 nm.

[0031] In some embodiments of the present invention, the specific surface area of ​​the catalyst is greater than or equal to 200 m 2 / g.

[0032] Furthermore, the specific surface area of ​​the catalyst is less than or equal to 1000 m 2 / g,

[0033] Furthermore, the specific surface area of ​​the catalyst is 200-800m 2 / g.

[0034] In some embodiments, the catalyst is a spherical structure. The "spherical structure" refers to a standard spherical structure or a structure close to a spherical structure, that is, including a substantially spherical structure.

[0035] In some embodiments of the present invention, the metal oxide support includes a zinc oxide support, a magnesium oxide support, a copper oxide support, an aluminum oxide support or a titanium oxide support.

[0036] In some embodiments of the present invention, for a catalyst without an active metal component, the catalyst is prepared by a preparation method that satisfies the following conditions:

[0037] (a) using a metal oxide precursor as a raw material, wherein the metal oxide precursor refers to a substance that can be converted into a metal oxide through one or more conversion treatments, wherein the conversion treatment at least includes a treatment for producing a chemical reaction;

[0038] (b) carrying out the one or more conversion treatments in the presence of the protic heteropolyacid and water.

[0039] In some embodiments of the present invention, for a catalyst containing an active metal component, the catalyst is prepared by a preparation method that meets the following conditions:

[0040] (a) using a metal oxide precursor and an active metal precursor as raw materials, respectively, wherein the metal oxide precursor and the active metal precursor refer to substances that can be converted into metal oxides or active metal components through one or more conversion treatments, and the conversion treatment at least includes a treatment that produces a chemical reaction;

[0041] (b) carrying out the one or more conversion treatments in the presence of the protic heteropolyacid and water.

[0042] In the present invention, the presence of the proton-type heteropolyacid can participate in the transformation process of the metal oxide precursor. The two work together to promote the transformation and formation of the metal oxide carrier with a three-dimensional porous structure, and to facilitate the dispersion of the proton-type heteropolyacid in a single molecule state. At the same time, it can also promote a more stable connection between the proton-type heteropolyacid and the metal oxide carrier, for example, it is conducive to the formation of covalent bonds between the polyatoms in the proton-type heteropolyacid, the terminal oxygen in the proton-type heteropolyacid and the metal atoms in the metal oxide carrier, and there may also be hydrogen bonding forces.

[0043] In some embodiments of the present invention, the precursor of the metal oxide is a compound containing a metal and an organic group selected from acidic, basic or neutral compounds.

[0044] In some embodiments of the present invention, the compound containing a metal and an organic group is selected from C1-C12 metal alkoxides, C1-C12 hydrocarbon metals, metal organic complexes or complexes.

[0045] In some embodiments of the present invention, the precursor of the metal oxide is a combination of one or more selected from aluminum alcohol compounds, magnesium alcohol compounds, copper alcohol compounds, zinc alcohol compounds, titanium alcohol compounds, hydrocarbyl aluminum compounds, hydrocarbyl titanium compounds, hydrocarbyl zinc compounds, organic aluminates, organic titanates and organic zincates.

[0046] In some embodiments of the present invention, the active metal precursor is a salt of an active metal component and / or an acid of an active metal component, the salt of the active metal component includes a combination of one or more selected from metal nitrates, metal sulfates, metal halides, metal acetylacetonate complexes, and metal sulfides, and the acid of the active metal component includes a halogenated metal acid.

[0047] In some embodiments of the present invention, the precursor of the metal oxide is a combination of one or more selected from trimethylaluminum, triethylaluminum, triisobutylaluminum, diethylaluminum chloride, aluminum isopropoxide, aluminum n-butoxide, aluminum acetate, aluminum propionate, titanium acetylacetonate, tetraethyl titanate, tetraisopropyl titanate, tetrabutyl titanate and zinc acetylacetonate.

[0048] In some embodiments of the present invention, the active metal precursor is a combination of one or more selected from palladium chloride, palladium nitrate, platinum acetylacetonate, gold chloride, silver nitrate, ruthenium chloride, ruthenium nitrate, rhodium chloride, rhodium nitrate, cobalt nitrate, nickel nitrate, ferric chloride, ferric sulfate, copper nitrate, copper sulfate, chloroplatinic acid, chloropalladic acid, chloroauric acid, and rhodium acetylacetonate.

[0049] In some embodiments of the present invention, the metal oxide precursor is a substance that can be converted into the metal oxide support having a three-dimensional porous structure by sequentially performing gelation treatment and calcination treatment.

[0050] In some embodiments of the present invention, the method for preparing the catalyst further satisfies the following conditions:

[0051] (c) The conversion treatment includes a gelation treatment, and the gelation treatment is performed in the simultaneous presence of water, an organic solvent, and a surfactant.

[0052] For a catalyst that does not contain active metal components, the present invention provides another technical solution: a method for preparing the above-mentioned catalyst, the preparation method comprising:

[0053] Gelation treatment: mixing and reacting the proton type heteropoly acid and the precursor of the metal oxide in the presence of water, an organic solvent and a surfactant, and inducing the solvent evaporation to form a gel, wherein: the temperature of the mixing reaction is controlled to be 20-50° C., and the reaction time is controlled to be not less than 12 hours;

[0054] Calcination treatment: the gel is dried and then calcined to obtain the catalyst.

[0055] For the catalyst containing active metal components, the present invention provides another technical solution: a method for preparing the above-mentioned catalyst, the preparation method comprising:

[0056] Gelation treatment: mixing and reacting the proton type heteropoly acid and the precursor of the metal oxide in the presence of water, an organic solvent and a surfactant, and inducing the solvent evaporation to form a gel, wherein: the temperature of the mixing reaction is controlled to be 20-50° C., and the reaction time is controlled to be not less than 12 hours;

[0057] Calcination treatment: drying the gel, calcining it, and performing a reduction treatment in the presence of a reducing agent to obtain the catalyst;

[0058] The preparation method further includes the step of adding an active metal precursor before the mixing reaction, or the step of coating with a solution containing the active metal precursor after the calcination and before the reduction treatment, wherein the coating includes spraying, brushing, rolling, dipping or scraping.

[0059] According to some preferred aspects of the present invention, the feed mass ratio of the water to the metal oxide precursor is 0.001 to 15:1.

[0060] Furthermore, the feed mass ratio of the water to the metal oxide precursor is 0.01 to 10:1.

[0061] Furthermore, the feed mass ratio of the water to the metal oxide precursor is 0.1 to 5:1.

[0062] In some embodiments of the present invention, the feed mass ratio of the water to the metal oxide precursor is 0.01 to 6:1, for example, 0.01 to 3:1, or 0.02 to 3:1, or 0.04 to 1:1.

[0063] According to some preferred aspects of the present invention, the volume ratio of water to the organic solvent is 0.001-5: 1. Further, the volume ratio of water to the organic solvent is 0.01-2: 1. Further, the volume ratio of water to the organic solvent is 0.005-1: 1.

[0064] In some embodiments of the present invention, the volume ratio of the water to the organic solvent is 0.001-1:1, for example, 0.001-0.5:1, or 0.001-0.2:1. In some embodiments of the present invention, the surfactant is a block copolymer nonionic surfactant and / or an ionic surfactant, the block copolymer nonionic surfactant includes a combination of one or more selected from nonionic surfactant P123, nonionic surfactant F127, and nonionic surfactant F108, and the ionic surfactant includes a combination of one or more selected from hexadecyltrimethylammonium bromide, sodium oleate, sodium dodecylbenzene sulfonate, and sodium stearate.

[0065] In some embodiments of the present invention, the feed mass ratio of the surfactant to the proton type heteropolyacid is 3 to 30:1.

[0066] In some embodiments of the present invention, the organic solvent is a polar organic solvent, and the feed mass ratio of the protic heteropoly acid to the organic solvent is 1:80-1000.

[0067] In some embodiments of the present invention, the organic solvent is a combination of one or more selected from methanol, ethanol, isopropanol, acetone, tetrahydrofuran, and N,N-dimethylformamide.

[0068] In some embodiments of the present invention, the time for controlling the mixing reaction is 12-15h, 15-18h, 18-21h, 21-24h, 24-27h, 27-30h or 30-48h.

[0069] In some embodiments of the present invention, the solvent evaporation induction is controlled to be carried out at a temperature of 40 to 120° C. for a time of 1 to 72 hours.

[0070] Furthermore, the solvent evaporation induction is controlled to be carried out at a temperature of 60-75° C. for a time of 10 to 60 hours.

[0071] In some embodiments of the present invention, the calcination is performed at 200-700°C.

[0072] In some embodiments of the present invention, the calcination is carried out in a muffle furnace, and the calcination time is controlled to be 1-6 hours and the heating rate is controlled to be 1-30° C. / min.

[0073] In some embodiments of the present invention, the calcination is performed in an aerobic environment, which includes an air atmosphere or a pure oxygen atmosphere. The pure oxygen atmosphere is formed by introducing pure oxygen gas with a purity greater than 99%.

[0074] In some preferred embodiments of the present invention, when the preparation method adopts impregnation or spraying with a solution containing the active metal precursor after the calcination and before the reduction treatment, the active metal precursor and the solid obtained by the calcination are respectively dispersed in a solvent, mixed and stirred, and separated to obtain a solid loaded with the active metal precursor, and then the reduction treatment is carried out.

[0075] Furthermore, the solvent may be a ketone solvent, such as acetone.

[0076] Furthermore, when the preparation method adopts the method of impregnating or spraying a solution containing the active metal precursor after the calcination and before the reduction treatment, the active metal precursor is dispersed in a ketone solvent and stirred sufficiently, and then the solid obtained by the calcination is ultrasonically dispersed in the aforementioned solution, continuously stirred, and heated until the ketone solvent is completely evaporated to obtain a solid loaded with the active metal precursor.

[0077] According to some specific aspects of the present invention, when the preparation method adopts adding an active metal precursor before the mixing reaction, the implementation of the gelation treatment includes:

[0078] The proton type heteropoly acid, water and organic solvent are mixed and dispersed uniformly to obtain solution A; then a surfactant, an aluminum oxide precursor and an active metal precursor are added to solution A for mixing and dispersion, reacted at room temperature, and induced by solvent evaporation to prepare a gel.

[0079] In some preferred embodiments of the present invention, the reduction treatment comprises: performing a first calcination in an oxygen environment and then performing a second calcination in a reducing atmosphere.

[0080] Furthermore, the calcination temperature of the first calcination is 200-400°C.

[0081] Furthermore, the second calcination temperature is set at 150-300°C.

[0082] In some preferred embodiments of the present invention, the calcination temperature of the second calcination is lower than the calcination temperature of the first calcination.

[0083] In some preferred embodiments of the present invention, during the reduction treatment, the aerobic environment includes an air atmosphere or a pure oxygen atmosphere, wherein the pure oxygen atmosphere is formed by introducing pure oxygen gas with a purity greater than 99%, and the reducing atmosphere includes a hydrogen atmosphere.

[0084] Another technical solution provided by the present invention is a catalyst composition, which comprises the catalyst described above and at least one other catalyst different from the catalyst, wherein the mass content of the catalyst exceeds 50%.

[0085] In some embodiments of the present invention, in the catalyst composition, the mass content of the above-mentioned catalyst exceeds 55%, or exceeds 60%, or exceeds 65%, or exceeds 70%, or exceeds 75%, or exceeds 80%, or exceeds 85%, or exceeds 90%, or exceeds 95%, or exceeds 96%, or exceeds 97%, or exceeds 98%, or exceeds 99%.

[0086] Another technical solution provided by the present invention is: use of the above-mentioned catalyst, or the catalyst prepared by the above-mentioned catalyst preparation method, or the above-mentioned catalyst composition in the following reactions: oxidation reaction of aromatic hydrocarbons, alcohols or aldehydes, esterification reaction of olefins and acids or esterification reaction of alcohols and acids, epoxidation reaction of olefins, alkylation reaction of aromatic compounds, isomerization reaction, dehydration reaction of alcohols, etherification reaction, hydration reaction of olefins, aldol condensation reaction, hydrogenation reaction, amination reaction of alcohols, ketones or olefins.

[0087] In some embodiments of the present invention, the oxidation reaction includes: using aromatic hydrocarbons, alcohols or aldehydes as starting materials, causing them to undergo an oxidation reaction in the presence of the catalyst or the catalyst composition and an oxidant to generate corresponding acids; wherein the oxidant is oxygen, and the oxidant is provided by introducing greater than 99% pure oxygen gas or air into the reaction system; in terms of mass percentage, the amount of the catalyst or the catalyst composition added is 0.01%-3% of the amount of the starting material added.

[0088] In some embodiments of the present invention, the oxidation reaction comprises: subjecting C3-C10 aldehyde, C3-C10 alcohol or C6-C12 aromatic hydrocarbon to oxidation reaction in the presence of an oxidant and the catalyst or the catalyst composition to prepare C3-C10 acid; further, the oxidant may be oxygen or air, etc., and the amount of the catalyst or the catalyst composition added is 0.01wt.%-2.0wt.% of the amount of the C3-C10 aldehyde added. Furthermore, when the C3-C10 aldehyde is used as a substrate, the reaction is carried out at 30-55°C; when the C3-C10 alcohol is used as a substrate, the reaction is carried out at 70-100°C; when the C6-C12 aromatic hydrocarbon is used as a substrate, the reaction is carried out at 120-160°C.

[0089] Furthermore, the oxidation reaction comprises: making phenyl C 1-6 Alkyl alcohol and hydrogen peroxide react in the presence of the catalyst or the catalyst composition to prepare phenyl C 1-6 Alkyl aldehyde; further, the reaction is carried out at 40-70°C; the amount of the catalyst or the catalyst composition added is phenyl C 1-6 The addition amount of alkyl alcohol is 0.01wt.%-3.0wt.%; phenyl C 1-6 The alkyl alcohol may be benzyl alcohol, phenylethyl alcohol or the like.

[0090] In some embodiments of the present invention, the epoxidation reaction of olefins comprises: 3-20 In the presence of an oxidant and the catalyst or the catalyst composition, an olefin undergoes an epoxidation reaction in a solvent to generate a corresponding epoxide; wherein the oxidant comprises hydrogen peroxide, and the amount of hydrogen peroxide added in the hydrogen peroxide is, in terms of mass percentage, 3-20 5%-50% of the amount of olefins added; in terms of mass percentage, the amount of the catalyst or the catalyst composition added is 3-20 The amount of olefin added is 0.1%-5%.

[0091] Furthermore, the olefin epoxidation reaction comprises: in the presence of the catalyst or the catalyst composition, reacting α-pinene with hydrogen peroxide to prepare epoxy pinane, and carrying out the reaction at 50-80°C; or, in the presence of the catalyst or the catalyst composition, reacting limonene with hydrogen peroxide to prepare epoxy limonene, and carrying out the reaction at 50-80°C.

[0092] In some embodiments of the present invention, the esterification reaction comprises: allowing an alcohol or an olefin to undergo an esterification reaction with an acid in the presence of the catalyst or the catalyst composition to generate an ester; wherein the alcohol comprises C 1-20 Hydrocarbyl alcohol, the acid comprising C 1-20 Hydrocarbyl carboxylic acid and / or C 1-20 Hydroxyloxy C 1-20 Hydrocarbyl carboxylic acid, the olefin comprises C 3-20 Cycloolefin; in terms of mass percentage, the added amount of the catalyst or the catalyst composition is 0.01%-3% of the added amount of the alcohol and the acid.

[0093] In some embodiments of the present invention, the esterification reaction includes: the esterification reaction of 2-methylbutyric acid with methanol, ethanol, isopropanol, n-butanol or n-hexanol respectively; or, the esterification reaction includes: the esterification reaction of salicylic acid with n-hexanol, n-pentanol, benzyl alcohol, leaf alcohol, cyclohexanol, isooctyl alcohol or isophorol respectively; or, the esterification reaction includes: the esterification reaction of allyl alcohol with acetic acid, hexanoic acid, heptanoic acid, phenylpropionic acid, phenoxyacetic acid or cyclohexyloxyacetic acid respectively; or, the esterification reaction includes: the esterification reaction of acetic acid with o-tert-butyl cyclohexanol, p-tert-butyl cyclohexanol, α-phenylethanol or β-phenylethanol respectively; or, the esterification reaction includes: the esterification reaction of dicyclopentadiene with acetic acid, propionic acid, n-butyric acid or isobutyric acid respectively; or, the esterification reaction includes: the esterification reaction of lauric acid with methanol.

[0094] Furthermore, in the esterification reaction, the acid may be 2-methylbutyric acid, and the alcohol may be methanol, ethanol, isopropanol, n-butanol, n-hexanol, n-pentanol, or n-hexanol. The reaction is carried out at 40-80° C., and the amount of the catalyst or the catalyst composition added is 0.01wt.%-2.0wt.% of the amount of the acid added.

[0095] Furthermore, in the esterification reaction, the acid can be salicylic acid, and the alcohol can be n-pentanol, n-hexanol, benzyl alcohol, leaf alcohol, cyclohexanol, isooctyl alcohol, or isophorol. The reaction is carried out at 60-100° C. and 300-700 mmHg, and the added amount of the catalyst or the catalyst composition is 0.01 wt.%-2.0 wt.% of the added amount of the acid.

[0096] Furthermore, in the esterification reaction, the acid can be acetic acid, hexanoic acid, heptanoic acid, phenylpropionic acid, phenoxyacetic acid, cyclohexyloxyacetic acid, and the alcohol can be allyl alcohol. The reaction is carried out at 60-100°C, and the added amount of the catalyst or the catalyst composition is 0.01wt.%-2.0wt.% of the added amount of the alcohol.

[0097] Furthermore, in the esterification reaction, the acid may be acetic acid, and the alcohol may be o-tert-butyl cyclohexanol, p-tert-butyl cyclohexanol, α-phenylethanol, or β-phenylethanol. The reaction is carried out at 60-100° C. and 300-700 mmHg, and the amount of the catalyst or the catalyst composition added is 0.01 wt.%-2.0 wt.% of the amount of the alcohol added.

[0098] Furthermore, in the esterification reaction, the olefin may be dicyclopentadiene, etc., and the acid may be acetic acid, propionic acid, n-butyric acid, isobutyric acid, etc. The reaction is carried out at 60-100° C., and the added amount of the catalyst or the catalyst composition is 0.01wt.%-2.0wt.% of the added amount of the olefin.

[0099] In some embodiments of the present invention, the alkylation reaction of the aromatic compound comprises reacting an olefin with a C 1-10 Alkyl-substituted phenol, or an alkylation reaction of an alcohol with a substituted or unsubstituted benzene in the presence of the catalyst or the catalyst composition; wherein the olefin is C 2-10 Olefins, the C 1-10 The alkyl-substituted phenol is a phenol substituted by one of methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl and neopentyl, and the substitution position is meta-position. The alcohol is C 1-6 Alkyl alcohol, the substituted or unsubstituted benzene is selected from benzene or C 1-6 Alkyl substituted benzene.

[0100] Furthermore, the alkylation reaction comprises: continuously alkylating propylene and m-cresol in the presence of the catalyst or the catalyst composition to prepare thymol; further, the reaction is carried out at 200-240° C. and 0.05-0.5 MPa.

[0101] In some embodiments of the present invention, the isomerization reaction includes: isomerizing o-cresol in the presence of the catalyst or the catalyst composition to prepare m-cresol and p-cresol; further, the reaction is carried out at 240-300°C and 0.05-0.4MPa; or, the isomerization reaction includes: hydroisomerizing 2-pentylidenecyclopentanone to prepare 2-pentylcyclopentenone; further, the reaction is carried out at 70-100°C and 100-500mmHg, and the added amount of the catalyst or the catalyst composition is 0.01wt.%-2.0wt.% of the added amount of the 2-(1-hydroxypentyl)-cyclopentanone.

[0102] In some embodiments of the present invention, the dehydration reaction of the alcohol comprises: under vacuum conditions, in the presence of the catalyst or the catalyst composition, dehydrating 2-(1-hydroxypentyl)-cyclopentanone to prepare 2-pentylidenecyclopentanone, or dehydrating hydroxycyclopentadecalactone to prepare habanolide; further, the reaction is carried out at 80-110°C and 150-500 mmHg, and the amount of the catalyst or the catalyst composition added is 0.01%-3% of the amount of the 2-(1-hydroxypentyl)-cyclopentanone or the hydroxycyclopentadecalactone added, in terms of mass percentage.

[0103] In some embodiments of the present invention, the hydration reaction of olefins comprises: in the presence of the catalyst or the catalyst composition, 2-20 The olefin reacts with water to produce the corresponding alcohol; wherein the C 2-20 The olefin is ethylene, propylene, butene, pentene, hexene, cyclopropene, cyclobutene, cyclopentene or cyclohexene.

[0104] Furthermore, the hydration reaction comprises: hydrating propylene to prepare isopropanol in the presence of the catalyst or the catalyst composition; further, the reaction is carried out at 100-160° C. and 1-8 MPa.

[0105] In some embodiments of the present invention, the hydrogenation reaction comprises: reacting a substituted or unsubstituted phenol with hydrogen in the presence of the catalyst or the catalyst composition to produce a corresponding substituted or unsubstituted cyclohexanol, or reacting cyclopentylbutyrolactone and alcohol with hydrogen to produce a corresponding substituted or unsubstituted cyclohexylpropionate, or hydrogenating rose ether to produce phenylpentyl alcohol, or hydrogenating harpa lactone to produce cyclopentadecanolide; wherein the substituted or unsubstituted phenol comprises C 1-6 Alkyl-substituted phenol, the alcohol being C 1-6 Alkyl alcohol.

[0106] Furthermore, the hydrogenation reaction comprises: in the presence of the catalyst or the catalyst composition, hydrogenating p-tert-butylphenol to prepare p-tert-butyl cyclohexanol; further, the reaction is carried out at a pressure of 1-5 MPa and a temperature of 60-90°C.

[0107] In some embodiments of the present invention, the hydrogenation reaction comprises: hydrogenating o-tert-butylphenol in the presence of the catalyst or the catalyst composition to produce o-tert-butyl cyclohexanol; further, the reaction is carried out at a pressure of 1-3 MPa and a reaction temperature of 60-90°C.

[0108] In some embodiments of the present invention, the hydrogenation reaction comprises: hydrogenating cyclopentylbutyrolactone in an alcohol-containing system in the presence of the catalyst or the catalyst composition to prepare cyclohexylpropionate. Further, the alcohol in the alcohol-containing system is selected from C 1-20 The hydrocarbon alcohol may be, for example, methanol, ethanol, n-propanol, isopropanol, n-butanol, allyl alcohol, etc. The reaction is carried out at 1-4 MPa and 100-150°C.

[0109] In some embodiments of the present invention, the hydrogenation reaction comprises: hydrogenating rose oxide in the presence of the catalyst or the catalyst composition to prepare phenylpentanol; further, the catalyst or the catalyst composition is added in an amount of 0.01wt.%-1.0wt.% of the amount of rose oxide added; and the reaction is carried out at 80-150°C and 1-3MPa.

[0110] In some embodiments of the present invention, the hydrogenation reaction comprises: in the presence of the catalyst or the catalyst composition, hydrogenating halbalactone to prepare cyclopentadecalactone; further, the reaction is carried out at 30-50°C, and the amount of the catalyst or the catalyst composition added is 0.01wt.%-1.0wt.% of the amount of halbalactone added.

[0111] In some embodiments of the present invention, the isomerization reaction comprises: subjecting 2-pentylcyclopentanone to hydroisomerization in the presence of the catalyst or the catalyst composition to prepare 2-pentylcyclopentenone; further, the reaction is carried out at 20-60°C, and the amount of the alumina-supported composite catalyst added is 0.01wt.%-1.0wt.% of the amount of 2-pentylcyclopentanone added.

[0112] In some embodiments of the present invention, the amination reaction comprises: in the presence of the catalyst or the catalyst composition, alcohol, ketone or olefin are mixed and reacted in the presence of ammonia to generate the corresponding amine; the alcohol is C 1-10 Hydrocarbyl alcohol, the ketone is C 3-10 Hydrocarbyl ketone, the olefin is C 2-20 Olefins.

[0113] Furthermore, the amination reaction comprises: making C 2-6 Hydroamination of alkyl alcohol with ammonia in the presence of the catalyst or the catalyst composition to prepare C 2-6 Alkylamine; further, the reaction is carried out at 100-150°C and a pressure of 0.1-0.6MPa; C 2-6 The alkyl alcohol may be ethanol, propanol, etc.

[0114] In some embodiments of the present invention, the amination reaction comprises: 3-6 Hydroamination of alkyl ketone with ammonia in the presence of the catalyst or the catalyst composition to prepare C 3-6 Alkylamine; further, the reaction is carried out at 100-150°C and a pressure of 0.1-0.6MPa; C 3-6 The alkyl ketone may be acetone, butanone or the like.

[0115] In some embodiments of the present invention, the amination reaction comprises: 2-10 Preparation of C by olefin and ammonia in the presence of the catalyst or the catalyst composition 2-10 Alkylamine; further, reacting at 120-180°C and 2-6MPa; C 2-10 The olefin may be isobutylene, ethylene, propylene, etc.

[0116] In some embodiments of the present invention, the etherification reaction comprises: in the presence of the catalyst or the catalyst composition, self-etherifying 2-(3-hydroxypropyl)cyclododecanone to prepare tridecanedione-oxabicyclo[10.4.0]hexadecene; further, the reaction is carried out at 80-100°C and 150-500 mmHg, and the amount of the catalyst or the catalyst composition added is 0.01wt.%-2.0wt.% of the amount of 2-(3-hydroxypropyl)cyclododecanone added.

[0117] In some embodiments of the present invention, the aldol condensation reaction comprises: in the presence of the catalyst or the catalyst composition, cyclopentanone and n-valeraldehyde undergo an aldol condensation reaction to generate 2-pentylidenecyclopentanone. Further, the aldol condensation reaction is carried out at 80-150° C. and 0.1-3 MPa, and further at 80-130° C. and 0.5-1.5 MPa.

[0118] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:

[0119] The present invention provides a novel catalyst structure, which is based on a metal oxide carrier with a three-dimensional porous structure and loaded with a proton type heteropoly acid that can provide hydrogen ions. In particular, the novel catalyst structure of the present invention is based on a metal oxide carrier with a three-dimensional porous structure. While realizing that the proton type heteropoly acid can be loaded and dispersed in a single molecule state, the two also have a stable connection relationship. Further, the present invention also provides a catalyst of proton type heteropoly acid single molecule state dispersion and active metal component single atom state dispersion composite on the basis of a metal oxide carrier with a three-dimensional porous structure. The interaction between their components and structures achieves a significant synergistic effect; the catalyst of the present invention has been proven to have higher catalytic activity and stability in multiple reaction systems. The preparation method of the present invention is simple to operate and has low raw material cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0120] Figure 1 XRD pattern of H3PMo / AS-20H prepared in Example 1;

[0121] Figure 2 TEM image of H3PMo / AS-20H prepared in Example 1;

[0122] Figure 3 This is the STEM-HAADF image of H3PMo / AS-20H prepared in Example 1;

[0123] Figure 4 The particle size distribution histogram corresponding to H3PMo / AS-20H prepared in Example 1;

[0124] Figure 5 Figure 1 is a nitrogen absorption and desorption diagram of H3PMo / AS-20H prepared in Example 1;

[0125] Figure 6 TEM image of H3PMo / TiO2-20H prepared in Example 12;

[0126] Figure 7 TEM image of H3PMo / ZnO-20H prepared in Example 13;

[0127] Figure 8 XRD pattern of Pd-H3PMo / AS-20H prepared in Example 14;

[0128] Fig. 9 This is the SEM image of Pd-H3PMo / AS-20H prepared in Example 14;

[0129] Fig.10 TEM image of Pd-H3PMo / AS-20H prepared in Example 14;

[0130] Fig.11 This is a STEM-HAADF image of Pd-H3PMo / AS-20H prepared in Example 14;

[0131] Fig.12 The particle size distribution histogram corresponding to Pd-H3PMo / AS-20H prepared in Example 14;

[0132] Fig.13 Figure 14 shows the nitrogen absorption and desorption of Pd-H3PMo / AS-20H prepared in Example 14;

[0133] Fig.14 XRD pattern of Pd-H3PW / AS-20H prepared in Example 15;

[0134] Fig.15 This is the SEM image of Pd-H3PW / AS-20H prepared in Example 15;

[0135] Fig.16 TEM image of Pd-H3PW / AS-20H prepared in Example 15;

[0136] Fig.17 This is the STEM-HAADF image of Pd-H3PW / AS-20H prepared in Example 15;

[0137] Fig.18 The particle size distribution histogram corresponding to Pd-H3PW / AS-20H prepared in Example 15;

[0138] Fig.19 Figure 15 shows the nitrogen absorption and desorption of Pd-H3PW / AS-20H prepared in Example 15;

[0139] Fig. 20 XRD pattern of Pd-H4SiW / AS-20H prepared in Example 16;

[0140] Fig.21 This is the SEM image of Pd-H4SiW / AS-20H prepared in Example 16;

[0141] Fig. 22 TEM image of Pd-H4SiW / AS-20H prepared in Example 16;

[0142] Fig.23 This is a nitrogen absorption and desorption diagram of Pd-H4SiW / AS-20H prepared in Example 16;

[0143] Fig.24 XRD pattern of Pd-H4SiMo / AS-20H prepared in Example 17;

[0144] Fig.25 This is a SEM image of Pd-H4SiMo / AS-20H prepared in Example 17;

[0145] Fig.26 TEM image of Pd-H4SiMo / AS-20H prepared in Example 17;

[0146] Fig. 27 This is a nitrogen absorption and desorption diagram of Pd-H4SiMo / AS-20H prepared in Example 17;

[0147] Fig.28 TEM image of Pd-H3PMo / AS-14H prepared in Example 18;

[0148] Fig.29 TEM image of Pd-H3PMo / AS-8H prepared in Example 19;

[0149] Fig.30 TEM image of Pd-H3PMo / AS-2H prepared in Example 20;

[0150] Fig.31 TEM image of Pd-H3PMo / AS-30H prepared in Example 21;

[0151] Fig.32 TEM image of Pd-H3PMo / AS-50H prepared in Example 22;

[0152] Fig.33 TEM image of Pd-H3PMo / AS-100H prepared in Example 23;

[0153] Fig.34 XRD pattern of Pt-H3PMo / AS-20H prepared in Example 24;

[0154] Fig.35 TEM image of Pt-H3PMo / AS-20H prepared in Example 24;

[0155] Fig.36 XRD pattern of Co-H3PMo / AS-20H prepared in Example 25;

[0156] Fig.37 XRD pattern of Ni-H3PMo / AS-20H prepared in Example 26;

[0157] Fig.38 XRD pattern of Pd@H3PMo / AS-20H prepared in Example 36;

[0158] Fig.39TEM image of Pd@H3PMo / AS-20H prepared in Example 36;

[0159] Fig.40 TEM image of Pd-H3PMo / AS-20H-85 prepared in Example 37;

[0160] Fig.41 TEM image of Pd-H3PMo / AS-F-20H prepared in Example 40;

[0161] Fig.42 TEM image of Pd-H3PMo / AS-C-20H prepared in Example 41;

[0162] Fig.43 XRD pattern of the catalyst H3PMo@AS prepared in Comparative Example 1;

[0163] Fig.44 XRD pattern of the catalyst Pd-APMo / AS-20H prepared in Comparative Example 2;

[0164] Fig.45 TEM image of the catalyst Pd-APMo / AS-20H prepared in Comparative Example 2;

[0165] Fig.46 TEM image of H3PMo / AS-ethanol of the catalyst prepared in Comparative Example 3. DETAILED DESCRIPTION

[0166] The present invention is directed to an in-depth study of catalysts loaded with heteropolyacids, and further studies the formation mechanism, and innovatively proposes a catalyst of a novel structure based on a metal oxide carrier loaded with proton-type heteropolyacids having a three-dimensional porous structure, the main features of which are: (1) a proton-type heteropolyacid capable of providing hydrogen ions is used as a loading component, (2) the proton-type heteropolyacid is dispersed in a single molecule state, and (3) the proton-type heteropolyacid can be connected to the metal oxide carrier with a three-dimensional porous structure, and a stable loading is achieved through a stable connection relationship; compared with the currently disclosed metal oxide carrier loaded with heteropolyacids, such as The composite nanocatalyst (polyoxometalate supported on the five-coordinated aluminum site of porous nanoalumina) disclosed in Chinese patent document CN117138812A has achieved better results in terms of catalyst preparation cost and catalyst activity; when the proton-type heteropoly acid single molecule state dispersion and the active metal component single atom state dispersion composite are further adopted, and the active metal component is connected to one or both of the heteropoly acid and the metal oxide carrier, a catalyst form of dual monodisperse and three-dimensional porous metal oxide is formed, so that the catalyst of the present invention can be suitable for more application scenarios.

[0167] Furthermore, in the catalyst structure of the present invention: the proton-type heteropolyacid is uniformly distributed in a single molecule state, so that the active sites of the proton-type heteropolyacid are fully exposed, and at the same time, the single molecule state in the catalyst of the double monodisperse and three-dimensional porous metal oxide promotes the active metal component to be dispersed in the form of a single atom and always maintain a uniform dispersion state, and the metal oxide carrier and the proton-type heteropolyacid and / or the proton-type heteropolyacid and the active metal component form a stable strong interaction and improve the microstructure, constructing a stable loading state, and can also form a catalyst with a three-dimensional porous structure. Practice shows that the catalyst of the present invention can obtain unexpectedly excellent stability, catalytic activity and selectivity in the catalytic process of acid-catalyzed reactions and selective catalytic reactions, such as oxidation reactions of aromatic hydrocarbons, alcohols or aldehydes, esterification reactions of olefins and acids or esterification reactions of alcohols and acids, epoxidation reactions of olefins, alkylation reactions of aromatic compounds, isomerization reactions, dehydration reactions of alcohols, etherification reactions, hydration reactions of olefins, etc., and has a long service life and good catalytic effect. It can also significantly improve the conditions of certain catalytic reactions, making the reactions milder. In addition, the catalyst cost is relatively low, and the preparation method is simple and controllable.

[0168] The above scheme is further described below in conjunction with specific embodiments; it should be understood that these embodiments are used to illustrate the basic principles, main features and advantages of the present invention, and the present invention is not limited to the scope of the following embodiments; the implementation conditions adopted in the embodiments can be further adjusted according to specific requirements, and the implementation conditions not specified are usually the conditions in conventional experiments.

[0169] The raw materials used in the following examples, unless otherwise specified, were purchased from commercial sources or prepared by conventional methods in the art, wherein the surfactant: P123 was purchased from Sigma-Aldrich.

[0170] Example 1

[0171] This example provides a method for preparing a catalyst and the catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and after it is evenly dispersed, sequentially adding 20 g of P123 and 50 g of aluminum isopropoxide, reacting them fully at room temperature for 24 hours, and then inducing solvent evaporation at 70°C, obtaining a gel after 48 hours, and then drying it in an oven overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350°C for 3 hours in an air atmosphere, and the heating rate is 5°C / min, to obtain the catalyst, which is recorded as H3PMo / AS-20H.

[0172] The structure of the obtained catalyst H3PMo / AS-20H was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was about 21.8%.

[0173] Figure 1 This is the XRD diagram of H3PMo / AS-20H. It is observed that there is no characteristic diffraction peak of heteropoly acid molecules on the XRD, indicating that the proton-type heteropoly acid - phosphomolybdic acid is uniformly dispersed on the porous alumina carrier.

[0174] Figure 2 This is the TEM image of H3PMo / AS-20H. It can be seen that the catalyst is a three-dimensional porous hollow structure assembled from two-dimensional sheets, with a diameter of about 180nm and a diameter of the hollow part of about 80nm.

[0175] Figure 3 This is the STEM-HAADF image of H3PMo / AS-20H. Figure 4 The particle size distribution histogram of the corresponding heteropoly acid shows that single clusters of phosphomolybdic acid with a size of about 0.71 nm are distributed on the catalyst, indicating that phosphomolybdic acid is dispersed in a single molecule on the catalyst H3PMo / AS-20H.

[0176] Figure 5 This is the nitrogen adsorption / desorption diagram of H3PMo / AS-20H. It is observed that the nitrogen adsorption / desorption diagram of the catalyst shows a typical type IV adsorption / desorption curve with a type I hysteresis loop, indicating that there are a large number of mesoporous structures in the catalyst.

[0177] The H3PMo / AS-20H catalyst is spherical with a diameter of about 180 nm and a specific surface area of ​​about 701 m 2 / g, the average pore size is about 6.5nm, the average pore volume is about 1.4cc / g, and the average density is about 3.0g / cm 3 .

[0178] Example 2

[0179] This example provides a method for preparing a catalyst and the catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphotungstic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and then adding 20 g of P123 and 50 g of aluminum isopropoxide in sequence after it is evenly dispersed at room temperature for 24 hours, and then inducing solvent evaporation at 70°C for 48 hours to obtain a gel, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, and calcined at 350°C for 3 hours in an air atmosphere, with a heating rate of 5°C / min, to obtain the catalyst, which is recorded as H3PW / AS-20H.

[0180] Example 3

[0181] This example provides a method for preparing a catalyst and the catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of silicotungstic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and after it is evenly dispersed, sequentially adding 20 g of P123 and 50 g of aluminum isopropoxide, reacting them fully at room temperature for 24 hours, and then inducing solvent evaporation at 70°C, obtaining a gel after 48 hours, and then drying it in an oven overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350°C for 3 hours in an air atmosphere, and the heating rate is 5°C / min, to obtain the catalyst, which is recorded as H4SiW / AS-20H.

[0182] Example 4

[0183] This example provides a method for preparing a catalyst and the catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of silicomolybdic acid, mixing with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring thoroughly, and after uniform dispersion, sequentially adding 20 g of P123 and 50 g of aluminum isopropoxide, reacting fully at room temperature for 24 h, and then inducing solvent evaporation at 70 ° C. After 48 h, a gel is obtained, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C. for 3 h in an air atmosphere, with a heating rate of 5 ° C. / min, to obtain the catalyst, which is recorded as H4SiMo / AS-20H.

[0184] Example 5

[0185] This example provides a method for preparing a catalyst and the catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 14 mL of deionized water, stirring it thoroughly, and after it is evenly dispersed, sequentially adding 20 g of P123 and 50 g of aluminum isopropoxide, reacting them fully at room temperature for 24 hours, and then inducing solvent evaporation at 70°C, obtaining a gel after 48 hours, and then drying it in an oven overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350°C for 3 hours in an air atmosphere, and the heating rate is 5°C / min, to obtain the catalyst, which is recorded as H3PMo / AS-14H.

[0186] Example 6

[0187] This example provides a method for preparing a catalyst and the catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 8 mL of deionized water, stirring it thoroughly, and then adding 20 g of P123 and 50 g of aluminum isopropoxide in sequence after it is evenly dispersed at room temperature for 24 hours, and then inducing solvent evaporation at 70°C, obtaining a gel after 48 hours, and then drying it in an oven overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350°C for 3 hours in an air atmosphere, and the heating rate is 5°C / min, to obtain the catalyst, which is recorded as H3PMo / AS-8H.

[0188] Example 7

[0189] This example provides a method for preparing a catalyst and the catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 2 mL of deionized water, stirring it thoroughly, and then adding 20 g of P123 and 50 g of aluminum isopropoxide in sequence after being uniformly dispersed at room temperature for 24 hours, and then inducing solvent evaporation at 70°C for 48 hours to obtain a gel, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, and calcined at 350°C for 3 hours in an air atmosphere, with a heating rate of 5°C / min, to obtain the catalyst, which is recorded as H3PMo / AS-2H.

[0190] Example 8

[0191] This example provides a method for preparing a catalyst and the catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 30 mL of deionized water, stirring it thoroughly, and then adding 20 g of P123 and 50 g of aluminum isopropoxide in sequence after it is evenly dispersed at room temperature for 24 hours, and then inducing solvent evaporation at 70°C for 48 hours to obtain a gel, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, and calcined at 350°C for 3 hours in an air atmosphere, with a heating rate of 5°C / min, to obtain the catalyst, which is recorded as H3PMo / AS-30H.

[0192] Example 9

[0193] This example provides a method for preparing a catalyst and the catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 50 mL of deionized water, stirring it thoroughly, and adding 20 g of P123 and 50 g of aluminum isopropoxide in sequence after it is evenly dispersed at room temperature for 24 hours, and then inducing solvent evaporation at 70°C for 48 hours to obtain a gel, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, and calcined at 350°C for 3 hours in an air atmosphere, with a heating rate of 5°C / min, to obtain the catalyst, which is recorded as H3PMo / AS-50H.

[0194] Example 10

[0195] This example provides a method for preparing a catalyst and the catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 100 mL of deionized water, stirring it thoroughly, and then adding 20 g of P123 and 50 g of aluminum isopropoxide in sequence after being uniformly dispersed at room temperature for 24 hours, and then inducing solvent evaporation at 70°C for 48 hours to obtain a gel, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350°C for 3 hours in an air atmosphere, and the heating rate is 5°C / min to obtain the catalyst, which is recorded as H3PMo / AS-100H.

[0196] Embodiment 11

[0197] This example provides a method for preparing a catalyst and the catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 0.8 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and then adding 20 g of P123 and 50 g of aluminum isopropoxide in sequence after being uniformly dispersed at room temperature for 24 hours, and then inducing solvent evaporation at 70°C for 48 hours to obtain a gel, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350°C for 3 hours in an air atmosphere, and the heating rate is 5°C / min to obtain the catalyst, which is recorded as 7% H3PMo / AS-20H.

[0198] Example 12

[0199] This example provides a method for preparing a catalyst and the catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and then adding 20 g of P123 and 50 g of tetrabutyl titanate in sequence after uniform dispersion, reacting them at room temperature for 24 h, and then inducing solvent evaporation at 70 ° C. After 48 h, a gel is obtained, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C. for 3 h in an air atmosphere, and the heating rate is 5 ° C. / min to obtain the catalyst, which is recorded as H3PMo / TiO2-20H.

[0200] Figure 6 This is the TEM image of H3PMo / TiO2-20H. It can be seen that the catalyst is a three-dimensional porous structure assembled from two-dimensional sheets.

[0201] The H3PMo / TiO2-20H catalyst is spherical with a diameter of about 50 nm and a specific surface area of ​​about 468 m 2 / g, the average pore diameter is about 8.9nm, the average pore volume is about 1.1cc / g, and the average density is about 4.0g / cm 3 .

[0202] Example 13

[0203] This example provides a method for preparing a catalyst and the catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and then adding 20 g of P123 and 50 g of zinc acetylacetonate in sequence after it is evenly dispersed, reacting it at room temperature for 24 hours, and then inducing solvent evaporation at 70°C, obtaining a gel after 48 hours, and then drying it in an oven overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350°C for 3 hours in an air atmosphere, and the heating rate is 5°C / min, to obtain the catalyst, which is recorded as H3PMo / ZnO-20H.

[0204] Figure 7 TEM image of H3PMo / ZnO-20H.

[0205] The H3PMo / ZnO-20H catalyst is spherical with a diameter of about 297 nm and a specific surface area of ​​about 510 m 2 / g, the average pore size is about 6.5nm, the average pore volume is about 1.2cc / g, and the average density is about 4.9g / cm 3 .

[0206] Embodiment 14

[0207] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and then adding 20 g of P123 and 50 g of aluminum isopropoxide in sequence after being uniformly dispersed at room temperature, reacting it for 24 h, and then inducing solvent evaporation at 70 ° C. After 48 h, a gel is obtained, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C. for 3 h in an air atmosphere, with a heating rate of 5 ° C. / min, to obtain a metal oxide-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C. until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Pd-H3PMo / AS-20H.

[0208] The structure of the obtained Pd-H3PMo / AS-20H was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 22%, and the actual loading amount of palladium was 0.6%.

[0209] Figure 8 This is the XRD diagram of Pd-H3PMo / AS-20H. It was observed that there were no characteristic diffraction peaks of heteropoly acid molecules or palladium, indicating that the heteropoly acid and palladium were uniformly dispersed on the porous alumina support.

[0210] Fig. 9 This is the SEM image of Pd-H3PMo / AS-20H. It was observed that the catalyst is a three-dimensional porous hollow structure assembled from two-dimensional sheets.

[0211] Fig.10 This is a TEM image of Pd-H3PMo / AS-20H. It is observed that the catalyst is a three-dimensional porous hollow structure assembled from two-dimensional sheets, with a diameter of about 181nm and a hollow part diameter of about 80nm. No palladium particles are observed, indicating that palladium is highly dispersed.

[0212] Fig.11 This is the STEM-HAADF image of Pd-H3PMo / AS-20H. Fig.12 The corresponding particle size distribution histogram shows that single clusters of phosphomolybdic acid with a size of about 0.71 nm are distributed on the catalyst, indicating that phosphomolybdic acid is dispersed in a single molecule on the catalyst Pd-H3PMo / AS-20H.

[0213] Fig.13 This is the nitrogen adsorption and desorption diagram of Pd-H3PMo / AS-20H. It is observed that the nitrogen adsorption and desorption diagram of the catalyst shows a typical type IV adsorption and desorption curve with a type I hysteresis loop, indicating that there are a large number of mesoporous structures in the catalyst.

[0214] The catalyst is spherical, with a diameter of about 181nm and a specific surface area of ​​about 697m 2 / g, average pore diameter is 6.6nm, average pore volume is 1.3cc / g, and average density is 2.6g / cm 3 .

[0215] Embodiment 15

[0216] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphotungstic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and after uniform dispersion, successively adding 20 g of P123 and 50 g of aluminum isopropoxide, fully reacting at room temperature for 24 h, then inducing solvent evaporation at 70 ° C, and obtaining a gel after 48 h, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C for 3 h in an air atmosphere, with a heating rate of 5 ° C / min, to obtain a metal oxide-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Pd-H3PW / AS-20H.

[0217] The structure of the catalyst was characterized, and the actual loading amount of phosphotungstic acid in the catalyst was 22%, and the actual loading amount of palladium in the catalyst was 0.6%;

[0218] Fig.14 The XRD pattern of Pd-H3PW / AS-20H shows that there is no characteristic diffraction peak of heteropoly acid molecules or palladium, indicating that heteropoly acid and palladium are uniformly dispersed on the catalyst.

[0219] Fig.15 This is the SEM image of Pd-H3PW / AS-20H. It is observed that the catalyst is a three-dimensional porous hollow structure assembled from two-dimensional sheets.

[0220] Fig.16This is the TEM image of Pd-H3PW / AS-20H. It is observed that the catalyst is a three-dimensional porous hollow structure assembled from two-dimensional sheets, and no palladium particles are observed, indicating that the palladium is highly dispersed;

[0221] Fig.17 This is the STEM-HAADF image of Pd-H3PW / AS-20H. Fig.18 The corresponding particle size distribution histogram shows that single clusters of phosphotungstic acid with a size of about 0.71 nm are distributed on the catalyst, indicating that phosphotungstic acid is dispersed in a single molecule on the catalyst Pd-H3PW / AS-20H;

[0222] Fig.19 The nitrogen adsorption and desorption diagram of Pd-H3PW / AS-20H shows a typical type IV adsorption and desorption curve with a type I hysteresis loop, indicating that there are a large number of mesoporous structures in the catalyst.

[0223] The catalyst is spherical, with a diameter of about 178nm and a specific surface area of ​​about 650m 2 / g, average pore diameter of 5.9nm, average pore volume of 1.1cc / g, average density of 2.8g / cm 3 .

[0224] Example 16

[0225] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of silicotungstic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and after uniform dispersion, successively adding 20 g of P123 and 50 g of aluminum isopropoxide, fully reacting at room temperature for 24 h, then inducing solvent evaporation at 70 ° C, and obtaining a gel after 48 h, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C for 3 h in an air atmosphere, with a heating rate of 5 ° C / min, to obtain a metal oxide-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Pd-H4SiW / AS-20H.

[0226] The structure of the catalyst was characterized, and the actual loading of silicotungstic acid and palladium in the catalyst was 23% and 0.6% respectively.

[0227] Fig. 20 The XRD pattern of Pd-H4SiW / AS-20H shows that there are no characteristic diffraction peaks of heteropoly acid molecules or palladium, indicating that heteropoly acid and palladium are uniformly dispersed on the catalyst.

[0228] Fig.21 This is the SEM image of Pd-H4SiW / AS-20H. It is observed that the catalyst is a three-dimensional porous hollow structure assembled from two-dimensional sheets.

[0229] Fig. 22 This is the TEM image of Pd-H4SiW / AS-20H. It is observed that the catalyst is a three-dimensional porous hollow structure assembled from two-dimensional sheets, and no palladium particles are observed, indicating that the palladium is highly dispersed;

[0230] Fig.23 The nitrogen adsorption and desorption diagram of Pd-H4SiW / AS-20H shows a typical type IV adsorption and desorption curve with a type I hysteresis loop, indicating that there are a large number of mesoporous structures in the catalyst.

[0231] The catalyst is spherical, with a diameter of about 175nm and a specific surface area of ​​about 647m 2 / g, average pore diameter of 5.8nm, average pore volume of 0.9cc / g, average density of 3.0g / cm 3 .

[0232] Embodiment 17

[0233] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of silicomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and after uniform dispersion, successively adding 20 g of P123 and 50 g of aluminum isopropoxide, reacting it thoroughly at room temperature for 24 h, and then inducing solvent evaporation at 70 ° C. After 48 h, a gel is obtained, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C. for 3 h in an air atmosphere, with a heating rate of 5 ° C. / min, to obtain a metal oxide-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C. until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Pd-H4SiMo / AS-20H.

[0234] The catalyst was characterized structurally. The actual loading amount of silicomolybdic acid in the catalyst was 22%, and the actual loading amount of palladium was 0.5%;

[0235] Fig.24 The XRD pattern of Pd-H4SiMo / AS-20H shows that there are no characteristic diffraction peaks of heteropoly acid molecules or palladium, indicating that heteropoly acid and palladium are uniformly dispersed on the catalyst.

[0236] Fig.25 This is the SEM image of Pd-H4SiMo / AS-20H. It is observed that the catalyst is a three-dimensional porous hollow structure assembled from two-dimensional sheets.

[0237] Fig.26 This is the TEM image of Pd-H4SiMo / AS-20H. It is observed that the catalyst is a three-dimensional porous hollow structure assembled from two-dimensional sheets, and no palladium particles are observed, indicating that the palladium is highly dispersed;

[0238] Fig. 27 The nitrogen adsorption and desorption diagram of Pd-H4SiMo / AS-20H shows a typical type IV adsorption and desorption curve with a type I hysteresis loop, indicating that there are a large number of mesoporous structures in the catalyst.

[0239] The catalyst is spherical with a diameter of about 177nm and a specific surface area of ​​about 682m 2 / g, average pore diameter is 6.4nm, average pore volume is 1.2cc / g, and average density is 2.8g / cm 3 .

[0240] Embodiment 18

[0241] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 14 mL of deionized water, stirring it thoroughly, and after uniform dispersion, successively adding 20 g of P123 and 50 g of aluminum isopropoxide, reacting it thoroughly at room temperature for 24 h, and then inducing solvent evaporation at 70 ° C. After 48 h, a gel is obtained, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C. for 3 h in an air atmosphere, with a heating rate of 5 ° C. / min, to obtain a metal oxide-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C. until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Pd-H3PMo / AS-14H.

[0242] The obtained catalyst was characterized in structure, and the actual loading amount of phosphomolybdic acid in the catalyst was 22%, and the actual loading amount of palladium was 0.7%;

[0243] Fig.28 This is the TEM image of Pd-H3PMo / AS-14H. It is observed that the catalyst is a three-dimensional porous hollow structure assembled from two-dimensional sheets. It can be seen that the hollowness of the catalyst decreases when the amount of water added decreases, and no palladium particles are observed, indicating that the palladium is highly dispersed.

[0244] The catalyst is spherical, with a diameter of about 157nm and a specific surface area of ​​about 619m 2 / g, average pore diameter is 6.3nm, average pore volume is 1.0cc / g, and average density is 3.1g / cm 3 .

[0245] Embodiment 19

[0246] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 8 mL of deionized water, stirring it thoroughly, and after uniform dispersion, successively adding 20 g of P123 and 50 g of aluminum isopropoxide, fully reacting at room temperature for 24 h, then inducing solvent evaporation at 70 ° C, and obtaining a gel after 48 h, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C for 3 h in an air atmosphere, with a heating rate of 5 ° C / min, to obtain a metal oxide-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Pd-H3PMo / AS-8H.

[0247] The structure of the catalyst was characterized. The actual loading amount of phosphomolybdic acid in the catalyst was 22%, and the actual loading amount of palladium was 0.6%.

[0248] Fig.29 The TEM image shows that as the amount of water added further decreases, the hollow structure is no longer obvious. No palladium particles are observed, indicating that palladium is highly dispersed.

[0249] The catalyst is spherical, with a diameter of about 152nm and a specific surface area of ​​about 384m 2 / g, the average pore size is about 6.6nm, the average pore volume is about 0.7cc / g, and the average density is about 3.3g / cm 3 .

[0250] Embodiment 20

[0251] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 2 mL of deionized water, stirring it thoroughly, and then adding 20 g of P123 and 50 g of aluminum isopropoxide in sequence after being uniformly dispersed at room temperature, reacting it thoroughly for 24 h, and then inducing solvent evaporation at 70 ° C. After 48 h, a gel is obtained, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C for 3 h in an air atmosphere, and the heating rate is 5 ° C / min to obtain a metal oxide-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Pd-H3PMo / AS-2H.

[0252] The obtained catalyst was characterized in structure. The actual loading amount of phosphomolybdic acid in the catalyst was 23%, and the actual loading amount of palladium was 0.6%.

[0253] Fig.30 This is a TEM image. It was observed that when the amount of water added was reduced to 2 mL, the hollow degree was lower and no palladium particles were observed, indicating that the palladium was highly dispersed.

[0254] The catalyst is spherical, with a diameter of about 141nm and a specific surface area of ​​about 573m 2 / g, the average pore size is about 5.5nm, the average pore volume is about 0.8cc / g, and the average density is about 2.9g / cm 3 .

[0255] Embodiment 21

[0256] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 30 mL of deionized water, stirring it thoroughly, and after uniform dispersion, successively adding 20 g of P123 and 50 g of aluminum isopropoxide, reacting it thoroughly at room temperature for 24 h, and then inducing solvent evaporation at 70 ° C. After 48 h, a gel is obtained, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C. for 3 h in an air atmosphere, with a heating rate of 5 ° C. / min, to obtain a metal oxide-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C. until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Pd-H3PMo / AS-30H.

[0257] The obtained catalyst was characterized in structure, and the actual loading amount of phosphomolybdic acid in the catalyst was 22%, and the actual loading amount of palladium was 0.6%.

[0258] Fig.31 This is the TEM image of Pd-H3PMo / AS-30H. It was observed that the catalyst has a three-dimensional porous structure and no palladium particles were observed, indicating that the palladium is highly dispersed.

[0259] The specific surface area of ​​the catalyst is about 480m 2 / g, average pore diameter is 9.2nm, average pore volume is 1.1cc / g, and average density is 3.1g / cm 3 .

[0260] Embodiment 22

[0261] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 50 mL of deionized water, stirring it thoroughly, and after uniform dispersion, successively adding 20 g of P123 and 50 g of aluminum isopropoxide, fully reacting at room temperature for 24 h, then inducing solvent evaporation at 70 ° C, and obtaining a gel after 48 h, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C for 3 h in an air atmosphere, with a heating rate of 5 ° C / min, to obtain a metal oxide-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Pd-H3PMo / AS-50H.

[0262] The obtained catalyst was characterized in structure. The actual loading amount of phosphomolybdic acid in the catalyst was 22%, and the actual loading amount of palladium was 0.5%.

[0263] Fig.32 This is the TEM image of Pd-H3PMo / AS-50H. It was observed that the catalyst has a three-dimensional porous structure and no palladium particles were observed, indicating that the palladium is highly dispersed.

[0264] The catalyst is in the form of nanosheets with a specific surface area of ​​about 402 m 2 / g, the average pore size is about 8.6nm, the average pore volume is about 1.0cc / g, and the average density is about 3.3g / cm 3 .

[0265] Embodiment 23

[0266] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 100 mL of deionized water, stirring it thoroughly, and then adding 20 g of P123 and 50 g of aluminum isopropoxide in sequence after uniform dispersion, reacting it thoroughly at room temperature for 24 h, and then inducing solvent evaporation at 70 ° C. After 48 h, a gel is obtained, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C for 3 h in an air atmosphere, and the heating rate is 5 ° C / min to obtain a metal oxide-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Pd-H3PMo / AS-100H.

[0267] The obtained catalyst was characterized in structure. The actual loading amount of phosphomolybdic acid in the catalyst was 23%, and the actual loading amount of palladium was 0.6%.

[0268] Fig.33 This is the TEM image of Pd-H3PMo / AS-100H. It was observed that the catalyst has a three-dimensional porous structure and no palladium particles were observed, indicating that the palladium is highly dispersed.

[0269] The catalyst is in the form of nanosheets with a specific surface area of ​​about 441 m 2 / g, the average pore diameter is about 11.7nm, the average pore volume is about 1.29cc / g, and the average density is about 3.2g / cm 3 .

[0270] Embodiment 24

[0271] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and after uniform dispersion, successively adding 20 g of P123 and 50 g of aluminum isopropoxide, reacting it thoroughly at room temperature for 24 h, and then inducing solvent evaporation at 70 ° C. After 48 h, a gel is obtained, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C. for 3 h in an air atmosphere, with a heating rate of 5 ° C. / min, to obtain a metal oxide-supported heteropoly acid. 31.2 mL of acetylacetonate platinum solution (100 mg of acetylacetonate platinum dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C. until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 200°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Pt-H3PMo / AS-20H.

[0272] The obtained catalyst was characterized in structure. The actual loading amount of phosphomolybdic acid in the catalyst was 22%, and the actual loading amount of platinum was 0.6%.

[0273] Fig.34 This is the XRD diagram of Pt-H3PMo / AS-20H. It was observed that there were no characteristic diffraction peaks of heteropoly acid molecules or platinum, indicating that the heteropoly acid and platinum were uniformly dispersed on the catalyst.

[0274] Fig.35 This is the TEM image of Pt-H3PMo / AS-20H. It was observed that the catalyst is a three-dimensional porous hollow structure assembled from two-dimensional sheets, and no palladium particles were observed, indicating that platinum is highly dispersed.

[0275] The catalyst is spherical, with a diameter of about 180nm and a specific surface area of ​​about 690m 2 / g, the average pore size is about 6.7nm, the average pore volume is about 1.3cc / g, and the average density is about 2.7g / cm 3 .

[0276] Embodiment 25

[0277] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and after uniform dispersion, successively adding 20 g of P123 and 50 g of aluminum isopropoxide, reacting it thoroughly at room temperature for 24 h, and then inducing solvent evaporation at 70 ° C. After 48 h, a gel is obtained, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C. for 3 h in an air atmosphere, with a heating rate of 5 ° C. / min, to obtain a metal oxide-supported heteropoly acid. 31.2 mL of cobalt nitrate solution (100 mg of cobalt nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C. until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Co-H3PMo / AS-20H.

[0278] The obtained catalyst was characterized in structure. The actual loading amount of phosphomolybdic acid in the catalyst was 23%, and the actual loading amount of cobalt was 0.7%.

[0279] Fig.36 This is the XRD diagram of Co-H3PMo / AS-20H. It was observed that there were no characteristic diffraction peaks of heteropoly acid molecules or cobalt, indicating that the heteropoly acid and cobalt were uniformly dispersed on the catalyst.

[0280] Embodiment 26

[0281] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and after uniform dispersion, successively adding 20 g of P123 and 50 g of aluminum isopropoxide, reacting it thoroughly at room temperature for 24 h, and then inducing solvent evaporation at 70 ° C. After 48 h, a gel is obtained, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C. for 3 h in an air atmosphere, with a heating rate of 5 ° C. / min, to obtain a metal oxide-supported heteropoly acid. 31.2 mL of nickel nitrate solution (100 mg of nickel nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C. until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Ni-H3PMo / AS-20H.

[0282] The obtained catalyst was characterized in structure. The actual loading amount of phosphomolybdic acid in the catalyst was 23%, and the actual loading amount of nickel was 0.5%.

[0283] Fig.37 This is the XRD diagram of Ni-H3PMo / AS-20H. It was observed that there were no characteristic diffraction peaks of heteropoly acid molecules or nickel, indicating that the heteropoly acid and nickel were uniformly dispersed on the catalyst.

[0284] Examples 27-35

[0285] These embodiments provide a method for preparing a catalyst and the catalyst prepared therefrom, which are basically the same as those in Example 14, except that some raw materials or their amounts are different, as shown in Table 1 for details.

[0286] Table 1

[0287]

[0288] Embodiment 36

[0289] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and after it is evenly dispersed, sequentially adding 20 g of P123, 31.2 mg of palladium nitrate and 50 g of aluminum isopropoxide, reacting it fully at room temperature for 24 h, and then inducing solvent evaporation at 70 ° C. After 48 h, a gel is obtained, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C for 3 h in an air atmosphere, and the heating rate is 5 ° C / min to obtain a metal oxide-supported heteropoly acid. Next, the obtained sample is reduced at 250 ° C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst is obtained after natural cooling, which is recorded as Pd@H3PMo / AS-20H.

[0290] The obtained catalyst was characterized in structure. The actual loading amount of phosphomolybdic acid in the catalyst was 23%, and the actual loading amount of palladium was 0.7%.

[0291] Fig.38 This is the XRD diagram of Pd@H3PMo / AS-20H. It was observed that there were no characteristic diffraction peaks of heteropoly acid molecules or palladium, indicating that the heteropoly acid and palladium were uniformly dispersed on the catalyst.

[0292] Fig.39 This is the TEM image of Pd@H3PMo / AS-20H. It was observed that the catalyst is a three-dimensional porous hollow structure assembled from two-dimensional sheets, and no palladium particles were observed, indicating that the palladium is highly dispersed.

[0293] The catalyst is spherical, with a diameter of about 166nm and a specific surface area of ​​about 625m 2 / g, the average pore size is about 6.7nm, the average pore volume is about 1.1cc / g, and the average density is about 3.1g / cm 3 .

[0294] Embodiment 37

[0295] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous isopropanol and 20 mL of deionized water, stirring it thoroughly, and after uniform dispersion, successively adding 20 g of P123 and 50 g of aluminum isopropoxide, reacting it thoroughly at room temperature for 24 h, and then inducing solvent evaporation at 85 ° C. After 48 h, a gel is obtained, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C. for 3 h in an air atmosphere, with a heating rate of 5 ° C. / min, to obtain a metal oxide-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C. until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Pd-H3PMo / AS-20H-85.

[0296] The obtained catalyst was characterized in structure. The actual loading amount of phosphomolybdic acid in the catalyst was 23%, and the actual loading amount of palladium was 0.6%.

[0297] Fig.40 This is the TEM image of Pd-H3PMo / AS-20H-85. It was observed that the catalyst has a hollow porous spherical structure and no palladium particles were observed, indicating that the palladium is highly dispersed.

[0298] Embodiment 38

[0299] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and after uniform dispersion, successively adding 20 g of P123 and 50 g of triisobutylaluminum, fully reacting at room temperature for 24 h, then inducing solvent evaporation at 70 ° C, and obtaining a gel after 48 h, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C for 3 h in an air atmosphere, with a heating rate of 5 ° C / min, to obtain a metal oxide-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Pd-H3PMo / AS-20H-T.

[0300] Embodiment 39

[0301] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and after uniform dispersion, successively adding 20 g of P123 and 50 g of aluminum acetate, fully reacting at room temperature for 24 h, then inducing solvent evaporation at 70 ° C, and obtaining a gel after 48 h, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C for 3 h in an air atmosphere, with a heating rate of 5 ° C / min, to obtain a metal oxide-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Pd-H3PMo / AS-20H-E.

[0302] Embodiment 40

[0303] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and after uniform dispersion, successively adding 20 g of F127 and 50 g of aluminum isopropoxide, reacting it thoroughly at room temperature for 24 h, and then inducing solvent evaporation at 70 ° C. After 72 h, a gel is obtained, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C. for 3 h in an air atmosphere, with a heating rate of 5 ° C. / min, to obtain a metal oxide-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C. until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Pd-H3PMo / AS-F-20H.

[0304] The obtained catalyst was characterized in structure. The actual loading amount of phosphomolybdic acid in the catalyst was 22%, and the actual loading amount of palladium was 0.6%.

[0305] Fig.41 This is the TEM image of Pd-H3PMo / AS-F-20H. It was observed that the catalyst is a three-dimensional porous hollow structure assembled from two-dimensional sheets, and no palladium particles were observed, indicating that the palladium is highly dispersed.

[0306] The catalyst is spherical, with a diameter of about 174nm and a specific surface area of ​​about 630m 2 / g, the average pore size is about 7.1nm, the average pore volume is about 1.2cc / g, and the average density is about 3.1g / cm 3 .

[0307] Embodiment 41

[0308] This example provides a method for preparing a catalyst and a catalyst prepared therefrom. Specifically, the method for preparing the catalyst comprises: weighing 2.9 g of phosphomolybdic acid, mixing it with 500 mL of anhydrous ethanol and 20 mL of deionized water, stirring it thoroughly, and after uniform dispersion, successively adding 20 g of hexadecyltrimethylammonium bromide (CTAB) and 50 g of aluminum isopropoxide, reacting them thoroughly at room temperature for 24 h, and then inducing solvent evaporation at 70 ° C. After 10 h, a gel is obtained, which is then placed in an oven and dried overnight. The solid obtained after drying is placed in a muffle furnace, calcined at 350 ° C. for 3 h in an air atmosphere, with a heating rate of 5 ° C. / min, to obtain a metal oxide-supported heteropoly acid. 31.2 mL of palladium nitrate solution (100 mg of palladium nitrate dissolved in 100 mL of acetone) is added to 150 mL of acetone and stirred thoroughly. Then, 3 g of metal oxide-supported heteropoly acid is ultrasonically dispersed in the above solution. After continuous stirring for 6 h, the mixture is heated to 40 ° C. until the acetone is completely evaporated. The obtained solid was then placed in a muffle furnace and calcined at 300°C for 2 h at a heating rate of 5°C / min in an air atmosphere. Next, the obtained sample was reduced at 250°C for 2 h in a pure H2 atmosphere in a muffle furnace, and the catalyst was obtained after natural cooling, which was recorded as Pd-H3PMo / AS-C-20H.

[0309] The obtained catalyst was characterized in structure. The actual loading amount of phosphomolybdic acid in the catalyst was 23%, and the actual loading amount of palladium was 0.5%.

[0310] Fig.42 This is the TEM image of Pd-H3PMo / AS-C-20H. It was observed that the catalyst is a three-dimensional porous hollow structure assembled from two-dimensional sheets, and no palladium particles were observed, indicating that the palladium is highly dispersed.

[0311] The catalyst is spherical, with a diameter of about 173nm and a specific surface area of ​​about 641m 2 / g, the average pore diameter is about 6.9nm, the average pore volume is about 1.2cc / g, and the average density is about 3.2g / cm 3 .

[0312] Comparative Example 1

[0313] This example provides a method for preparing a catalyst and the catalyst prepared therefrom, and the specific preparation steps include:

[0314] 20 g of polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123) was placed in 400 mL of anhydrous ethanol, and 2.2 g of phosphomolybdic acid was dispersed in 80 mL of anhydrous ethanol, and then uniformly added dropwise to the ethanol solution of polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer, and stirred to mix, to obtain a first configuration.

[0315] 40.8 g of aluminum isopropoxide was placed in the first configuration and stirred for 6 hours to obtain a second configuration.

[0316] The second configuration was placed in an oven at 60°C for aging for 48 hours to obtain a solid mixture, and the solid mixture was calcined in an air furnace at a calcination temperature of 350°C, a heating rate of 1°C / min, and a calcination time of 4 hours to obtain the catalyst H3PMo@AS.

[0317] Fig.43 This is the XRD image of H3PMo@AS prepared in this example. It can be seen from the figure that the diffraction peak of heteropoly acid appears, indicating that the heteropoly acid is not dispersed on the catalyst in a single molecule state.

[0318] Comparative Example 2

[0319] The method is basically the same as Example 14, except that phosphomolybdic acid is replaced by an aprotic heteropoly acid, ammonium phosphomolybdate, of equal mass. The obtained catalyst is recorded as Pd-APMo / AS-20H.

[0320] The obtained catalyst was characterized in structure. The actual loading amount of ammonium phosphomolybdate in the catalyst was about 21%, and the actual loading amount of palladium was about 0.3%.

[0321] Fig.44 Figure 2 is the XRD pattern of Pd-APMo / AS-20H. It is observed that the XRD spectrum of the composite sample shows the characteristic diffraction peak of ammonium phosphomolybdate, indicating that the salt form of non-proton heteropoly acid-heteropoly acid cannot be monodispersed on the porous alumina support. This can be attributed to the lack of proton H + When the reaction is not complete, the interaction between the raw materials is insufficient, resulting in the inability to achieve good dispersion of the salt form of the aprotic heteropolyacid-heteropolysalt.

[0322] Fig.45 This is the TEM image of Pd-APMo / AS-20H. It was observed that the catalyst basically presents a two-dimensional nanosheet structure.

[0323] Comparative Example 3

[0324] The method is basically the same as Example 1, except that the deionized water is replaced with an equal volume of anhydrous ethanol. The obtained catalyst is recorded as H3PMo / AS-ethanol.

[0325] Fig.46 The TEM image of H3PMo / AS-ethanol shows that only a solid structure can be obtained without adding water, proving that water is a necessary condition for the formation of a hollow structure.

[0326] Application Example 1

[0327] The catalytic performance of the catalysts prepared in Examples 1-13 and Comparative Examples 1 and 3 in the selective oxidation of 2-methylbutyraldehyde to prepare 2-methylbutyric acid was evaluated using a reactor. The operation process is as follows:

[0328] The operation process is as follows: 4g catalyst and 800g 2-methylbutyraldehyde are added to a 2L reactor in sequence, oxygen is continuously introduced after nitrogen replacement, the oxygen flow rate is 30mL / min, the temperature is raised to 45°C for reaction, and the reaction is stopped after 8 hours. After separation, the product is analyzed by Shimadzu GC2014 gas chromatograph, in which the chromatographic column is HP-INNOWax and the detector is FID detector. The conversion rate of 2-methylbutyraldehyde and the selectivity of 2-methylbutyric acid are calculated by normalization method, and the calculation results are shown in Table 2.

[0329] Table 2

[0330] catalyst Conversion rate (%) Selectivity (%) Example 1 100 94.6 Example 2 99.7 93.2 Example 3 98.9 94.1 Example 4 99.3 93.6 Example 5 96.4 94.0 Example 6 95.0 92.7 Example 7 93.2 91.8 Example 8 100 94.1 Example 9 99.9 94.0 Example 10 100 93.8 Embodiment 11 92.7 90.8 Example 12 94.2 92.1 Example 13 92.9 93.0 Comparative Example 1 78.4 87.6 Comparative Example 3 76.2 85.9

[0331] Application Example 2

[0332] The catalytic performance of the catalysts prepared in Examples 1-13 and Comparative Examples 1 and 3 in the esterification reaction of lauric acid and methanol to prepare dimethyl laurate was evaluated using a reactor. The operation process is as follows:

[0333] 0.02g catalyst, 10g lauric acid and 30g methanol were added to a 100mL autoclave in turn, and the temperature was raised to 60°C for 12h. After separation, the reaction products were analyzed by Shimadzu GC2014 gas chromatograph, where the chromatographic column was HP-INNOWax and the detector was FID detector. The conversion rate of lauric acid and the selectivity of dimethyl laurate were calculated by normalization method. The specific results are shown in Table 3.

[0334] Table 3

[0335]

[0336]

[0337] Application Example 3

[0338] The performance of the catalysts prepared in Examples 1 to 14, Example 25, Example 26 and Comparative Examples 1 to 3 in the continuous alkylation of propylene and m-cresol to prepare thymol was evaluated: a stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, the length was 600 mm, and the catalyst loading was 10 g. Reaction conditions: reaction temperature 220°C, reaction pressure 0.2 MPa, mass liquid hourly space velocity of m-cresol was 2.5 h -1 , the molar ratio of propylene to m-cresol is 0.6:1, and the operation time is 200h.

[0339] See Table 4 for specific results.

[0340] Table 4

[0341]

[0342]

[0343] Application Example 4 (Hydrogenation of o-tert-butylphenol)

[0344] (1) The performance of the catalysts prepared in Examples 14-23, Example 33, Examples 36-41 and Comparative Example 2 in the hydrogenation of o-tert-butylphenol to prepare o-tert-butyl cyclohexanol was evaluated. The operation process was as follows: a stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, and the length was 600 mm. The catalyst loading was 10 g. The reaction pressure was 3 MPa, the reaction temperature was 80-85°C, and the mass liquid hourly space velocity of o-tert-butylphenol was 1 h -1 , hydrogen is the hydrogenating agent, and the molar ratio of hydrogen to o-tert-butylphenol is 5:1.

[0345] See Table 5 for specific results.

[0346] Table 5

[0347]

[0348] Application Example 5 (Hydrogenation of Cyclopentylbutyrolactone)

[0349] (1) The performance of the catalysts prepared in Examples 14-23, Example 33, Examples 36-41 and Comparative Example 2 in the hydrogenation reaction of cyclopentylbutyrolactone was evaluated. The operation process was as follows: 0.1 g of catalyst, 20 g of cyclopentylbutyrolactone, and 20 g of methanol were added to a 100 mL autoclave in sequence, and the pressure was increased to 4 MPa after hydrogen replacement, and then the temperature was raised to 150° C. for reaction for 12 h. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was an FID detector. The conversion rate and selectivity were calculated by the normalization method.

[0350] The reaction formula is:

[0351]

[0352] For specific results, see Table 6-1.

[0353] Table 6-1

[0354]

[0355] (2) Cyclic stability test:

[0356] The catalytic reaction was carried out in a fixed bed reactor, and the mass space velocity of cyclopentylbutyrolactone was 0.5h -1 The molar ratio of methanol to cyclopentylbutyrolactone is 5:1, the molar ratio of hydrogen to cyclopentylbutyrolactone is 20:1, the catalyst loading is 8g, the reaction temperature is 145°C, the reaction pressure is 4MPa, and the results of conversion rate and selectivity at each operating time stage are shown in Table 6-2.

[0357] Table 6-2

[0358]

[0359]

[0360] Application Example 6 (Preparation of 2-pentylcyclopentenone by hydroisomerization of 2-pentylidenecyclopentanone)

[0361] The reaction performance of the catalysts prepared in Examples 14-23, Example 33, Examples 36-41 and Comparative Example 2 in the preparation of 2-pentylcyclopentenone by hydroisomerization of 2-pentylcyclopentanone was evaluated. The operation process was as follows: 6 g of catalyst and 1200 g of 2-pentylcyclopentenone were added to a 2L reactor in sequence, and hydrogen was continuously introduced after nitrogen replacement at a hydrogen flow rate of 200 mL / min, and then the temperature was raised to 40°C and the reaction was carried out at a constant temperature for 12 hours. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was an FID detector.

[0362] The reaction formula is:

[0363]

[0364] See Table 7 for specific results.

[0365] Table 7

[0366]

[0367] Application Example 7 (Preparation of phenylpentanol by hydrogenation of rose ether)

[0368] The reaction performance of the catalyst prepared in Example 24 in the hydrogenation of rose oxide to prepare phenylpentanol was evaluated. The operation process was as follows: 0.1 g of catalyst and 50 g of rose oxide were added to a 100 mL high-pressure reactor in sequence, and the pressure was increased to 3 MPa after hydrogen replacement, and then the temperature was raised to 140° C. for reaction for 12 h. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was an FID detector. The conversion rate and selectivity were calculated by the normalization method.

[0369] The reaction formula is:

[0370]

[0371] See Table 8 for specific results.

[0372] Table 8

[0373]

[0374] Application Example 8 (Preparation of Ethylamine by Hydroamination of Ethanol)

[0375] Evaluation of the performance of the catalyst prepared in Example 25 in the preparation of ethylamine by ethanol amination: A stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, and the length was 600 mm, and the catalyst loading was 10 g. Reaction conditions: reaction temperature 140°C, reaction pressure 0.4 MPa, mass liquid hourly space velocity of ethanol 0.5 h -1 , the molar ratio of ammonia to alcohol is 1: 1. After separation, the product is analyzed by Agilent 7890 gas chromatograph, wherein the chromatographic column is HP-INNOWax and the detector is TCD detector.

[0376] The reaction formula is:

[0377]

[0378] See Table 9 for specific results.

[0379] Table 9

[0380]

[0381] Note: The selectivity of ethylamine is the total selectivity of monoethylamine + diethylamine + triethylamine.

[0382] Application Example 9 (Preparation of Isopropylamine by Amination of Acetone)

[0383] Evaluation of the performance of the catalyst prepared in Example 26 in the preparation of isopropylamine by amination of acetone: A stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, and the length was 600 mm, and the catalyst loading was 10 g. Reaction conditions: reaction temperature 90°C, reaction pressure 0.4 MPa, mass liquid hourly space velocity of acetone 2 h -1 , the molar ratio of ammonia to acetone is 2:1, and the molar ratio of hydrogen to acetone is 1.5:1. After separation, the products are analyzed by Agilent 7890 gas chromatograph, wherein the chromatographic column is HP-INNOWax and the detector is TCD detector.

[0384] The reaction formula is:

[0385]

[0386] See Table 10 for specific results.

[0387] Table 10

[0388]

[0389] Note: Isopropylamine selectivity refers to the total selectivity of monoisopropylamine and diisopropylamine.

[0390] Application Example 10 (Preparation of tert-butylamine by amination of isobutylene)

[0391] The performance of the catalyst prepared in Example 26 in the reaction of preparing tert-butylamine by amination of isobutylene was evaluated. A stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, the length was 600 mm, and the catalyst loading was 10 g. Reaction conditions: reaction temperature 170°C, reaction pressure 6 MPa, mass liquid hourly space velocity of isobutylene 0.5 h -1 , the molar ratio of ammonia to isobutylene is 1: 1. After separation, the product is analyzed by Agilent 7890 gas chromatograph, wherein the chromatographic column is HP-INNOWax and the detector is TCD detector.

[0392] The reaction formula is:

[0393]

[0394] See Table 11 for specific results.

[0395] Table 11

[0396]

[0397] Application Example 11

[0398] The performance of the catalysts prepared in Examples 1 to 4, 14-17 and Comparative Examples 1-3 in the hydrogen peroxide oxidation reaction of benzyl alcohol was evaluated. The operation process was as follows: 10 g of catalyst, 600 g of benzyl alcohol, 620 mL of 30% by mass hydrogen peroxide and 1000 mL of acetonitrile were added in sequence into a 5 L round-bottom flask, condensed and refluxed, and the temperature was raised to 60° C. for reaction for 10 h.

[0399] The reaction formula is:

[0400]

[0401] See Table 12 for specific results.

[0402] Table 12

[0403]

[0404] Application Example 12 (Selective Oxidation Reaction of C3-C10 Aldehydes)

[0405] The performance of the catalysts prepared in Examples 1 to 14, Examples 25, 26 and Comparative Examples 1-3 in the selective oxidation of C3-C10 aldehydes to prepare the corresponding acid was evaluated. The operation process was as follows: 4 g of catalyst and 800 g of substrate were added to a 2L reactor in sequence, and oxygen was continuously introduced after nitrogen replacement at an oxygen flow rate of 30 mL / min. The temperature was raised to 45°C for reaction, and the reaction was stopped after 8 hours. After separation, the product was analyzed using a Shimadzu GC2014 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was a FID detector.

[0406] See Table 13 for specific results.

[0407] Table 13

[0408]

[0409]

[0410]

[0411] Application Example 13 (Selective oxidation of alcohol to produce acid)

[0412] The performance of the catalysts prepared in Examples 1 to 14, Example 25, Example 26 and Comparative Examples 1-3 in the selective oxidation of alcohol to produce acid was evaluated. The operation process was as follows: 4 g of catalyst and 800 g of substrate were added to a 2L reactor in sequence, oxygen was continuously introduced after nitrogen replacement, the pressure was increased to 0.5 MPa, the oxygen flow rate was 50 mL / min, the temperature was increased to 95 ° C, and the reaction was stopped after 8 hours. After separation, the product was analyzed by Shimadzu GC2014 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was FID detector. The conversion rate and selectivity were calculated by normalization method.

[0413] See Table 14 for specific results.

[0414] Table 14

[0415]

[0416]

[0417] Application Example 14 (Selective oxidation of aromatic hydrocarbons to prepare aromatic acids)

[0418] The performance of the catalysts prepared in Examples 1 to 14, Example 25, Example 26 and Comparative Examples 1-3 in the selective oxidation of aromatic hydrocarbons to prepare aromatic acids was evaluated. The operation process was as follows: 4 g of catalyst and 800 g of substrate were added to a 2L reactor in sequence, oxygen was continuously introduced after nitrogen replacement, the pressure was increased to 2 MPa, the oxygen flow rate was 50 mL / min, the temperature was increased to 145 ° C, and the reaction was stopped after 8 hours of reaction. After separation, the product was analyzed by Shimadzu GC2014 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was FID detector. The conversion rate and selectivity were calculated by normalization method.

[0419] See Table 15 for specific results.

[0420] Table 15

[0421]

[0422] Application Example 15 (Esterification Reaction)

[0423] The catalysts prepared in Examples 1 to 14, Example 25, Example 26 and Comparative Examples 1 to 3 were evaluated for their esterification performance with 2-methylbutyric acid and methanol, ethanol, isopropanol, n-butanol and n-hexanol. The operation process was as follows: 0.1 g of catalyst and 20 g of 2-methylbutyric acid and the corresponding alcohol (the acid-alcohol molar ratio was controlled to be 0.7:1) were added sequentially into a 100 mL autoclave, and the temperature was raised to 65°C for 6 h. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was an FID detector. The conversion rate and selectivity were calculated by the normalization method.

[0424] For specific results, please refer to Table 16 (the conversion rate is the conversion rate of 2-methylbutyric acid, and the selectivity is the selectivity of the corresponding ester prepared).

[0425] Table 16

[0426]

[0427] Application Example 16 (Esterification Reaction)

[0428] The esterification performance of the catalysts prepared in Examples 1 to 14, Example 25, Example 26 and Comparative Examples 1 to 3 in salicylic acid with n-pentanol, n-hexanol, benzyl alcohol, leaf alcohol, cyclohexanol, isooctyl alcohol and isophorol was evaluated. The operation process was as follows: 4 g of catalyst and 800 g of salicylic acid and the corresponding alcohol (the acid-alcohol molar ratio was controlled to be 0.95:1) were added in sequence to a 2L reactor, the temperature was raised to 80°C, the system pressure was controlled to be 500 mmHg, the water produced was separated by a water separator, the oil phase was refluxed, and the reaction was performed for 6 hours. After separation, the product was analyzed by Agilent 1260 liquid chromatograph. The conversion rate and selectivity were calculated by normalization method.

[0429] For specific results, please refer to Table 17 (the conversion rate is the conversion rate of salicylic acid, and the selectivity is the selectivity of the corresponding ester prepared).

[0430] Table 17

[0431]

[0432] Application Example 17 (Esterification Reaction)

[0433] The catalysts prepared in Examples 1 to 14, Example 25, Example 26 and Comparative Examples 1 to 3 were evaluated for their esterification performance in acetic acid, hexanoic acid, heptanoic acid, phenylpropionic acid, phenoxyacetic acid, cyclohexyloxyacetic acid and allyl alcohol. The operation process was as follows: 0.1 g of catalyst and 20 g of allyl alcohol and the corresponding acid (the acid-alcohol molar ratio was controlled to be 1.1:1) were added sequentially into a 100 mL autoclave, and the temperature was raised to 75°C for 9 hours. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was an FID detector. The conversion rate and selectivity were calculated by the normalization method.

[0434] See Table 18 for specific results.

[0435] Table 18

[0436]

[0437] Application Example 18 (Esterification Reaction)

[0438] The catalysts prepared in Examples 1 to 14, Example 25, Example 26 and Comparative Examples 1-3 were evaluated for their esterification performance in catalyzing acetic acid with o-tert-butyl cyclohexanol, p-tert-butyl cyclohexanol, α-phenylethanol and β-phenylethanol. The operation process was as follows: 4 g of catalyst and 800 g of acetic acid and the corresponding alcohol (the acid-alcohol molar ratio was controlled to be 1.2) were added sequentially to a 2L reactor, the temperature was raised to 80°C, the vacuum degree of the system was controlled to be 500 mmHg, the water produced was separated by a water separator, the oil phase was refluxed, and the reaction was performed for 6 hours. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was an FID detector. The conversion rate and selectivity were calculated by the normalization method.

[0439] See Table 19 for specific results.

[0440] Table 19

[0441]

[0442]

[0443] Application Example 19 (Esterification Reaction)

[0444] The catalysts prepared in Examples 1 to 14, Example 25, Example 26 and Comparative Examples 1 to 3 were evaluated for their esterification performance in acetic acid, propionic acid, n-butyric acid, isobutyric acid and dicyclopentadiene. The operation process was as follows: 4 g of catalyst and 800 g of dicyclopentadiene and the corresponding acid (the acid-ene molar ratio was controlled to be 1.2:1) were added sequentially to a 2L reactor, and the temperature was raised to 80°C for reaction for 6 hours. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was an FID detector. The conversion rate and selectivity were calculated by the normalization method.

[0445] See Table 20 for specific results.

[0446] Table 20

[0447]

[0448]

[0449] Application Example 20

[0450] (1) Preparation of epoxide pinane by reaction of α-pinene with hydrogen peroxide

[0451] The reaction performance of the catalysts prepared in Examples 14-26, Example 33, Example 36-41 and Comparative Examples 1-3 in the preparation of epoxy pinane by the reaction of α-pinene with hydrogen peroxide was evaluated. The operation process was as follows: 4g of catalyst, 600g of toluene, and 300g of α-pinene were added to a 2L reactor in sequence, the temperature was raised to 70°C, 200g of hydrogen peroxide (mass fraction 50%) was added dropwise, the addition was continued for 12 hours, and the reaction was continued at a constant temperature for 3 hours. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was an FID detector.

[0452] Reaction:

[0453]

[0454] (2) Preparation of epoxylimonene by reaction of limonene with hydrogen peroxide

[0455] The reaction performance of the catalysts prepared in Examples 14-26, Example 33, Example 36-41 and Comparative Examples 1-3 in the preparation of epoxy limonene by the reaction of limonene with hydrogen peroxide was evaluated. The operation process was as follows: 4g of catalyst, 600g of toluene, and 300g of limonene were added to a 2L reactor in sequence, the temperature was raised to 70°C, 60g of hydrogen peroxide (mass fraction 50%) was added dropwise, the addition lasted for 8 hours, and the reaction was carried out at a constant temperature for 3 hours. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, in which the chromatographic column was HP-INNOWax and the detector was a FID detector.

[0456] Reaction:

[0457]

[0458] See Table 21 for specific results.

[0459] Table 21

[0460]

[0461]

[0462] Application Example 22 (Isomerization of o-cresol to prepare m-cresol and p-cresol)

[0463] Evaluation of the performance of the catalysts prepared in Examples 1 to 14, Example 25, Example 26 and Comparative Examples 1 to 3 in the isomerization of o-cresol to prepare m-cresol and p-cresol: A stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, the length was 600 mm, and the catalyst loading was 10 g. Reaction conditions: reaction temperature 280°C, reaction pressure 0.15 MPa, mass liquid hourly space velocity of o-cresol was 0.8 h -1 , run for 100h. The single-pass conversion rate of o-cresol, m-cresol selectivity and p-cresol selectivity were analyzed by chromatography.

[0464] See Table 23 for specific results.

[0465] Table 23

[0466]

[0467]

[0468] Application Example 23 (Preparation of 2-pentylidenecyclopentanone by dehydration of 2-(1-hydroxypentyl)-cyclopentanone)

[0469] The reaction performance of the catalyst prepared in Examples 1 to 14, Example 25, Example 26 and Comparative Examples 1-3 in the dehydration of 2-(1-hydroxypentyl)-cyclopentanone to prepare 2-pentylidenecyclopentanone was evaluated. The operation process was as follows: 6 g of catalyst and 1200 g of 2-(1-hydroxypentyl)-cyclopentanone were added to a 2L reactor in sequence, and the temperature was raised to 90°C. The vacuum degree of the system was controlled to be about 350 mmHg, and the reaction was carried out at a constant temperature for 12 hours. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was a FID detector.

[0470] Reaction:

[0471]

[0472] See Table 24 for specific results.

[0473] Table 24

[0474]

[0475]

[0476] Application Example 24 (Preparation of Habanolide by Dehydration of Hydroxycyclopentadecalactone)

[0477] The reaction performance of the catalysts prepared in Examples 1 to 14, Example 25, Example 26 and Comparative Examples 1-3 in the dehydration of hydroxycyclopentadecalactone to prepare harpa lactone was evaluated. The operation process was as follows: 6 g of catalyst and 1200 g of hydroxycyclopentadecalactone were added to a 2L reactor in sequence, and the temperature was raised to 100°C. The vacuum degree of the system was controlled to be about 350 mmHg, and the reaction was carried out at a constant temperature for 12 hours. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, in which the chromatographic column was HP-INNOWax and the detector was a FID detector.

[0478] Reaction:

[0479]

[0480] See Table 25 for specific results.

[0481] Table 25

[0482]

[0483]

[0484] Application Example 25

[0485] The reaction performance of the catalysts prepared in Examples 1-5, 14, 25, 26 and Comparative Examples 1-3 in the etherification of isopropyl alcohol to prepare isopropyl ether was evaluated. The operation process was as follows: 3 g of catalyst, 600 g of isopropyl alcohol, and 600 g of cyclohexane were added to a 2L reactor in sequence, and the temperature was raised to 69° C. and the reaction was carried out at a constant temperature for 12 hours. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, wherein the chromatographic column was HP-INNOWax and the detector was a FID detector.

[0486] See Table 26 for specific results.

[0487] Table 26

[0488]

[0489]

[0490] Application Example 26 (Preparation of Isopropyl Alcohol by Hydration of Propylene)

[0491] The performance of the catalysts prepared in Examples 1 to 14, Example 25, Example 26 and Comparative Examples 1 to 3 in the preparation of isopropanol by hydration of propylene was evaluated: a stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, the length was 600 mm, and the catalyst loading was 10 g. Reaction conditions: reaction temperature was 150°C, reaction pressure was 7 MPa, and the volumetric liquid hourly space velocity of propylene was 0.8 h -1 , the molar ratio of water to propylene is 10: 1. After separation, the product is analyzed by Agilent 7890 gas chromatograph, wherein the chromatographic column is HP-INNOWax and the detector is FID detector.

[0492] See Table 27 for specific results.

[0493] Table 27

[0494]

[0495] Application Example 27 (Preparation of Cyclopentadecalactone by Hydrogenation of Habanolide)

[0496] The reaction performance of the catalyst prepared in Example 24 in the hydrogenation of halba lactone to prepare cyclopentadecalactone was evaluated. The operation process was as follows: 0.1 g of catalyst and 50 g of halba lactone were added to a 100 mL high-pressure reactor in sequence, and the pressure was filled to 0.5 MPa after hydrogen replacement, and then the temperature was raised to 40°C for reaction for 12 hours. After separation, the product was analyzed by an Agilent 7890 gas chromatograph, in which the chromatographic column was HP-INNOWax and the detector was an FID detector. The conversion rate and selectivity were calculated by the normalization method.

[0497] The reaction formula is:

[0498]

[0499] See Table 28 for specific results.

[0500] Table 28

[0501]

[0502] Application Example 28 (Preparation of p-tert-butyl cyclohexanol by hydrogenation of p-tert-butylphenol)

[0503] The performance of the catalyst prepared in Example 25 in the hydrogenation reaction of tert-butylphenol was evaluated. The operation process was as follows: a stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, and the length was 600 mm. The catalyst loading was 10 g. The reaction pressure was 3 MPa, the reaction temperature was 80-85°C, and the mass liquid hourly space velocity of tert-butylphenol was 0.5 h -1 , hydrogen is used as the hydrogenating agent, and the molar ratio of hydrogen to p-tert-butylphenol is 5:1.

[0504] See Table 29 for specific results.

[0505] Table 29

[0506]

[0507] Application Example 29

[0508] The performance of the catalysts prepared in Examples 27-32 and 34-35 in the hydrogenation of thymol to produce menthol was evaluated. The operation process was as follows: a stainless steel tube was used as a reactor, wherein the outer diameter was 16 mm, the inner diameter was 12 mm, and the length was 600 mm. The catalyst loading was 10 g. The reaction pressure was 4 MPa, the reaction temperature was 140-150°C, and the mass liquid hourly space velocity of thymol was 0.5 h -1 , hydrogen is the hydrogenating agent, and the molar ratio of hydrogen to thymol is 10:1.

[0509] See Table 30 for specific results.

[0510] Table 30

[0511]

[0512]

[0513] Application Example 30 (Aldol Condensation Reaction)

[0514] The catalytic performance of the catalysts prepared in Examples 1 to 14, Example 25, Example 26 and Comparative Examples 1 to 3 in the aldol condensation reaction of cyclopentanone and n-valeraldehyde to prepare 2-pentylidenecyclopentanone was evaluated using a reactor, and the operation process was as follows:

[0515] Under nitrogen atmosphere, 168g of cyclopentanone and 3.4g of catalyst were added to the autoclave, the pressure was increased to 1MPa, stirring was started and the temperature was raised to 130°C; then 68g of n-valeraldehyde was added dropwise (addition time 6h), and the temperature was kept constant for 2h after the addition was completed. The catalyst was separated from the reaction liquid by filtration, and the quantitative analysis of the reaction liquid was carried out on an Agilent 7890 gas chromatograph, using a chromatographic column HP-INNOWax and a FID detector for detection.

[0516] See Table 31 for specific results.

[0517] Table 31

[0518]

[0519]

[0520] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

[0521] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

Claims

1. A catalyst, characterized in that: The catalyst includes a metal oxide support having a three-dimensional porous structure and a heteropoly acid dispersed in a single molecule state and connected to the metal oxide support, wherein the heteropoly acid is a proton type heteropoly acid capable of providing hydrogen ions.

2. The catalyst according to claim 1, characterized in that: In the proton-type heteropolyacid, heteroatoms and polyatoms are coordinated and bridged by oxygen atoms, the heteroatoms include at least one selected from P, Si, Fe, and Co, and the polyatoms include at least one selected from Mo, W, V, Nb, and Ta. The proton-type heteropolyacid is connected to the metal oxide support at least through a covalent bond, and the covalent bond is formed between the polyatoms in the proton-type heteropolyacid, the terminal oxygen in the proton-type heteropolyacid, and the metal atom in the metal oxide support.

3. The catalyst according to claim 1, characterized in that: The metal oxide carrier is a hollow structure.

4. The catalyst according to claim 3, characterized in that: The hollow structure has a single hollow chamber or a cavity combination formed by a plurality of hollow chambers gathered in a connected state or a partially connected state.

5. The catalyst according to claim 4, characterized in that: The average diameter of the hollow chamber or the cavity combination is 1-90 nm; or, the ratio of the average diameter of the hollow chamber or the cavity combination to the average particle size of the catalyst is 0.3-0.9:

1.

6. The catalyst according to claim 1, characterized in that: The catalyst comprises a hollow spherical porous alumina carrier formed by self-assembly of two-dimensional nanosheets, and the proton-type heteropolyacid is dispersed in the skeleton, inside the pores and on the surface of the porous alumina carrier in a single-molecule state; and / or the proton-type heteropolyacid is distributed in the skeleton, inside the pores and on the surface of the metal oxide carrier in a single-molecule state.

7. The catalyst according to claim 1, characterized in that: The proton-type heteropolyacid comprises a combination of one or more selected from phosphomolybdic acid, phosphotungstic acid, silicotungstic acid, silicomolybdic acid, phosphovanadium heteropolyacid, phosphoniobic acid, phosphotantalum heteropolyacid, ferromolybdenum heteropolyacid, ferrotungsten heteropolyacid, ferrovanadium heteropolyacid, cobaltmolybdenum heteropolyacid, cobalttungsten heteropolyacid, and cobaltvanadium heteropolyacid; and / or, in terms of mass percentage, the mass content of the proton-type heteropolyacid in the catalyst is 1%-68%.

8. The catalyst according to claim 7, characterized in that: In terms of mass percentage, the mass content of the proton-type heteropoly acid in the catalyst is 7%-45%.

9. The catalyst according to claim 8, characterized in that: In terms of mass percentage, the mass content of the proton-type heteropoly acid in the catalyst is 7%-25%.

10. The catalyst according to claim 1, characterized in that: The catalyst has an average pore diameter of 2-30 nm, an average pore volume of 0.4-1.5 cc / g, and an average density of 0.5-4.0 g / cm 3 and / or, the average particle size of the catalyst is 10-350 nm, and the specific surface area of ​​the catalyst is greater than or equal to 200 m 2 / g.

11. The catalyst according to claim 10, characterized in that: The specific surface area of ​​the catalyst is less than or equal to 1000 m 2 / g, and the average particle size of the catalyst is 80-250nm.

12. The catalyst according to claim 11, characterized in that: The specific surface area of ​​the catalyst is 200-800m 2 / g.

13. The catalyst according to claim 1, characterized in that: The metal oxide carrier includes a zinc oxide carrier, a magnesium oxide carrier, a copper oxide carrier, an aluminum oxide carrier or a titanium oxide carrier.

14. The catalyst according to claim 1, characterized in that: The catalyst is prepared by a preparation method that meets the following conditions: (a) using a metal oxide precursor as a raw material, wherein the metal oxide precursor refers to a substance that can be converted into a metal oxide through one or more conversion treatments, wherein the conversion treatment at least includes a treatment for producing a chemical reaction; (b) carrying out the one or more conversion treatments in the presence of the protic heteropolyacid and water.

15. The catalyst according to claim 14, characterized in that: The precursor of the metal oxide is a compound containing a metal and an organic group selected from acidic, alkaline or neutral compounds.

16. The catalyst according to claim 15, characterized in that: The compound containing metal and organic group is selected from C1-C12 metal alkoxide, C1-C12 hydrocarbon metal, metal organic complex or complex.

17. The catalyst according to claim 14, characterized in that: The metal oxide precursor is a combination of one or more selected from aluminum alcohol compounds, magnesium alcohol compounds, copper alcohol compounds, zinc alcohol compounds, titanium alcohol compounds, hydrocarbyl aluminum compounds, hydrocarbyl titanium compounds, hydrocarbyl zinc compounds, organic aluminates, organic titanates and organic zincates.

18. The catalyst according to claim 14, characterized in that: The metal oxide precursor is a combination of one or more selected from trimethylaluminum, triethylaluminum, triisobutylaluminum, diethylaluminum chloride, aluminum isopropoxide, aluminum n-butoxide, aluminum acetate, aluminum propionate, titanium acetylacetonate, tetraethyl titanate, tetraisopropyl titanate, tetrabutyl titanate and zinc acetylacetonate.

19. The catalyst according to claim 14, characterized in that: The metal oxide precursor is a substance that can be converted into the metal oxide support having a three-dimensional porous structure through sequential gelation treatment and calcination treatment.

20. The catalyst according to claim 14, characterized in that: The preparation method of the catalyst also meets the following conditions: (c) The conversion treatment includes a gelation treatment, and the gelation treatment is performed in the simultaneous presence of water, an organic solvent, and a surfactant.

21. A method for preparing the catalyst according to any one of claims 1 to 20, characterized in that: The preparation method comprises: Gelation treatment: mixing and reacting the proton type heteropoly acid and the precursor of the metal oxide in the presence of water, an organic solvent and a surfactant, and inducing the solvent evaporation to form a gel, wherein: the temperature of the mixing reaction is controlled to be 20-50° C., and the reaction time is controlled to be not less than 12 hours; Calcination treatment: the gel is dried and then calcined to obtain the catalyst.

22. The method for preparing a catalyst according to claim 21, characterized in that: The feed mass ratio of the water to the metal oxide precursor is 0.001-15:1; and / or the feed volume ratio of the water to the organic solvent is 0.001-5:

1.

23. The method for preparing a catalyst according to claim 22, characterized in that: The feed mass ratio of the water to the metal oxide precursor is 0.01-10:1; and / or the feed volume ratio of the water to the organic solvent is 0.01-2:

1.

24. The method for preparing a catalyst according to claim 23, characterized in that: The feed mass ratio of the water to the metal oxide precursor is 0.1-5:1; and / or the feed volume ratio of the water to the organic solvent is 0.005-1:

1.

25. The method for preparing a catalyst according to claim 21, characterized in that: The surfactant is a block copolymer nonionic surfactant and / or an ionic surfactant, the block copolymer nonionic surfactant includes a combination of one or more selected from nonionic surfactant P123, nonionic surfactant F127, and nonionic surfactant F108, the ionic surfactant includes a combination of one or more selected from hexadecyltrimethylammonium bromide, sodium oleate, sodium dodecylbenzenesulfonate, and sodium stearate, the feed mass ratio of the surfactant to the proton type heteropolyacid is 3 to 30:1; and / or the organic solvent is a polar organic solvent, and the feed mass ratio of the proton type heteropolyacid to the organic solvent is 1:80 to 1000.

26. The method for preparing a catalyst according to claim 21, characterized in that: The organic solvent is a combination of one or more selected from methanol, ethanol, isopropanol, acetone, tetrahydrofuran, and N,N-dimethylformamide.

27. The method for preparing a catalyst according to claim 21, characterized in that: The time of the mixed reaction is controlled to be 12-15h, 15-18h, 18-21h, 21-24h, 24-27h, 27-30h or 30-48h.

28. The method for preparing a catalyst according to claim 21, characterized in that: The solvent evaporation induction is controlled to be carried out at a temperature of 40 to 120° C. and a time of 1 to 72 hours.

29. The method for preparing the catalyst according to claim 28, characterized in that: The solvent evaporation induction is controlled to be carried out at a temperature of 60-75° C. for a time of 10 to 60 hours.

30. The method for preparing the catalyst according to claim 21, characterized in that: The calcination is performed at 200-700° C.; and / or, the calcination is performed in a muffle furnace, the calcination time is controlled to be 1-6 hours, and the heating rate is controlled to be 1-30° C. / min; and / or, the calcination is performed in an aerobic environment, the aerobic environment includes an air atmosphere or a pure oxygen atmosphere, and the pure oxygen atmosphere is formed by introducing pure oxygen gas with a purity greater than 99%.

31. A catalyst composition, characterized in that: The catalyst composition comprises the catalyst according to any one of claims 1 to 20 and at least one other catalyst different from the catalyst, wherein the mass content of the catalyst exceeds 50%.

32. Use of the catalyst according to any one of claims 1 to 20, or the catalyst prepared by the method for preparing the catalyst according to any one of claims 21 to 30, or the catalyst composition according to claim 31 in the following reactions: oxidation reaction of aromatic hydrocarbons, alcohols or aldehydes, esterification reaction of olefins with acids or esterification reaction of alcohols with acids, epoxidation reaction of olefins, alkylation reaction of aromatic compounds, isomerization reaction, dehydration reaction of alcohols, etherification reaction, hydration reaction of olefins.

33. A catalyst, characterized in that: The catalyst includes a metal oxide support having a three-dimensional porous structure, a heteropoly acid dispersed in a single molecule state and connected to the metal oxide support, and an active metal component dispersed in a single atom state and connected to one or both of the heteropoly acid and the metal oxide support, wherein the heteropoly acid is a proton-type heteropoly acid capable of providing hydrogen ions.

34. The catalyst according to claim 33, characterized in that: The active metal component is connected to the proton type heteropoly acid through a chemical bond, wherein the chemical bond includes a coordination bond, and the active metal component is also selectively adsorbed on the metal oxide carrier.

35. The catalyst according to claim 33, characterized in that: The active metal component is a combination of one or more selected from transition metals; and / or, in terms of mass percentage, the mass content of the active metal component in the catalyst is 0.01%-15%.

36. The catalyst according to claim 35, characterized in that: The active metal component is a combination of one or more selected from Group IB-IIB and Group VB-VIIIB.

37. The catalyst according to claim 33, characterized in that: The active metal component is a combination of one or more selected from Pd, Pt, Ru, Au, Ag, Rh, Ni, Cu, Fe and Co; and / or, in terms of mass percentage, the mass content of the active metal component in the catalyst is 0.04%-15%.

38. The catalyst according to claim 33, characterized in that: The catalyst is prepared by a preparation method that meets the following conditions: (a) using a metal oxide precursor and an active metal precursor as raw materials, respectively, wherein the metal oxide precursor and the active metal precursor refer to substances that can be converted into metal oxides or active metal components through one or more conversion treatments, and the conversion treatment at least includes a treatment that produces a chemical reaction; (b) carrying out the one or more conversion treatments in the presence of the protic heteropolyacid and water.

39. The catalyst according to claim 38, characterized in that: The active metal precursor is a salt of an active metal component and / or an acid of an active metal component. The salt of the active metal component includes a combination of one or more selected from metal nitrates, metal sulfates, metal halides, metal acetylacetonate complexes, and metal sulfides. The acid of the active metal component includes a halogenated metal acid.

40. The catalyst according to claim 39, characterized in that: The active metal precursor is a combination of one or more selected from palladium chloride, palladium nitrate, platinum acetylacetonate, gold chloride, silver nitrate, ruthenium chloride, ruthenium nitrate, rhodium chloride, rhodium nitrate, cobalt nitrate, nickel nitrate, ferric chloride, ferric sulfate, copper nitrate, copper sulfate, chloroplatinic acid, chloropalladic acid, chloroauric acid, and rhodium acetylacetonate.

41. A method for preparing the catalyst according to any one of claims 33 to 40, characterized in that: The preparation method comprises: Gelation treatment: mixing and reacting the proton type heteropoly acid and the precursor of the metal oxide in the presence of water, an organic solvent and a surfactant, and inducing the solvent evaporation to form a gel, wherein: the temperature of the mixing reaction is controlled to be 20-50° C., and the reaction time is controlled to be not less than 12 hours; Calcination treatment: drying the gel, calcining it, and performing a reduction treatment in the presence of a reducing agent to obtain the catalyst; The preparation method further includes the step of adding an active metal precursor before the mixing reaction, or the step of coating with a solution containing the active metal precursor after the calcination and before the reduction treatment, wherein the coating includes spraying, brushing, rolling, dipping or scraping.

42. The method for preparing the catalyst according to claim 41, characterized in that: When the preparation method uses a solution containing the active metal precursor for impregnation or spraying after the calcination and before the reduction treatment, the active metal precursor and the solid obtained by the calcination are dispersed in a solvent respectively, mixed and stirred, and separated to obtain a solid loaded with the active metal precursor, and then the reduction treatment is carried out.

43. The method for preparing the catalyst according to claim 41 or 42, characterized in that: The reduction treatment includes: performing a first calcination in an oxygen environment and then performing a second calcination in a reducing atmosphere.

44. The method for preparing the catalyst according to claim 43, characterized in that: The calcination temperature of the first calcination is 200-400°C, and the calcination temperature of the second calcination is 150-300°C.

45. The method for preparing the catalyst according to claim 44, characterized in that: The roasting temperature of the second roasting is lower than the roasting temperature of the first roasting; and / or, in the reduction treatment, the aerobic environment includes an air atmosphere or a pure oxygen atmosphere, the pure oxygen atmosphere is formed by introducing pure oxygen gas with a purity greater than 99%, and the reducing atmosphere includes a hydrogen atmosphere.

46. ​​A catalyst composition, characterized in that: The catalyst composition comprises the catalyst according to any one of claims 33 to 40 and at least one other catalyst different from the catalyst, wherein the mass content of the catalyst exceeds 50%.

47. Use of the catalyst according to any one of claims 33 to 40, or the catalyst prepared by the method for preparing the catalyst according to any one of claims 41 to 45, or the catalyst composition according to claim 46 in the following reactions: oxidation reaction of aromatic hydrocarbons, alcohols or aldehydes, esterification reaction of olefins with acids or esterification reaction of alcohols with acids, epoxidation reaction of olefins, alkylation reaction of aromatic compounds, isomerization reaction, dehydration reaction of alcohols, etherification reaction, hydration reaction of olefins, aldol condensation reaction, hydrogenation reaction, amination reaction of alcohols, ketones or olefins.

48. The use according to claim 32 or 47, characterized in that: The oxidation reaction comprises: using aromatic hydrocarbons, alcohols or aldehydes as starting materials, causing them to undergo oxidation reaction in the presence of the catalyst or the catalyst composition and an oxidant to generate corresponding acids; wherein the oxidant is oxygen, and the oxidant is provided by introducing more than 99% pure oxygen gas or air into the reaction system; and in terms of mass percentage, the added amount of the catalyst or the catalyst composition is 0.01%-3% of the added amount of the starting materials.

49. The use according to claim 32 or 47, characterized in that: The esterification reaction comprises: allowing an alcohol or an olefin to undergo an esterification reaction with an acid in the presence of the catalyst or the catalyst composition to generate an ester; wherein the alcohol comprises C 1-20 Hydrocarbyl alcohol, the acid comprising C 1-20 Hydrocarbyl carboxylic acid and / or C 1-20 Hydroxyloxy C 1-20 Hydrocarbyl carboxylic acid, the olefin comprises C 3-20 Cycloolefin; in terms of mass percentage, the added amount of the catalyst or the catalyst composition is 0.01%-3% of the added amount of the alcohol and the acid.

50. The use according to claim 49, characterized in that: The esterification reaction includes: the esterification reaction of 2-methylbutyric acid with methanol, ethanol, isopropanol, n-butanol or n-hexanol; or, the esterification reaction includes: the esterification reaction of salicylic acid with n-hexanol, n-pentanol, benzyl alcohol, leaf alcohol, cyclohexanol, isooctyl alcohol or isophorol; or, the esterification reaction includes: the esterification reaction of allyl alcohol with acetic acid, hexanoic acid, heptanoic acid, phenylpropionic acid, phenoxyacetic acid or cyclohexyloxyacetic acid; or, the esterification reaction includes: the esterification reaction of acetic acid with o-tert-butyl cyclohexanol, p-tert-butyl cyclohexanol, α-phenylethanol or β-phenylethanol; or, the esterification reaction includes: the esterification reaction of dicyclopentadiene with acetic acid, propionic acid, n-butyric acid or isobutyric acid.

51. The use according to claim 32 or 47, characterized in that: The olefin epoxidation reaction comprises: 3-20 In the presence of an oxidant and the catalyst or the catalyst composition, an olefin undergoes an epoxidation reaction in a solvent to generate a corresponding epoxide; wherein the oxidant comprises hydrogen peroxide, and the amount of hydrogen peroxide added in the hydrogen peroxide is, by weight percentage, 3-20 5%-50% of the amount of olefins added; in terms of mass percentage, the amount of the catalyst or the catalyst composition added is 3-20 The amount of olefin added is 0.1%-5%.

52. The use according to claim 51, characterized in that: The C 3-20 The olefins include α-pinene and / or limonene.

53. The use according to claim 32 or 47, characterized in that: The alkylation reaction of the aromatic compound comprises reacting an olefin with a C 1-10 Alkyl-substituted phenol, or an alkylation reaction of an alcohol with a substituted or unsubstituted benzene in the presence of the catalyst or the catalyst composition; wherein the olefin is C 2-10 Olefins, the C 1-10 The alkyl-substituted phenol is a phenol substituted by one of methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl and neopentyl, and the substitution position is meta-position. The alcohol is C 1-6 Alkyl alcohol, the substituted or unsubstituted benzene is selected from benzene or C 1-6 Alkyl substituted benzene.

54. The use according to claim 32 or 47, characterized in that: The isomerization reaction comprises: isomerizing o-cresol in the presence of the catalyst or the catalyst composition to prepare m-cresol and p-cresol, or hydroisomerizing 2-pentylcyclopentanone to prepare 2-pentylcyclopentenone.

55. The use according to claim 32 or 47, characterized in that: The dehydration reaction of the alcohol comprises: under vacuum conditions, in the presence of the catalyst or the catalyst composition, dehydrating 2-(1-hydroxypentyl)-cyclopentanone to prepare 2-pentylidenecyclopentanone, or dehydrating hydroxycyclopentadecalactone to prepare habanolide; in terms of mass percentage, the added amount of the catalyst or the catalyst composition is 0.01%-3% of the added amount of the 2-(1-hydroxypentyl)-cyclopentanone or the hydroxycyclopentadecalactone.

56. The use according to claim 32 or 47, characterized in that: The etherification reaction comprises: in the presence of the catalyst or the catalyst composition, self-etherifying 2-(3-hydroxypropyl)cyclododecanone to prepare trideca-oxabicyclo[10.4.0]hexadecene; the addition amount of the catalyst or the catalyst composition is 0.01wt.%-2.0wt.% of the addition amount of the 2-(3-hydroxypropyl)cyclododecanone.

57. The use according to claim 32 or 47, characterized in that: The hydration reaction of olefins comprises: in the presence of the catalyst or the catalyst composition, 2-20 The olefin reacts with water to produce the corresponding alcohol; wherein the C 2-20 The olefin is ethylene, propylene, butene, pentene, hexene, cyclopropene, cyclobutene, cyclopentene or cyclohexene.

58. The use according to claim 47, characterized in that: The hydrogenation reaction comprises: in the presence of the catalyst or the catalyst composition, reacting a substituted or unsubstituted phenol with hydrogen to produce a corresponding substituted or unsubstituted cyclohexanol, or reacting cyclopentylbutyrolactone and alcohol with hydrogen to produce a corresponding substituted or unsubstituted cyclohexylpropionate, or hydrogenating rose oxide to produce phenylpentyl alcohol, or hydrogenating harpa lactone to produce cyclopentadecanolide; wherein the substituted or unsubstituted phenol comprises C 1-6 Alkyl-substituted phenol, the alcohol being C 1-6 Alkyl alcohol.

59. The use according to claim 47, characterized in that: The amination reaction comprises: in the presence of the catalyst or the catalyst composition, alcohol, ketone or olefin are mixed and reacted in the presence of ammonia to generate the corresponding amine; the alcohol is C 1-10 Hydrocarbyl alcohol, the ketone is C 3-10 Hydrocarbyl ketone, the olefin is C 2-20 Olefins.

60. The use according to claim 47, characterized in that: The aldol condensation reaction comprises: in the presence of the catalyst or the catalyst composition, cyclopentanone and n-valeraldehyde undergo an aldol condensation reaction to generate 2-pentylidenecyclopentanone.

Citation Information

Cited By

  • Method for preparing habanolide and intermediate thereof

    WO2026036662A1