3DP sand mold printing cast steel coating and preparation method thereof
Through the preparation of 3DP sand-printed cast steel coatings, high-aluminum powder, concave-convex rod powder, bentonite and potassium feldspar powder are used to solve the problem of sand sticking in casting production, improve the anti-shrink and anti-sand properties of the coating, and realize the The finish and high temperature crack resistance of the casting surface.
Patent Information
- Application Number
- CN202411228868.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-22
AI Technical Summary
Existing casting coatings have sand bonding defects in casting production, which affects the quality and production efficiency of castings, and is difficult to effectively prevent sand bonding.
The 3DP sand-type printed cast steel coating is used to contain high-aluminum powder, concave and convex rod powder, bentonite, potassium feldspar powder, sucrose and potassium oxide and other raw materials. It is prepared by hydrothermal treatment and stirring to form a coating with anti-sticking and easy-to-peel properties.
It significantly improves the anti-shrinking ability and anti-sanding properties of the paint, reduces costs, realizes the smoothness and high-temperature crack resistance of the casting surface, and reduces the phenomenon of sand sticking.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of coatings, and in particular to a 3DP sand mold printing cast steel coating and a preparation method thereof. Background Art
[0002] 3DP is a type of additive manufacturing (AM) technology, first developed by Emanul Sachs and others at the Massachusetts Institute of Technology in 1898, and was granted a U.S. patent in 1993. Since then, printing equipment, molding materials, system software, etc. related to 3DP technology have gradually gained attention and developed rapidly. Due to the development of high-precision equipment and the expansion of molding materials, 3DP has been applied to many fields such as biology, medicine, and casting.
[0003] The working principle of 3DP printing parts is: first, the powder roller evenly spreads the powder provided by the powder feeding cylinder on the printing platform of the working cylinder, and then the binder is transported to the printer nozzle by pressurization. Under the control of the computer on the printer, the nozzle selectively sprays the binder on the powder plane according to the molding data of the current section to complete the bonding of the powder; after a layer of powder bonding is completed, the working cylinder printing platform drops a preset printing powder layer thickness, the powder feeding cylinder rises again to provide powder, and the powder roller spreads the powder to start a new layer of bonding; this process is repeated layer by layer to eventually complete the molding of the part.
[0004] With the advancement of science and technology and the improvement of human's requirements for the use of tools, the quality requirements for castings are getting higher and higher. The quality of molding materials directly affects the quality of castings. About 70% of the total cost of casting production and more than half of the quality problems are related to molding materials and their applications. Among the castings made of various molding materials, the most common and widely used is molding sand. In my country or worldwide, castings produced using sand molds account for more than 80% of castings produced using various casting molds. In the sand casting process, the most common casting defect is sand sticking. The mechanism of sand sticking has not yet been fully understood, but the more mature and recognized sand sticking mechanisms are mainly mechanical sand sticking and chemical sand sticking. Mechanical sand sticking is a mechanical mixture of sand and metal adhered to part or surface of the casting. This is formed by the penetration of molten metal into the micropores on the surface of the casting. The difficulty of cleaning depends on the depth of metal penetration into the micropores. Chemical sand sticking is the result of a chemical reaction between metal oxides and casting materials to generate a series of low-melting point substances that firmly adhere to the surface of the casting.
[0005] In casting production, applying casting coating is a very effective technical measure to prevent sand from sticking to castings, improve the surface quality and grade of castings, reduce the labor of sand falling and cleaning of castings, and improve economic benefits.
[0006] With the commercialization, specialization and serialization of foundry coatings, it has become one of the indispensable and important molding materials in foundry production. The development trend of foundry production in the future is near-net shape and green intensive casting. The development of foundry coatings must also conform to the general development trend of foundry technology and give full play to the role of foundry coatings in casting refinement, improving casting quality, saving resources and protecting the environment. Developing new refractory coatings to improve the anti-sand sticking performance of coatings and studying light-colored coatings for castings to improve the working environment are the main issues that should be solved in the development of foundry coatings at present and for a long time to come. Summary of the invention
[0007] In order to provide a method for effectively preventing sand sticking defects from occurring in castings, the present invention provides a 3DP sand mold printing cast steel coating and a preparation method thereof.
[0008] A 3DP sand mold printing cast steel coating comprises the following raw materials, measured by weight: 200-300 parts of high aluminum powder, 80-150 parts of attapulgite powder, 10-15 parts of bentonite, 35-45 parts of co-solvent, 22-25 parts of suspending agent and 50-70 parts of water; wherein the co-solvent is a mixture of potassium feldspar powder, sucrose and potassium oxide.
[0009] In some embodiments of the present invention, the mass percentage of aluminum oxide in the high aluminum powder is not less than 85%, and the particle size is 350-400 mesh.
[0010] In some embodiments of the present invention, the mass percentage of silicate in the attapulgite powder is not less than 90%, and the particle size is 350-400 meshes.
[0011] In some embodiments of the present invention, in the co-solvent, the mass ratio of potassium feldspar powder to sucrose and potassium oxide is 100:17.1-68.4:56-67.2.
[0012] Furthermore, in the co-solvent, the mass ratio of potassium feldspar powder to sucrose and potassium oxide is 100:34.2-51.3:56-67.2.
[0013] The presence of sucrose can promote the thermal decomposition of potassium feldspar by calcium oxide and form tobermorite. An appropriate amount of sucrose will also affect the crystal structure of tobermorite: an appropriate amount of sucrose will cause the surface structure of tobermorite to change from tightly crossed needle-like crystals to loose layered crystals, which allows the resulting coating to be infiltrated into the mold powder particles as a needle-like structure, and to form a protective ceramic layer between the metal and the mold as a layered crystal, while achieving the characteristics of anti-sand sticking and easy sintering peeling.
[0014] However, excessive sucrose will also chelate with calcium ions decomposed from calcium oxide to form a large amount of complexes, thereby inhibiting the thermal decomposition of potassium feldspar and the formation of tobermorite, and thus failing to form a good peeling layer. High-temperature liquid metal will also break through the coating layer and flow into the gaps between the mold powder particles, resulting in poor surface finish of the metal casting. Therefore, based on the use of the three components in the co-solvent, the mass ratio of potassium feldspar powder, sucrose and calcium oxide is preferably 100:34.2-51.3:56-67.2 through experiments.
[0015] In some embodiments of the present invention, the mass ratio of the bentonite to the co-solvent is 1:2.5-3.
[0016] In the present invention, bentonite is used as aggregate powder, together with high alumina powder and attapulgite powder, so that the coating has a suitable particle size ratio, which can effectively improve the performance of the coating. More importantly, bentonite can also be used as a high-temperature binder, and used together with sucrose in the cosolvent as a low-temperature binder: sucrose can ensure the strength of the coating at room temperature, and bentonite can ensure the high-temperature strength when pouring liquid metal, improve the anti-scouring ability of the coating, prevent the occurrence of cracks, and achieve a smooth surface of the casting. In order to achieve more ideal casting performance, in the present invention, the preferred weight ratio of the bentonite to the cosolvent is 1:2.5-3.
[0017] In some embodiments of the present invention, the suspending agent is at least one of carboxymethyl cellulose, sodium alginate, and polyacrylamide.
[0018] The preparation method of the above-mentioned 3DP sand mold printing cast steel coating comprises the following steps: S1: Weigh high alumina powder, attapulgite powder and bentonite and grind them in a ball mill to prepare aggregate slurry; S2: drying the aggregate slurry obtained in S1, and then grinding it to obtain aggregate powder; S3: mixing potassium feldspar powder, sucrose and potassium oxide, grinding them, hydrothermally treating them for 20-30 minutes, cooling and drying them, and grinding them to obtain a solvent; S4: After the solvent, suspending agent and water are stirred evenly, the aggregate powder obtained in S2 is added in batches and stirred evenly to obtain the 3DP sand mold printing cast steel coating.
[0019] Furthermore, the hydrothermal treatment temperature in S3 is 60-80°C.
[0020] Furthermore, the aggregate powder in S4 is fed in 3-5 batches, and the quality of each batch is the same or different.
[0021] Beneficial effects: Compared with the prior art, the 3DP sand mold printing cast steel coating of the present invention has strong anti-scouring ability, good anti-sand sticking performance, low cost, good stripping effect, and no tungsten dust phenomenon. DETAILED DESCRIPTION
[0022] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0023] Example 1 A 3DP sand mold printing cast steel coating comprises the following raw materials, measured by weight: 200 parts of high aluminum powder, 80 parts of attapulgite powder, 10 parts of bentonite, 35 parts of co-solvent, 22 parts of suspending agent and 50 parts of water.
[0024] Among them, the mass percentage of alumina in the high-aluminum powder is not less than 85%, and the particle size is 350 mesh; the mass percentage of silicate in the attapulgite powder is not less than 90%, and the particle size is 375 mesh; the co-solvent is a mixture of potassium feldspar powder, sucrose and potassium oxide in a mass ratio of 100:17.1:56.
[0025] The preparation process is as follows: S1: Weigh high alumina powder, attapulgite powder and bentonite and grind them in a ball mill to prepare aggregate slurry; S2: drying the aggregate slurry obtained in S1, and then grinding it to obtain aggregate powder; S3: mixing potassium feldspar powder, sucrose and potassium oxide, grinding them, hydrothermally treating them at 60° C. for 30 min, cooling and drying them, and grinding them to obtain a solvent; S4: After the solvent, suspending agent and water are stirred evenly, the aggregate powder obtained in S2 is added in three batches, with the same amount added each time, and the 3DP sand mold printing cast steel coating is obtained after stirring evenly.
[0026] Example 2 A 3DP sand mold printing cast steel coating comprises the following raw materials, measured by weight: 150 parts of high aluminum powder, 120 parts of attapulgite powder, 12 parts of bentonite, 40 parts of co-solvent, 23 parts of suspending agent and 60 parts of water.
[0027] Among them, the mass percentage of alumina in the high-aluminum powder is not less than 85%, and the particle size is 375 mesh; the mass percentage of silicate in the attapulgite powder is not less than 90%, and the particle size is 400 mesh; the co-solvent is a mixture obtained by mixing potassium feldspar powder with sucrose and potassium oxide in a mass ratio of 100:30:61.5.
[0028] The preparation process is as follows: S1: Weigh high alumina powder, attapulgite powder and bentonite and grind them in a ball mill to prepare aggregate slurry; S2: drying the aggregate slurry obtained in S1, and then grinding it to obtain aggregate powder; S3: mixing potassium feldspar powder, sucrose and potassium oxide, grinding them, hydrothermally treating them at 70° C. for 25 min, cooling and drying them, and grinding them to obtain a solvent; S4: After the solvent, suspending agent and water are stirred evenly, the aggregate powder obtained in S2 is added in four batches, with a different amount added each time, and the 3DP sand mold printing cast steel coating is obtained after stirring evenly.
[0029] Example 3 A 3DP sand mold printing cast steel coating comprises the following raw materials, measured by weight: 300 parts of high aluminum powder, 150 parts of attapulgite powder, 15 parts of bentonite, 45 parts of co-solvent, 25 parts of suspending agent and 70 parts of water.
[0030] Among them, the mass percentage of alumina in the high-aluminum powder is not less than 85%, and the particle size is 400 mesh; the mass percentage of silicate in the attapulgite powder is not less than 90%, and the particle size is 400 mesh; the co-solvent is a mixture obtained by mixing potassium feldspar powder with sucrose and potassium oxide in a mass ratio of 100:68.4:67.2.
[0031] The preparation process is as follows: S1: Weigh high alumina powder, attapulgite powder and bentonite and grind them in a ball mill to prepare aggregate slurry; S2: drying the aggregate slurry obtained in S1, and then grinding it to obtain aggregate powder; S3: mixing potassium feldspar powder, sucrose and potassium oxide, grinding them, hydrothermally treating them at 80° C. for 20 min, cooling and drying them, and grinding them to obtain a solvent; S4: After the solvent, suspending agent and water are stirred evenly, the aggregate powder obtained in S2 is added in five batches, with the same amount added each time, and the mixture is stirred evenly to obtain the 3DP sand mold printing cast steel coating.
[0032] Example 4 Similar to Example 2, except that the usage fraction of the bentonite is 14.3 parts.
[0033] Example 5 Similar to Example 3, except that the mass ratio of potassium feldspar powder, sucrose and potassium oxide in the solvent is 100:51.3:67.2.
[0034] Comparative Example 1 Similar to Example 5, except that no bentonite was added.
[0035] Comparative Example 2 Similar to Example 5, except that no sucrose is added to the co-solvent used.
[0036] Performance Testing According to JB / T 9226-2008 "Coatings for Sand Casting", the coatings obtained in Examples 1-5 and Comparative Examples 1-2 were tested and evaluated for suspension rate, gas emission, coating appearance and high temperature exposure crack grade after being placed for 24 hours. The test results are shown in Table 1:
[0037] Among them, although the coatings obtained in Examples 1-3 have no visible pinholes in appearance, they feel slightly rough.
[0038] As can be seen from the results in Table 1, the coating provided by the present invention has good suspension and surface finish, and has excellent crack resistance to high temperature exposure. The appearance and high temperature exposure crack resistance of the coating obtained in Examples 4-5 are better than those in Examples 1-3, which may be because the proportion of bentonite and the co-solvent containing sucrose and the proportion of sucrose contained in the co-solvent are adjusted, so that the coating has better anti-scouring ability, thereby preventing the occurrence of cracks. The results of Comparative Examples 1-2 show the opposite, that the bentonite contained in the coating and the sucrose contained in the co-solvent both have a promoting effect on the performance of the coating.
[0039] The embodiments of the present invention are described in detail above, but the contents are only preferred embodiments of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of this patent. The embodiments of the present invention are described in detail above, but the contents are only preferred embodiments of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of this patent.
Claims
1. A 3DP sand mold printing cast steel coating, It is characterized in that The invention comprises the following raw materials by weight: 200-300 parts of high alumina powder, 80-150 parts of attapulgite powder, 10-15 parts of bentonite, 35-45 parts of solvent, 22-25 parts of suspending agent and 50-70 parts of water; wherein the solvent is a mixture of potassium feldspar powder, sucrose and potassium oxide.
2. According to claim 1, the 3DP sand mold printing cast steel coating, It is characterized in that The mass percentage of aluminum oxide in the high aluminum powder is not less than 85%, and the particle size is 350-400 meshes.
3. The 3DP sand mold printing cast steel coating according to claim 1, It is characterized in that The mass percentage of silicate in the attapulgite powder is not less than 90%, and the particle size is 350-400 meshes.
4. The 3DP sand mold printing cast steel coating according to claim 1, It is characterized in that In the auxiliary solvent, the mass ratio of potassium feldspar powder to sucrose and potassium oxide is 100:17.1-68.4:56-67.
2.
5. The 3DP sand mold printing cast steel coating according to claim 4, It is characterized in that In the auxiliary solvent, the mass ratio of potassium feldspar powder to sucrose and potassium oxide is 100:34.2-51.3:56-67.
2.
6. The 3DP sand mold printing cast steel coating according to claim 1, It is characterized in that The mass ratio of the bentonite to the co-solvent is 1:2.5-3.
7. The 3DP sand mold printing cast steel coating according to claim 1, It is characterized in that The suspending agent is at least one of carboxymethyl cellulose, sodium alginate and polyacrylamide.
8. The method for preparing the 3DP sand mold printing cast steel coating according to any one of claims 1 to 7, It is characterized in that The following steps are involved: S1: Weigh high alumina powder, attapulgite powder and bentonite and grind them in a ball mill to prepare aggregate slurry; S2: drying the aggregate slurry obtained in S1, and then grinding it to obtain aggregate powder; S3: mixing potassium feldspar powder, sucrose and potassium oxide, grinding them, hydrothermally treating them for 20-30 minutes, cooling and drying them, and grinding them to obtain a solvent; S4: After the solvent, suspending agent and water are stirred evenly, the aggregate powder obtained in S2 is added in batches and stirred evenly to obtain the 3DP sand mold printing cast steel coating.
9. The method for preparing the 3DP sand mold printing cast steel coating according to claim 8, It is characterized in that The hydrothermal treatment temperature in S3 is 60-80°C.
10. The method for preparing the 3DP sand mold printing cast steel coating according to claim 8, It is characterized in that The aggregate powder in S4 is fed in 3-5 batches, and the quality of each batch is the same or different.
Citation Information
Cited By
Sand casting water-based paint and preparation method thereof
CN120325889A