Corner longitudinal crack cleaning method for X80 casting blank cast by chamfering crystallizer
By using three-step flame cleaning and mechanical slag removal methods in the casting of X80 billets in the chamfer crystallizer, the problem of longitudinal crack cleaning at the corners is solved, ensuring the comprehensive cleaning and stable quality of the corners of the casting billets, and avoiding crack problems after rolling.
Patent Information
- Application Number
- CN202411206994.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
AI Technical Summary
In the casting of X80 billets in chamfered crystallizer, longitudinal cracks at corners extending along the stretching direction of the casting bill appear, which are difficult to completely solve in traditional cutting and flame cleaning methods, resulting in crack defects that may occur after rolling, affecting product quality.
Three-step flame cleaning method is adopted: clean the upper corner, middle corner and corner sides respectively, and the cleaning depth is controlled at 3-5mm in each step. Combined with the mechanical slag removal process, ensure the corners of the casting billet are fully cleaned, and the movement rate of the flame gun is adjusted. and the angle between the two can achieve uniform heating.
It effectively avoids post-rolling cracks caused by the uncleared corners of the casting blank, ensures the integrity and quality of the corners of the casting blank, and avoids the plate roll being scrapped.
Smart Images

Figure CN118989265A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal continuous casting, and in particular to a method for cleaning longitudinal cracks at corners of an X80 ingot cast in a chamfered crystallizer. Background Art
[0002] Chamfered mold is an important equipment used in continuous casting production. During the continuous casting process, molten steel is poured into the chamfered mold from the tundish. Cooling water flows through the mold, causing the molten steel to cool and solidify rapidly on the inner wall of the mold, forming a billet shell with a certain thickness. Among them, the copper plate is a key component that allows the molten steel to cool and solidify rapidly in the mold, forming a billet with a certain shape and size. Figure 1 and Figure 2 As shown, the copper plate 100 of the chamfered crystallizer is not only provided with a water trough 110 and a cooling hole 120 on its body to ensure uniform and rapid cooling of the molten steel, but also adds an obtuse chamfer 130 on each side. The obtuse chamfer 130 can be designed to different angles according to actual working conditions, such as a 150° obtuse chamfer. This chamfer design adds a cooling surface to the cooling of the original right-angle position of the edge, which can delay the cooling of the corner of the billet, disperse the low-temperature zone, increase the temperature of the corner of the billet, avoid the 700-900°C straightening brittle temperature range, and make the growth of the billet shell at the corner more uniform, and the stress distribution more reasonable, which can effectively alleviate the stress concentration at the corner, effectively improve or eliminate the transverse cracks at the corner of the billet, and reduce the probability of defects at the corner of the billet. Therefore, for some steel varieties with high quality requirements, such as high-grade pipeline steel (such as X80 steel), the chamfered crystallizer can better meet its production needs. Nevertheless, some materials, especially those with high niobium, vanadium and titanium content, will have some longitudinal cracks at the corners extending along the stretching direction of the ingot when cast in a chamfered crystallizer. On the one hand, the ingot cast in the chamfered crystallizer has a chamfered shape at the corners, and it is not suitable to remove the longitudinal cracks at the corners by cutting away a part of the ingot; on the other hand, when using the traditional flame cleaning method, the cleaned molten steel solidifies again at the cracks, and the surface is smooth. Workers may mistakenly think that the cleaning is complete, resulting in the ingot having longitudinal crack defects at the corners after hot rolling, resulting in the scrapping of the coil.
[0003] Therefore, how to effectively clean the longitudinal cracks at the corners of the X80 ingot cast by the chamfered crystallizer has become a technical problem that needs to be solved urgently in the field of metal continuous casting technology. Summary of the invention
[0004] In view of the shortcomings of the prior art, the main purpose of the present invention is to provide a method for cleaning longitudinal cracks at the corners of X80 ingots cast by chamfering crystallizers. The method is divided into three steps, one shot for each corner, one shot for each corner, and one shot for each corner. The cleaning depth of each shot is controlled at 3-5mm, which can achieve comprehensive cleaning of the corners of the ingots cast by chamfering crystallizers, and effectively avoid the scrapping of the ingots due to post-rolling cracks caused by the incomplete cleaning of the corners.
[0005] In order to solve at least one of the above technical problems, the present invention adopts the following technical solution: According to the present invention, a method for cleaning longitudinal cracks at corners of an X80 ingot cast by a chamfered crystallizer is provided, wherein the ingot comprises a chamfer extending along its length direction, and the method comprises a preparation step, a flame cleaning step and a slag removal step, wherein the flame cleaning step comprises: cleaning on the corner: moving a flame gun above a wide surface of the ingot along the length direction of the ingot to heat an area within a predetermined width range adjacent to the wide surface of the ingot and the chamfer; cleaning in the middle of the corner: moving the flame gun along the length direction of the ingot obliquely above the chamfered surface to heat the chamfered surface; cleaning on the side of the corner: moving the flame gun on the side of a narrow surface of the ingot along the length direction of the ingot to heat an area within a predetermined height range adjacent to the narrow surface of the ingot and the chamfer; wherein the order of the cleaning on the corner, the cleaning in the middle of the corner and the cleaning on the side of the corner is adjustable.
[0006] According to an embodiment of the present invention, the preparation process includes: after confirming that the pressure of oxygen is ≥1.25MPa and the pressure of coal gas is ≥0.2MPa, igniting the flame gun.
[0007] According to one embodiment of the present invention, the cleaning depths of the corner cleaning, the corner middle cleaning and the corner side cleaning are 3-5 mm.
[0008] According to an embodiment of the present invention, in the flame cleaning process, the flame gun is controlled to move at a uniform speed along the length direction of the ingot.
[0009] According to an embodiment of the present invention, the movement speed of the flame gun is 1-1.5 m / min.
[0010] According to one embodiment of the present invention, the flame cleaning process includes: controlling the flame gun to form an angle of 30~40° with the wide surface of the ingot; controlling the flame gun to form an angle of 30~40° with the chamfered surface; controlling the flame gun to form an angle of 30~40° with the narrow surface of the ingot.
[0011] According to one embodiment of the present invention, the slag removal step comprises: using mechanical means to remove the oxidized slag on the wide surface of the ingot, the chamfered surface and the side surface of the ingot.
[0012] According to an embodiment of the present invention, the method comprises: when it is found that there is an uncleaned area during the slag removal process, performing a secondary flame cleaning process and a secondary slag removal process.
[0013] According to an embodiment of the present invention, the secondary flame cleaning process comprises: performing at least one of the corner cleaning, the corner middle cleaning and the corner side cleaning starting from the end of the ingot based on the location of the uncleaned area.
[0014] According to an embodiment of the present invention, in the secondary flame cleaning process, the angle between the flame gun and the cleaning area is greater than the angle between the flame gun and the cleaned area.
[0015] By adopting the above technical solution, the present invention has at least one of the following advantages compared with the prior art: (1) According to the method of the present invention, during the flame cleaning, cleaning is performed on the corner, in the middle of the corner and on the side of the corner of the ingot, thereby achieving comprehensive cleaning of the corner of the ingot cast by the chamfered crystallizer; (2) According to the method of the present invention, the cleaning depth is controlled to be 3-5 mm, which can eliminate the cracks deeper in the corners of the ingot, and effectively avoid the scrapping of the ingot due to the post-rolling cracks caused by the incomplete cleaning of the corners. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 Schematic diagram of the copper plate of the chamfered crystallizer; Figure 2 It is a side view of the copper plate of the chamfered crystallizer; Figure 3 Schematic diagram of the corner of a chamfered crystallizer for casting an X80 ingot according to an embodiment of the present invention.
[0018] In the accompanying drawings, 100, copper plate, 110, water tank, 120, cooling hole, 130, blunt chamfer. DETAILED DESCRIPTION
[0019] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.
[0020] It should be understood that the embodiments of the present invention shown in the exemplary embodiments are only illustrative. Although only a few embodiments are described in detail in the present invention, it is easy for those skilled in the art to appreciate that multiple modifications are feasible without actually departing from the teaching of the subject matter of the present invention. Accordingly, all such modifications should be included within the scope of the present invention. Without departing from the gist of the present invention, other replacements, modifications, changes and deletions may be made to the design, operating conditions and parameters of the following exemplary embodiments.
[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field of the present invention; the terms used in this specification are only for the purpose of describing specific embodiments and are not intended to limit the present invention. For example, the directions or positions indicated by the terms "length", "width", "up", "down", "left", "right", "front", "back", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc. are based on the directions or positions shown in the drawings, which are only for the convenience of description and should not be understood as limitations on the present technical solution.
[0022] It should be noted that all expressions using "first" and "second" in the embodiments of the present invention are for distinguishing two non-identical entities with the same name or non-identical parameters. It can be seen that "first" and "second" are only for the convenience of expression and should not be understood as limitations on the embodiments of the present invention. The subsequent embodiments will not explain this one by one.
[0023] X80 steel is a high-strength pipeline steel. It has high strength, with a minimum yield strength of up to 552MPa; it has high toughness, good weldability, and certain resistance to hydrogen-induced cracking (HIC) and sulfide stress corrosion cracking (SSC), and is widely used in the fields of oil and natural gas pipelines. In order to improve the comprehensive performance of X80 oil pipeline steel, its composition usually contains: 0.04%~0.06% niobium (Nb), which can improve the strength and toughness of steel through grain refinement and precipitation strengthening; 0.04%~0.08% vanadium (V), which can play a role in grain refinement and precipitation strengthening; and 0.01%~0.02% titanium (Ti), which is used to fix nitrogen in steel to prevent nitrogen from having adverse effects on the performance of steel.
[0024] According to an embodiment of the present invention, a method for cleaning longitudinal cracks at corners of X80 ingots cast in a chamfered crystallizer is provided, which generally includes a preparation step, a flame cleaning step and a slag removal step.
[0025] The preparation process is to prepare for the subsequent flame cleaning process. In an embodiment of the present invention, a flame gun can be used to perform the subsequent flame cleaning process. The flame gun can connect the combustible gas (such as acetylene, coal gas) and the combustion-supporting gas (such as oxygen), mix them inside the gun body, and then spray the flame from the nozzle. The preparation work for using the flame gun may include: checking whether the various parts of the flame gun are intact and the connections are tight to ensure that there is no gas leakage; preparing the combustible gas and the combustion-supporting gas, and ensuring that the gas supply is stable and meets safety standards; and placing the ingot to be cleaned in a suitable working position for easy operation. In an embodiment of the present invention, coal gas is used as the combustible gas and oxygen is used as the combustion-supporting gas. In the preparation process, it is necessary to confirm that the oxygen pressure is ≥1.25MPa and the coal gas pressure is ≥0.2MPa, and then ignite the flame gun.
[0026] For example Figure 3 The flame cleaning process of the corner of the X80 ingot cast by the chamfered crystallizer shown mainly includes: cleaning on the corner, moving the flame gun along the length direction of the ingot above the wide surface of the ingot to heat the area within a predetermined width range adjacent to the chamfer of the wide surface of the ingot; cleaning in the middle of the corner, moving the flame gun along the length direction of the ingot above the chamfer slope to heat the chamfer slope; cleaning on the side of the corner, moving the flame gun along the length direction of the ingot on the side of the narrow surface of the ingot to heat the area within a predetermined height range adjacent to the chamfer of the narrow surface of the ingot. Therefore, during flame cleaning, cleaning is performed on the corner, in the middle of the corner and on the side of the corner of the ingot, respectively, so as to achieve comprehensive cleaning of the corner of the ingot cast by the chamfered crystallizer. Among them, the predetermined width / predetermined height of the cleaning on the corner and the cleaning on the side of the corner can be 30~60mm, preferably 40mm. According to the method of the present invention, the order of cleaning on the corner, cleaning in the middle of the corner and cleaning on the side of the corner can be arbitrarily changed. For example, in one embodiment, the upper corner portion can be cleaned by pulling it from the end portion along the length direction of the ingot in the first step, and the middle corner portion can be cleaned by pulling it from the end portion along the length direction of the ingot in the second step; and finally, the diagonal side portion can be cleaned by pulling it from the end portion along the length direction of the ingot. In another embodiment, the cleaning can be carried out in the order of the corner side, the middle corner, and the upper corner. In another embodiment, the cleaning can be carried out in the order of the middle corner, the upper corner, and the side corner.
[0027] The cracks at the corners of the ingot are usually related to the casting process and the material properties. The use of a chamfered crystallizer can only suppress the generation of corner cracks to a certain extent, and cannot be completely avoided. Different materials have different crack propagation characteristics, and the crack depths generated under the same process will also be different. Generally speaking, the depth of flame cleaning should be sufficient to remove the crack tip to ensure the structural integrity after subsequent treatment and prevent the crack from continuing to expand; but too much depth not only consumes too much energy, but also has an adverse effect on the performance of the ingot, such as long-term high-temperature heating makes the grain size and organizational morphology near the corners of the ingot obviously different from other parts of the ingot, destroying the uniformity of the organization and affecting the comprehensive performance of the ingot. In an embodiment of the present invention, for casting X80 ingots with chamfered crystallizers, the preferred cleaning depth is 3~5mm. During the cleaning process, it is necessary to control the flame gun to move at a uniform speed along the length direction of the ingot to achieve uniform heating of each part and avoid uneven cleaning surfaces. In an embodiment of the present invention, it is preferred to control the movement rate of the flame gun to be 1~1.5m / min. During the cleaning process, the flame gun is controlled to form an angle of 30-40° with the wide surface of the ingot; the flame gun is controlled to form an angle of 30-40° with the chamfered surface; and the flame gun is controlled to form an angle of 30-40° with the narrow surface of the ingot. The cleaning depth can be controlled by adjusting the moving speed of the flame gun and the angle between the flame gun and the surface to be cleaned. For example, increasing the moving speed of the flame gun and / or reducing the angle between the flame gun and the surface to be cleaned can reduce the cleaning depth; reducing the moving speed of the flame gun and / or increasing the angle between the flame gun and the surface to be cleaned can increase the cleaning depth.
[0028] The slag removal process refers to removing impurities such as slag on the surface of the corner area after the flame cleaning process. In the embodiment of the present invention, mechanical means such as a shovel or a scraper can be used to remove impurities such as slag on the wide surface, chamfered surface and side surface of the ingot.
[0029] Preferably, when an uncleaned part is found during the slag removal process, i.e., a missing gun is found, a secondary flame cleaning process and a secondary slag removal process can be performed. The secondary flame cleaning process is similar to the above-mentioned flame cleaning process, except that at least one of corner cleaning, corner cleaning and corner side cleaning is performed based on the location of the uncleaned part, and all of them do not need to be performed. For example, if the uncleaned part is found to be located in the corner area, only the corner cleaning is performed. It should be noted that no matter which area of the longitudinal direction of the billet the uncleaned part is located, it is necessary to start the cleaning from the end of the billet. In the secondary flame cleaning process, the angle between the flame gun and the cleaning part (i.e., the uncleaned part of the missing gun after the first cleaning) is greater than the angle between the flame gun and the cleaned part, so that the cleaning depth of the cleaned part is slightly lower than that of the uncleaned part, ensuring that the cleaning depth of the entire billet is consistent. After the secondary flame cleaning process is completed, the secondary slag removal process is performed with reference to the above-mentioned slag removal process. If an uncleaned part is still found during the secondary slag removal, the third flame cleaning process and the third slag removal process can be continued, and so on.
[0030] The following is a specific embodiment of the method for cleaning longitudinal cracks at corners of X80 ingots cast in a chamfered crystallizer according to the present invention and its specific process parameters.
[0031] Example 1 The method for cleaning longitudinal cracks at corners disclosed in this embodiment is used to clean corner cracks of X80 ingots cast in a chamfered crystallizer with a thickness of 230 mm. The crystallizer copper plate has a 150° chamfer and the ingot chamfer width is 60 mm. The specific process is as follows: Step S1: Preparation process, after confirming that the oxygen pressure is ≥1.25MPa and the gas pressure is ≥0.2MPa, the flame gun is ignited.
[0032] Step S2: Flame cleaning process: Step S21: cleaning the corners, moving the flame gun at a rate of 1.0 m / min along the length direction of the ingot above the wide surface of the ingot, with the flame gun and the wide surface of the ingot forming an angle of 30°, so as to heat the area within a range of 40 mm adjacent to the wide surface of the ingot and the chamfer; Step S22: cleaning the corners, moving a flame gun at a rate of 1.0 m / min along the length direction of the ingot above the chamfered surface, with the flame gun and the chamfered surface forming an angle of 40° to heat the chamfered surface; Step S23: cleaning the corner side, moving the flame gun at a speed of 1.0 m / min along the length direction of the billet at the side of the narrow surface of the billet, with the flame gun forming an angle of 30° with the narrow surface of the billet to heat the area within 40 mm adjacent to the narrow surface of the billet and the chamfer.
[0033] Step S3: Slag removal process, using a shovel to remove the oxidized slag on the wide surface, chamfered surface and side surface of the ingot.
[0034] After cleaning, ultrasonic testing showed that the X80 ingot had no cracks at the corners and had a smooth transition.
[0035] Example 2 The method for cleaning longitudinal cracks at corners disclosed in this embodiment is used to clean corner cracks of X80 ingots cast in a chamfered crystallizer with a thickness of 230 mm. The crystallizer copper plate has a 150° chamfer and the ingot chamfer width is 60 mm. The specific process is as follows: Step S1: Preparation process, after confirming that the oxygen pressure is ≥1.25MPa and the gas pressure is ≥0.2MPa, the flame gun is ignited.
[0036] Step S2: Flame cleaning process: Step S21: cleaning the corner side, moving the flame gun at a speed of 1.3 m / min along the length direction of the billet at the side of the narrow side of the billet, with the flame gun and the narrow side of the billet forming an angle of 35° to heat the area within 30 mm adjacent to the narrow side of the billet and the chamfer; Step S22: cleaning the corners, moving a flame gun at a rate of 1.0 m / min along the length direction of the ingot above the chamfered surface, with the flame gun and the chamfered surface forming an angle of 40° to heat the chamfered surface; Step S23: cleaning the corners, moving the flame gun at a rate of 1.2 m / min along the length direction of the ingot above the wide surface of the ingot, with the flame gun forming an angle of 40° with the wide surface of the ingot, to heat the area within 30 mm adjacent to the wide surface of the ingot and the chamfer.
[0037] Step S3: Slag removal process, using a shovel to remove the oxidized slag on the wide surface, chamfered surface and side surface of the ingot.
[0038] After cleaning, ultrasonic testing showed that the X80 ingot had no cracks at the corners and had a smooth transition.
[0039] Example 3 The method for cleaning longitudinal cracks at corners disclosed in this embodiment is used to clean corner cracks of X80 ingots cast in a chamfered crystallizer with a thickness of 230 mm. The crystallizer copper plate has a 150° chamfer and the ingot chamfer width is 60 mm. The specific process is as follows: Step S1: Preparation process, after confirming that the oxygen pressure is ≥1.25MPa and the gas pressure is ≥0.2MPa, the flame gun is ignited.
[0040] Step S2: Flame cleaning process: Step S21: cleaning the corner side, moving the flame gun at a speed of 1.5 m / min along the length direction of the billet at the side of the narrow side of the billet, with the flame gun and the narrow side of the billet at an angle of 40° to heat the area within 50 mm adjacent to the narrow side of the billet and the chamfer; Step S22: cleaning the corners, moving the flame gun at a rate of 1.2 m / min along the length direction of the ingot above the wide surface of the ingot, with the flame gun and the wide surface of the ingot forming an angle of 35°, so as to heat the area within 60 mm of the wide surface of the ingot adjacent to the chamfer; Step S23: cleaning the corners, moving the flame gun at a speed of 1.5 m / min along the length direction of the ingot at an angle of 30° between the flame gun and the chamfered surface to heat the chamfered surface.
[0041] Step S3: Slag removal process, using a shovel to remove the oxidized slag on the wide surface, chamfered surface and side surface of the ingot.
[0042] After cleaning, ultrasonic testing showed that the X80 ingot had no cracks at the corners and had a smooth transition.
[0043] The above description is only a preferred embodiment of the present invention and is not intended to limit the scope of implementation of the present invention. If the present invention is modified or replaced by equivalents without departing from the spirit and scope of the present invention, it should be included in the protection scope of the claims of the present invention.
[0044] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention is limited to these examples; under the idea of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.
Claims
1. A method for cleaning longitudinal cracks at the corners of X80 ingots cast in a chamfered crystallizer. It is characterized in that The ingot comprises a chamfer extending along its length direction, and the method comprises a preparation step, a flame cleaning step and a slag removal step, wherein the flame cleaning step comprises: Corner cleaning: moving a flame gun above the wide surface of the ingot along the length direction of the ingot to heat the area within a predetermined width range adjacent to the chamfer on the wide surface of the ingot; Corner cleaning: moving the flame gun along the length direction of the ingot at an angle above the chamfered surface to heat the chamfered surface; Corner side cleaning: moving the flame gun along the length direction of the ingot on the side of the narrow surface of the ingot to heat the area within a predetermined height range adjacent to the chamfer of the narrow surface of the ingot; The order of the corner cleaning, the corner middle cleaning and the corner side cleaning is adjustable.
2. The method for cleaning longitudinal cracks at corners of X80 ingots cast by chamfering mold according to claim 1, It is characterized in that The preparation process comprises: After confirming that the pressure of oxygen is ≥1.25MPa and the pressure of coal gas is ≥0.2MPa, the flame gun is ignited.
3. The method according to claim 1, It is characterized in that The cleaning depths of the corner cleaning, the corner middle cleaning and the corner side cleaning are 3 to 5 mm.
4. The method for cleaning longitudinal cracks at corners of X80 ingots cast by chamfering mold according to claim 3, It is characterized in that In the flame cleaning process, the flame gun is controlled to move at a uniform speed along the length direction of the ingot.
5. The method for cleaning longitudinal cracks at corners of X80 ingots cast by chamfering mold according to claim 4, It is characterized in that The moving speed of the flame gun is 1-1.5 m / min.
6. The method for cleaning longitudinal cracks at corners of X80 ingots cast by chamfering mold according to claim 1, It is characterized in that The flame cleaning process comprises: Control the flame gun to form an angle of 30-40° with the wide surface of the ingot; Control the flame gun to form an angle of 30-40° with the chamfered surface; The flame gun is controlled to form an angle of 30-40° with the narrow surface of the ingot.
7. The method for cleaning longitudinal cracks at corners of X80 ingots cast by chamfering mold according to claim 1, It is characterized in that The slag removal process comprises: Mechanical means are used to remove slag from the wide surface of the ingot, the chamfered surface and the side surface of the ingot.
8. The method for cleaning longitudinal cracks at corners of X80 ingots cast by chamfering mold according to claim 1, It is characterized in that The method comprises: When it is found that there are uncleaned areas during the slag removal process, a secondary flame cleaning process and a secondary slag removal process are performed.
9. The method for cleaning longitudinal cracks at corners of X80 ingots cast by chamfering mold according to claim 8, It is characterized in that The secondary flame cleaning process comprises: At least one of the corner cleaning, the corner middle cleaning and the corner side cleaning is performed starting from the end of the casting strand based on the location of the uncleaned portion.
10. The method for cleaning longitudinal cracks at corners of X80 ingots cast by chamfering mold according to claim 9, It is characterized in that In the secondary flame cleaning process, the angle between the flame gun and the cleaning area is greater than the angle between the flame gun and the cleaned area.