Preparation method of cobalt-chromium-molybdenum alloy powder
Through the coupling processes of cold isostatic pressure, hot isostatic pressure, vacuum smelting and spray powdering, the problem of poor composition uniformity of cobalt chromium molybdenum materials is solved, and the mechanical properties of finished products are significantly improved.
Patent Information
- Application Number
- CN202411177391.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-22
AI Technical Summary
The composition uniformity of existing cobalt chromium molybdenum materials is poor during the preparation process, resulting in poor mechanical properties of finished products.
The coupled preparation methods of cold isostatic pressure, hot isostatic pressure, vacuum smelting and spray powder are adopted to improve the composition uniformity of cobalt chromium molybdenum alloy powder through specific process parameters optimization.
The composition uniformity of cobalt chromium molybdenum alloy powder is improved, thereby improving the mechanical properties of finished products.
Smart Images

Figure BDA0005011079140000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cobalt-chromium-molybdenum alloys, and in particular to a method for preparing cobalt-chromium-molybdenum alloy powder. Background Art
[0002] At present, cobalt, chromium and molybdenum are widely used in medical devices. Cast CoCrMo alloy has been used in dentistry for decades and is also used to manufacture artificial joints.
[0003] For example, CN110129591A discloses a method for producing CoCrMo alloy for artificial joints. The method first obtains a forging blank by vacuum induction furnace smelting and electroslag remelting. The blank is then heated to 1150°C-1250°C for insulation and then forged. During the forging process, the temperature of the blank is strictly controlled within a certain temperature range. The insulation temperature of the last fire is 1150°C, and the final forging temperature of each fire is not less than 1000°C to ensure that the CoCrMo forging blank is always in a good plastic processing state. After forging, diffusion annealing is performed at a temperature of 1000°C-1050°C.
[0004] CN214387786U discloses a forged cobalt-chromium-molybdenum alloy artificial hip joint, comprising a femoral ball head and a femoral stem, wherein one end of the femoral ball head is slidably connected to the acetabulum cup and the other end is plug-connected to the femoral stem, the femoral ball head comprises an outer spherical shell and an inner sphere, the inner sphere is matched and embedded in the outer spherical shell, an acetabulum liner that slides relative to the outer spherical shell is disposed outside the outer spherical shell, an acetabulum cup is matched and sleeved outside the acetabulum liner, and a femoral stem is plug-connected in the inner sphere; the femoral stem comprises a stem neck, a stem body, and an elastic connector arranged at the connection between the stem neck and the stem body, the stem body comprises a stem proximal portion and a stem distal portion, the stem proximal portion is provided with a plurality of wavy water-patterned grooves, and the front and rear side surfaces of the stem distal portion are provided with vertical grooves.
[0005] The existing cobalt-chromium-molybdenum material production process mainly adopts vacuum melting-atomization powder method to prepare powder, and then adopts melting, hot isostatic pressing or additive manufacturing to prepare it into a molded body. However, the cobalt-chromium-molybdenum alloy powder prepared currently still has the defect of poor composition uniformity, which leads to poor mechanical properties of the products obtained by finished material manufacturing. Summary of the invention
[0006] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for preparing cobalt-chromium-molybdenum alloy powder to solve the problem that the cobalt-chromium-molybdenum alloy powder currently prepared still has the defect of poor composition uniformity, thereby resulting in poor mechanical properties of the products obtained by finished material manufacturing.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] The present invention provides a method for preparing cobalt-chromium-molybdenum alloy powder, the preparation method comprising:
[0009] Mixing cobalt powder, chromium powder and molybdenum powder to obtain mixed powder;
[0010] The mixed powder is subjected to cold isostatic pressing, hot isostatic pressing, vacuum melting and spray powdering in sequence to obtain cobalt-chromium-molybdenum alloy powder.
[0011] The preparation method provided by the present invention realizes the preparation of cobalt-chromium-molybdenum alloy powder with uniform composition by adopting the coupling coordination of specific preparation processes such as hot isostatic pressing, vacuum melting and spray powder making, which is beneficial to the improvement of the mechanical properties of the products obtained by finished material manufacturing.
[0012] As a preferred technical solution of the present invention, the particle size of the cobalt powder is 2-10 μm.
[0013] Preferably, the particle size of the chromium powder is 2-10 μm.
[0014] Preferably, the particle size of the molybdenum powder is 2-10 μm.
[0015] As a preferred technical solution of the present invention, the mixing is carried out under an inert atmosphere.
[0016] Preferably, the mixing speed is 10-15 r / min.
[0017] Preferably, the mixing time is 12-24 hours.
[0018] As a preferred technical solution of the present invention, the mass ratio of cobalt powder, chromium powder and molybdenum powder in the mixed powder is (60-65):(25-30):(5-10).
[0019] As a preferred technical solution of the present invention, the pressure of the cold isostatic pressing is 170-250 MPa.
[0020] As a preferred technical solution of the present invention, the cold isostatic pressing time is 30-60 minutes.
[0021] As a preferred technical solution of the present invention, the temperature of the hot isostatic pressing is 1000-1150°C.
[0022] Preferably, the hot isostatic pressing pressure is 100-190 MPa.
[0023] As a preferred technical solution of the present invention, the hot isostatic pressing time is 2-7h.
[0024] As a preferred technical solution of the present invention, the absolute vacuum degree of the vacuum melting is ≤0.001Pa.
[0025] Preferably, the vacuum melting temperature is 1500-1600°C.
[0026] Preferably, the vacuum melting time is 2-2.5 hours.
[0027] As a preferred technical solution of the present invention, the operating pressure of the spray powder making is 8-15MPa.
[0028] Compared with the prior art solutions, the present invention has the following beneficial effects:
[0029] The preparation method provided by the present invention realizes the preparation of cobalt-chromium-molybdenum alloy powder with uniform composition by adopting a specific preparation process, which is beneficial to improving the performance of the cobalt-chromium-molybdenum alloy powder, thereby improving the performance of cobalt-chromium-molybdenum alloy products. DETAILED DESCRIPTION
[0030] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0031] This embodiment provides a method for preparing cobalt-chromium-molybdenum alloy powder, the preparation method comprising:
[0032] Mixing cobalt powder, chromium powder and molybdenum powder to obtain mixed powder;
[0033] The mixed powder is subjected to cold isostatic pressing, hot isostatic pressing, vacuum melting and spray powdering in sequence to obtain cobalt-chromium-molybdenum alloy powder.
[0034] Wherein, the particle size of the cobalt powder is 2-10 μm.
[0035] In the present invention, the purity of the cobalt powder used is ≥99.96%.
[0036] Wherein, the particle size of the chromium powder is 2-10 μm.
[0037] In the present invention, the purity of the chromium powder used is ≥99.96%.
[0038] Wherein, the particle size of the molybdenum powder is 2-10 μm.
[0039] In the present invention, the purity of the molybdenum powder used is ≥99.96%.
[0040] In the present invention, the particle size of the metal powder is defined as an aggregate of particles of any particle size within a limited range, or an aggregate of all particles within a certain range, exemplified by an aggregate of particles with a particle size of 2 μm, an aggregate of particles with a particle size of 4 μm, an aggregate of particles with a particle size of 6 μm, an aggregate of particles with a particle size of 8 μm, an aggregate of particles with a particle size of 10 μm, or an aggregate of all particles within a particle size range of 3-6 μm, or an aggregate of all particles within a particle size range of 5-8 μm, or an aggregate of all particles within a particle size range of 7-10 μm, etc.
[0041] Wherein, the mixing is carried out under an inert atmosphere.
[0042] In the present invention, the inert atmosphere refers to a gas that does not affect the properties of the obtained alloy, such as nitrogen, helium, argon or neon, etc., which are commonly used inert gases in the art.
[0043] The mixing speed is 10-15 r / min, for example, it can be 10 r / min, 11 r / min, 12 r / min, 13 r / min, 14 r / min or 15 r / min, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0044] The mixing time is 12-24 hours, for example, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0045] Among them, the mass ratio of cobalt powder, chromium powder and molybdenum powder in the mixed powder is (60-65):(25-30):(5-10), for example, it can be 60:25:5, 61:26:6, 62:27:7, 63:28:8, 64:29:9, 65:30:10, 60:25:10, 65:25:10 or 60:30:5, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0046] Wherein, the pressure of the cold isostatic pressing is 170-250MPa, for example, it can be 170MPa, 175MPa, 180MPa, 185MPa, 190MPa, 195MPa, 200MPa, 205MPa, 210MPa, 215MPa, 220MPa, 225MPa, 230MPa, 235MPa, 240MPa, 245MPa or 250MPa, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0047] The cold isostatic pressing time is 30-60 min, for example, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min or 60 min, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0048] Wherein, the temperature of the hot isostatic pressing is 1000-1150°C, for example, it can be 1000°C, 1010°C, 1020°C, 1030°C, 1040°C, 1050°C, 1060°C, 1070°C, 1080°C, 1090°C, 1100°C, 1110°C, 1120°C, 1130°C, 1140°C or 1150°C, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0049] The hot isostatic pressing pressure is 100-190 MPa, for example, 100 MPa, 110 MPa, 120 MPa, 130 MPa, 140 MPa, 150 MPa, 160 MPa, 170 MPa, 180 MPa or 190 MPa, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0050] The hot isostatic pressing time is 2-7 hours, for example, it can be 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours, 6 hours, 6.5 hours or 7 hours, but is not limited to the listed values. Other values not listed in this range also meet the requirements.
[0051] In the present invention, the hot isostatic pressing needs to be combined with the jacketing and degassing treatments for the intermediate powder.
[0052] The sheath treatment can be carried out according to the conventional requirements in the field of hot isostatic pressing, and the material used for the sheath is stainless steel and other materials.
[0053] The degassing treatment is to degas the assembly obtained by the sheathing treatment, illustratively, the degassing is performed at a temperature of 500-600° C. under an absolute vacuum degree of ≤0.005 Pa for 1-3 hours.
[0054] Among them, the absolute vacuum degree in the degassing treatment is ≤0.005Pa, for example, it can be 0.005Pa, 0.0045Pa, 0.004Pa, 0.0035Pa, 0.003Pa, 0.0025Pa, 0.002Pa, 0.0015Pa, 0.001Pa or 0.0001Pa, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0055] Among them, the temperature in the degassing treatment is 500-600℃, for example, it can be 500℃, 510℃, 520℃, 530℃, 540℃, 550℃, 560℃, 570℃, 580℃, 590℃ or 600℃, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0056] The degassing time is 1-3h, for example, it can be 1h, 1.2h, 1.4h, 1.6h, 1.8h, 2h, 2.2h, 2.4h, 2.6h, 2.8h or 3h, but is not limited to the listed values. Other values not listed within the range also meet the requirements.
[0057] The absolute vacuum degree of the vacuum melting is ≤0.001Pa, for example, it can be 0.001Pa, 0.0008Pa, 0.0006Pa, 0.0004Pa, 0.0002Pa or 0.0001Pa, etc., but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0058] The temperature of the vacuum melting is 1500-1600°C, for example, it can be 1500°C, 1520°C, 1540°C, 1560°C, 1580°C or 1600°C, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0059] The vacuum melting time is 2-2.5 h, for example, 2 h, 2.1 h, 2.2 h, 2.3 h, 2.4 h or 2.5 h, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0060] Among them, the operating pressure of the spray powder making is 8-15MPa, for example, it can be 8MPa, 8.5MPa, 9MPa, 9.5MPa, 10MPa, 10.5MPa, 11MPa, 11.5MPa, 12MPa, 12.5MPa, 13MPa, 13.5MPa, 14MPa, 14.5MPa or 15MPa, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0061] Furthermore, in order to illustrate the good effects that can be achieved by preparing the cobalt-chromium-molybdenum alloy powder of the present invention, actual examples are used for illustration, as follows:
[0062] Example 1
[0063] This embodiment provides a method for preparing cobalt-chromium-molybdenum alloy powder, the preparation method comprising:
[0064] Mixing cobalt powder, chromium powder and molybdenum powder to obtain mixed powder;
[0065] The mixed powder is subjected to cold isostatic pressing, hot isostatic pressing, vacuum melting and spray powdering in sequence to obtain cobalt-chromium-molybdenum alloy powder;
[0066] The particle size of the cobalt powder is 3-6 μm, and the purity is 99.96%; the particle size of the chromium powder is 4-10 μm, and the purity is 99.97%; the particle size of the molybdenum powder is 5-8 μm, and the purity is 99.96%;
[0067] The mixing is carried out under an inert atmosphere (neon); the mixing speed is 14r / min; the mixing time is 20h;
[0068] The mass ratio of cobalt powder, chromium powder and molybdenum powder in the mixed powder is 64:26:8;
[0069] The cold isostatic pressing pressure is 200 MPa; the cold isostatic pressing time is 50 min;
[0070] The temperature of the hot isostatic pressing is 1100°C; the pressure of the hot isostatic pressing is 130MPa; and the time of the hot isostatic pressing is 5h;
[0071] The absolute vacuum degree of the vacuum melting is 0.0001Pa; the temperature of the vacuum melting is 1580°C; the time of the vacuum melting is 2.2h; and the operating pressure of the spray powder making is 12MPa.
[0072] Example 2
[0073] This embodiment provides a method for preparing cobalt-chromium-molybdenum alloy powder, the preparation method comprising:
[0074] Mixing cobalt powder, chromium powder and molybdenum powder to obtain mixed powder;
[0075] The mixed powder is subjected to cold isostatic pressing, hot isostatic pressing, vacuum melting and spray powdering in sequence to obtain cobalt-chromium-molybdenum alloy powder;
[0076] The particle size of the cobalt powder is 7-10 μm, and the purity is 99.99%; the particle size of the chromium powder is 2-5 μm, and the purity is 99.97%; the particle size of the molybdenum powder is 3-8 μm, and the purity is 99.98%;
[0077] The mixing is carried out under an inert atmosphere (helium); the mixing speed is 12 r / min; the mixing time is 18 h;
[0078] The mass ratio of cobalt powder, chromium powder and molybdenum powder in the mixed powder is 62:28:7;
[0079] The cold isostatic pressing pressure is 220 MPa; the cold isostatic pressing time is 40 min;
[0080] The temperature of the hot isostatic pressing is 1050°C; the pressure of the hot isostatic pressing is 160MPa; and the time of the hot isostatic pressing is 3h;
[0081] The absolute vacuum degree of the vacuum melting is 0.0008 Pa; the temperature of the vacuum melting is 1540° C.; the time of the vacuum melting is 2.4 h; and the operating pressure of the spray powder making is 10 MPa.
[0082] Example 3
[0083] This embodiment provides a method for preparing cobalt-chromium-molybdenum alloy powder, the preparation method comprising:
[0084] Mixing cobalt powder, chromium powder and molybdenum powder to obtain mixed powder;
[0085] The mixed powder is subjected to cold isostatic pressing, hot isostatic pressing, vacuum melting and spray powdering in sequence to obtain cobalt-chromium-molybdenum alloy powder;
[0086] The particle size of the cobalt powder is 2-5 μm, and the purity is 99.99%; the particle size of the chromium powder is 8-10 μm, and the purity is 99.98%; the particle size of the molybdenum powder is 6-7 μm, and the purity is 99.97%;
[0087] The mixing is carried out under an inert atmosphere (neon); the mixing speed is 15 r / min; the mixing time is 12 h;
[0088] The mass ratio of cobalt powder, chromium powder and molybdenum powder in the mixed powder is 60:25:5;
[0089] The cold isostatic pressing pressure is 250 MPa; the cold isostatic pressing time is 30 min;
[0090] The temperature of the hot isostatic pressing is 1150°C; the pressure of the hot isostatic pressing is 100MPa; and the time of the hot isostatic pressing is 7h;
[0091] The absolute vacuum degree of the vacuum melting is 0.0002Pa; the temperature of the vacuum melting is 1500°C; the time of the vacuum melting is 2.5h; and the operating pressure of the spray powder making is 8MPa.
[0092] Example 4
[0093] This embodiment provides a method for preparing cobalt-chromium-molybdenum alloy powder, the preparation method comprising:
[0094] Mixing cobalt powder, chromium powder and molybdenum powder to obtain mixed powder;
[0095] The mixed powder is subjected to cold isostatic pressing, hot isostatic pressing, vacuum melting and spray powdering in sequence to obtain cobalt-chromium-molybdenum alloy powder;
[0096] The particle size of the cobalt powder is 2-10 μm, and the purity is 99.96%; the particle size of the chromium powder is 3-6 μm, and the purity is 99.96%; the particle size of the molybdenum powder is 7-10 μm, and the purity is 99.99%;
[0097] The mixing is carried out under an inert atmosphere (argon); the mixing speed is 10 r / min; the mixing time is 24 h;
[0098] The mass ratio of cobalt powder, chromium powder and molybdenum powder in the mixed powder is 65:30:10;
[0099] The cold isostatic pressing pressure is 170 MPa; the cold isostatic pressing time is 60 min;
[0100] The temperature of the hot isostatic pressing is 1000°C; the pressure of the hot isostatic pressing is 190MPa; and the time of the hot isostatic pressing is 2h;
[0101] The absolute vacuum degree of the vacuum melting is 0.001 Pa; the temperature of the vacuum melting is 1600° C.; the time of the vacuum melting is 2 hours; and the operating pressure of the spray powder making is 8 MPa.
[0102] Comparative Example 1
[0103] The only difference from Example 1 is that cold isostatic pressing is not performed, but hot isostatic pressing is performed directly on the powder in the mold.
[0104] Comparative Example 2
[0105] The only difference from Example 1 is that hot isostatic pressing was not performed.
[0106] Comparative Example 3
[0107] The only difference from Example 1 is that hot isostatic pressing is replaced by hot pressing sintering under the same conditions.
[0108] In the above-mentioned embodiments and comparative examples, the degassing treatment before hot isostatic pressing is performed at 550° C. and an absolute vacuum degree of 0.005 Pa for 2 h.
[0109] 20 samples were randomly sampled from the cobalt-chromium-molybdenum alloy powder obtained in the embodiments and comparative examples, and the total amount of the samples accounted for 50% of the total amount of the powder. The components were tested, and the relative standard deviation of each element between the samples was calculated to analyze the composition uniformity of the cobalt-chromium-molybdenum alloy powder product. Furthermore, the particle size D90 value of the cobalt-chromium-molybdenum alloy powder obtained was tested according to GB / T19077, the bulk density of the cobalt-chromium-molybdenum alloy powder obtained was tested according to GB / T1479.2, and the oxygen content of the cobalt-chromium-molybdenum alloy powder obtained was tested according to GB / T4164. The results are shown in Table 1 below.
[0110] Table 1
[0111]
[0112] As can be seen from Table 1, in the solution provided by the present invention, uniform powder is obtained by sieving through 200 mesh, the vacuum degree of the smelting process is improved, the oxygen content of the cobalt-chromium-molybdenum powder is reduced, and the specific spray powder making pressure is controlled to obtain relatively fine powder particles. In Comparative Example 1, since the cold isostatic pressing process is not carried out, the degassing of the powder is difficult, the hot isostatic pressing process is not formed, and the next process cannot be effectively carried out. In Comparative Example 2, since the hot isostatic pressing process is not carried out, its vacuum smelting is a powder blank, and its smelting effect is uneven, resulting in different particle sizes. In Comparative Example 3, the hot pressing sintering process is adopted, and the blank cannot complete pressure sintering, and can only achieve low-temperature sintering. Its oxygen content is high, the formability is poor, and the particles are uneven.
[0113] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0114] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0115] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing cobalt-chromium-molybdenum alloy powder, It is characterized in that The preparation method comprises: Mixing cobalt powder, chromium powder and molybdenum powder to obtain mixed powder; The mixed powder is subjected to cold isostatic pressing, hot isostatic pressing, vacuum melting and spray powdering in sequence to obtain cobalt-chromium-molybdenum alloy powder.
2. The preparation method according to claim 1, It is characterized in that The particle size of the cobalt powder is 2-10 μm; The particle size of the chromium powder is 2-10 μm; The particle size of the molybdenum powder is 2-10 μm.
3. The preparation method according to claim 1, It is characterized in that The mixing is carried out under an inert atmosphere; The mixing speed is 10-15r / min; The mixing time is 12-24h.
4. The preparation method according to claim 1, It is characterized in that The mass ratio of cobalt powder, chromium powder and molybdenum powder in the mixed powder is (60-65):(25-30):(5-10).
5. The preparation method according to claim 1, It is characterized in that The cold isostatic pressing pressure is 170-250 MPa.
6. The preparation method according to claim 1, It is characterized in that The cold isostatic pressing time is 30-60 minutes.
7. The preparation method according to claim 1, It is characterized in that The temperature of the hot isostatic pressing is 1000-1150°C; The hot isostatic pressing pressure is 100-190 MPa.
8. The preparation method according to claim 1, It is characterized in that The hot isostatic pressing time is 2-7h.
9. The preparation method according to claim 1, It is characterized in that The absolute vacuum degree of the vacuum melting is ≤0.001Pa; The temperature of the vacuum melting is 1500-1600°C; The vacuum melting time is 2-2.5h.
10. The preparation method according to claim 1, It is characterized in that The operating pressure of the spray powder making is 8-15MPa.