Sintered preformed brazing filler metal and preparation method and application thereof
By using sintered preformed brazing materials with magnesium film, aluminum powder, copper oxide powder and nickel powder during the brazing process, the problem of excessive temperature caused by aluminum-based brazing is solved, and high-efficiency brazing of aluminum alloys at low temperatures is achieved , reduce energy consumption and improve solder joint strength.
Patent Information
- Application Number
- CN202411132637.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-16
AI Technical Summary
When existing aluminum-based brazing materials are used to braze aluminum alloys, excessive temperatures can easily lead to overheating damage to the heat-resistant parts of the aluminum alloy connectors and high energy consumption.
Sintered preformed brazing material, including magnesium film, aluminum powder, copper oxide powder and nickel powder, igniting heat through the low ignition point of the magnesium film to promote the reaction of aluminum powder and copper oxide powder, and generate intermetallic compounds or solid solution to achieve brazing Welding connections, and breaking the oxide film and promoting the oxidation slag through aluminum flux to improve the quality of the weld.
Brazing is achieved at lower temperatures, reducing the brazing temperature to about 500°C, improving solder joint strength, reducing energy consumption, and improving brazing quality.
Smart Images

Figure BDA0004999063030000091 
Figure BDA0004999063030000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of brazing, and in particular to a sintered preformed brazing material and a preparation method and application thereof. Background Art
[0002] Brazing uses an alloy with a lower melting point than the base metal as the brazing filler metal. When heated, the brazing filler metal melts and fills and remains in the joint gap by wetting and capillary action, while the base metal is in a solid state. The brazed joint is formed by mutual diffusion between the liquid brazing filler metal and the solid base metal. Brazing has little effect on the physical and chemical properties of the base metal, small welding stress and deformation, and can weld dissimilar metals with large differences in performance. It can complete multiple welds at the same time, and the joint appearance is beautiful and neat. The equipment is simple and the production investment is small.
[0003] The metal connecting material used in brazing is called solder. Solders are generally divided into two categories according to their liquidus temperature. Solders with liquidus temperatures below 450°C are usually called soft solders, and solders with liquidus temperatures above 450°C are called hard solders. According to the matrix elements that make up the solder, it can be divided into bismuth-based, indium-based, tin-based, lead-based, antimony-based and zinc-based solders, which are also called soft solders; and aluminum-based, silver-based, copper-based, manganese-based, nickel-based and palladium-based solders, which are also called hard solders. Usually, the solder should have good fluidity, uniform composition, small melting range, and good brazing joint strength. In addition, the melting point of the solder is an important physical property of the solder. The melting point of the solder refers to the temperature at which the solder is completely liquefied, which is also called the liquidus temperature. Except for the solders of pure metals and eutectic alloys, most solders have a corresponding interval from the beginning of melting to complete liquefaction. When brazing, the melting point of the brazing filler metal is usually several tens of degrees or more lower than that of the brazing metal. Otherwise, the brazing process is difficult to control, and the brazing metal grains may grow, overburn, or even partially melt. Among the many types of brazing fillers, aluminum alloys have been increasingly widely used in connectors because of their good thermal and electrical conductivity and corrosion resistance.
[0004] However, the melting point of aluminum-based brazing filler metals currently used for brazing aluminum alloys, such as the commonly used aluminum silicon brazing filler metals, is 577°C, while the brazing temperature usually needs to be 25°C higher than the melting point of the brazing filler metal, that is, the brazing temperature needs to be at least 600°C. The brazing temperature is too high, and it is close to the melting point of the aluminum alloy. Therefore, when heating the aluminum-based brazing filler metal and the aluminum alloy connector to melt the aluminum-based brazing filler metal and then braze the aluminum alloy connector, the other heat-sensitive parts of the aluminum alloy connector are easily overheated and damaged due to the high temperature, and the energy consumption is high. Summary of the invention
[0005] In view of this, it is necessary to provide a sintered preformed brazing filler metal and its preparation method and application to address the above problems. The sintered preformed brazing filler metal provided by the present invention can induce local brazing at a relatively low temperature to solve the problem of overheating damage when brazing other heat-sensitive parts of aluminum alloy connectors with aluminum-based brazing filler metal, and further reduce the brazing temperature while ensuring the brazing strength.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a sintered brazing preform comprising a magnesium film and aluminum powder, copper oxide powder and nickel powder attached to one side of the magnesium film, and an aluminum brazing flux attached to the other side of the magnesium film.
[0008] Furthermore, the mass of the nickel powder is 1.7%-2.7% of the total mass of the sintered preformed solder.
[0009] Furthermore, the mass ratio of the aluminum powder to the copper oxide powder is ≥9:40.
[0010] The mass ratio of aluminum to copper oxide for complete reaction is 9:40, and the copper and nickel generated by the reaction of aluminum and copper oxide are infinitely solid-soluble, which is beneficial to brazing. Moreover, if there is excess aluminum after the reaction, it can form an intermetallic compound with nickel, which is further beneficial to brazing. Therefore, it is necessary to ensure that there is enough aluminum involved in the reaction, that is, the mass ratio of aluminum powder to copper oxide powder in the present invention should be ≥9:40.
[0011] Furthermore, the mass of the aluminum powder is M1, the mass of the copper oxide powder is M2, and the mass of the nickel powder is M3, wherein (M1-9M2 / 40):M3=(6-10):1.
[0012] Nickel reacts with aluminum to form a nickel-aluminum alloy, which has excellent anti-aging properties and is beneficial to improving the strength of the solder joint. However, nickel has a high melting point. If the amount of nickel powder added is too large, it is easy to cause part of the nickel to fail to completely fuse with aluminum and copper; but if the amount of nickel powder added is too small, it will not have the effect of improving the strength of the solder joint. Therefore, in the present invention, the mass M1 of aluminum powder, the mass M2 of copper oxide powder, and the mass M3 of nickel powder should meet the relationship of (M1-9M2 / 40): M3 = (6~10): 1.
[0013] Furthermore, the particle sizes of the aluminum powder and the copper oxide powder are 10 μm to 50 μm, and the particle size of the nickel powder is 200 nm to 800 nm.
[0014] The smaller the particle size of aluminum powder, the larger the specific surface area, and the easier it is to oxidize; in addition, the smaller the particle size of aluminum powder and copper oxide powder, the higher the manufacturing cost; but too large a particle size is not conducive to the full mixing of powders, the full aluminothermic reaction during brazing, and the full contact of aluminum, copper and nickel to form intermetallic compounds or solid solutions to achieve brazing connection. Nickel has a high melting point. If nickel can be fully fused with aluminum and copper, the particle size of nickel powder needs to be as small as possible. However, the smaller the particle size of nickel powder, the larger the specific surface area, the easier it is to oxidize, and the smaller the particle size, the higher the powder making cost. Therefore, in the present invention, the particle size of aluminum powder and copper oxide powder is selected to be 10μm to 50μm, and the particle size of nickel powder is 200nm to 800nm. The powder particle size within this range can save costs and ensure that the powder is fully mixed to achieve good brazing.
[0015] Furthermore, the thickness of the magnesium film is 1 / 25 to 1 / 20 of the total thickness of the sintered preformed solder, and the mass of the magnesium film is 1.5% to 1.9% of the total mass of the sintered preformed solder. Magnesium has a low ignition point of only about 490°C. The heat generated by igniting the magnesium film at a lower temperature during brazing causes the aluminum powder and the copper oxide powder to produce a thermite reaction. The high temperature released by the thermite reaction further causes a part of the aluminum powder and the nickel powder to produce copper by thermite reaction, forming an intermetallic compound or solid solution, thereby achieving the purpose of brazing connection. If the magnesium film is too thin, the magnesium content is too little, and the heat generated is insufficient to trigger the thermite reaction; if the magnesium film is too thick, the magnesium content is too much, and the magnesium oxide slag generated after ignition will be too much, affecting the brazing quality. Therefore, the thickness of the magnesium film in the present invention is selected to be 1 / 25 to 1 / 20 of the total thickness of the sintered preformed solder (excluding the aluminum brazing agent part), and the mass of the magnesium film is 1.5% to 1.9% of the total mass of the sintered preformed solder.
[0016] Furthermore, in the sintered preformed brazing material, the side of the magnesium film not attached with aluminum powder, copper oxide powder and nickel powder is coated with aluminum brazing flux. The aluminum brazing flux can break the oxide film on the surface of the aluminum part, push the oxide slag generated during the brazing process to the periphery of the weld, and increase the activity of the aluminum powder to ensure the brazing quality of the weld.
[0017] Preferably, the aluminum brazing flux is a fluoroaluminate aluminum brazing flux.
[0018] More preferably, the aluminum brazing agent is cesium aluminum fluoroaluminate brazing agent or potassium aluminum fluoroaluminate brazing agent, and the content is 2%-8% of the total mass of the sintered preformed brazing material. If the brazing agent content is too little, the effect of removing the oxide film on the surface of the aluminum part is not good; if the brazing agent content is too much, too much brazing agent will remain after brazing, affecting the brazing effect and appearance. Therefore, in the present invention, the aluminum brazing agent content is 2%-8% of the total mass of the sintered preformed brazing material.
[0019] In a second aspect, the present invention provides a method for preparing a sintered preformed solder, comprising the following steps:
[0020] S1, mixing aluminum powder, copper oxide powder and nickel powder uniformly to obtain a mixed powder;
[0021] S2, rolling the magnesium strip into a magnesium film of a desired thickness, and cutting it into a desired size;
[0022] S3, laying the magnesium film prepared in step S2 in the mold cavity of the die-casting machine, and then placing the mixed powder prepared in step S1 on the magnesium film in the mold cavity, and then performing die-casting so that the mixed powder is compacted on the magnesium film to form a solder compact;
[0023] S4, coating the side of the magnesium film without the mixed powder in the solder compact prepared in step S3 with an aluminum solder flux to form a sintered preformed solder.
[0024] In a third aspect, the present invention provides application of the sintered preformed brazing filler metal or the method for preparing the sintered preformed brazing filler metal in brazing.
[0025] The beneficial effects of the present invention are:
[0026] (1) The brazing temperature of commonly used aluminum-silicon brazing materials is as high as over 600°C, which consumes a lot of energy and may cause overheating and damage to other heat-sensitive parts of aluminum alloy connectors due to excessively high temperatures. The present invention takes advantage of the fact that magnesium has an ignition point as low as 490°C. The magnesium film is ignited at a relatively low temperature during brazing. The heat generated causes the aluminum powder and copper oxide powder to produce a thermite reaction. The high temperature released by the thermite reaction further causes part of the aluminum powder to react with the nickel powder and the copper generated by the thermite reaction to form an intermetallic compound or solid solution, thereby achieving the purpose of brazing connection. Therefore, the present invention only needs to apply a temperature as low as about 500°C to the weld to achieve the purpose of brazing aluminum alloy connectors;
[0027] (2) In the present invention, the side of the magnesium film to which aluminum powder, copper oxide powder and nickel powder are not attached is coated with aluminum brazing flux, which can break the oxide film on the surface of the aluminum alloy brazing part and push the oxide slag generated during the brazing process to the surrounding of the weld. In addition, the activity of the aluminum powder can be increased, further improving the brazing quality of the weld. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be further clearly and completely described in combination with the embodiments of the present invention. It should be noted that the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0029] In the description of the present invention, it should be noted that, if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0030] Example 1
[0031] A sintered preformed brazing material, comprising a magnesium film and aluminum powder, copper oxide powder and nickel powder attached to the same side of the magnesium film; an aluminum brazing agent is coated on the side of the magnesium film to which the aluminum powder, copper oxide powder and nickel powder are not attached; the size (excluding the brazing agent part) is 10*10*0.5mm, and the total mass is 4.736g; the particle size of the aluminum powder is 10μm, the particle size of the copper oxide powder is 10μm, and the particle size of the nickel powder is 200nm; the mass of the aluminum powder is 1.38g; the mass of the copper oxide powder is 2.76g, and the mass of the nickel powder is 200nm; The mass of the aluminum powder M1, the mass of the copper oxide powder M2, and the mass of the nickel powder M3 are in the relationship of (M1-9M2 / 40): M3=6:1; the thickness of the magnesium foil is 25 μm and the mass is 0.09 g, that is, the thickness of the magnesium film is 1 / 20 of the total thickness of the sintered preformed solder, and the mass of the magnesium film is 1.9% of the total mass of the sintered preformed solder; the aluminum brazing agent is cesium aluminum fluoroaluminate brazing agent, the mass is 0.379 g, and the content is 8% of the total mass of the sintered preformed solder.
[0032] The sintered preformed brazing material is prepared by the following method:
[0033] S1. Prepare mixed powder: 1.38 g of aluminum powder with a particle size of 10 μm, 2.76 g of copper oxide powder with a particle size of 10 μm, and 0.127 g of nickel powder with a particle size of 200 nm are mixed evenly to prepare a mixed powder;
[0034] S2. Preparation of magnesium film: rolling a magnesium strip into a magnesium film with a thickness of 25 μm, and cutting the film into a size of 10 mm*10 mm, the weight of which is 0.09 g;
[0035] S3, preparing solder compacts: spreading the magnesium film prepared in step S2 in the mold cavity of a die-casting machine, and then placing 4.267 g of the mixed powder prepared in step S1 (wherein the mass of aluminum powder is 1.38 g, the mass of copper oxide powder is 2.76 g, and the mass of nickel powder is 0.127 g) on the magnesium film in the mold cavity, and then performing die-casting, so that the mixed powder is compacted on the magnesium film to form solder compacts with a size of 10*10*0.5 mm, wherein the total mass of each solder compact is 4.357 g, wherein the mass of the magnesium film is 0.09 g, and the mass of the mixed powder is 4.267 g;
[0036] S4. Preparation of sintered preformed solder: 0.379 g of cesium aluminum fluoroaluminate solder flux is coated on the side of the solder compact prepared in step S3 that is not attached with the magnesium film of the mixed powder to form a sintered preformed solder.
[0037] Example 2
[0038] A sintered preformed solder, which is different from Example 1 in that the particle size of the aluminum powder is 50 μm.
[0039] Example 3
[0040] A sintered preformed solder, which is different from Example 1 in that the particle size of the copper oxide powder is 50 μm.
[0041] Example 4
[0042] A sintered preformed solder, which is different from Example 1 in that the particle sizes of the aluminum powder and the copper oxide powder are both 50 μm.
[0043] Example 5
[0044] A sintered preformed solder, which is different from Example 1 in that the particle size of the nickel powder is 800 nm.
[0045] Example 6
[0046] A sintered preformed solder, which differs from Example 1 in that the total mass of the mixed powder is 4.31 g, of which the mass of the aluminum powder is 1.43 g, the mass of the copper oxide powder is 2.8 g, and the mass of the nickel powder is 0.08 g, i.e., the mass of the nickel powder is 1.7% of the total mass of the sintered preformed solder; the mass of the cesium aluminum fluoroaluminate solder is 0.383 g, i.e., the content is 8% of the total mass of the sintered preformed solder; the mass of the magnesium film is 0.09 g, i.e., 1.9% of the total mass of the sintered preformed solder; the relationship among the mass M1 of the aluminum powder, the mass M2 of the copper oxide powder, and the mass M3 of the nickel powder is (M1-9M2 / 40): M3=10:1.
[0047] Example 7
[0048] A sintered preformed solder, which differs from Example 1 in that the thickness of the magnesium film is 20 μm and the mass is 0.072 g, that is, the thickness of the magnesium film is 1 / 25 of the total thickness of the sintered preformed solder, and the mass of the magnesium film is 1.5% of the total mass of the sintered preformed solder.
[0049] Example 8
[0050] A sintered preformed solder, which differs from Example 1 in that the mass of the cesium aluminum fluoroaluminate solder is 0.089 g, and its content is 2% of the total mass of the sintered preformed solder.
[0051] Example 9
[0052] A sintered preformed brazing material, which is different from Example 1 in that the aluminum brazing flux is potassium fluoroaluminate aluminum brazing flux among fluoroaluminate aluminum brazing fluxes.
[0053] Comparative Example 1
[0054] A sintered preformed solder, which differs from Example 1 in that cobalt powder is used instead of nickel powder.
[0055] Comparative Example 2
[0056] A sintered preform solder, which differs from Example 1 in that a tin film is used instead of a magnesium film.
[0057] Comparative Example 3
[0058] A sintered preformed solder, which differs from Example 1 in that it does not contain a magnesium film; the size of the solder compact is also 10*10*0.5mm (excluding the aluminum solder part), the mass of the solder compact is 4.492g, and one of the upper and lower surfaces of the solder is coated with cesium aluminum fluoroaluminate solder, the mass of the cesium aluminum fluoroaluminate solder is 0.391g, accounting for 8% of the total mass.
[0059] Comparative Example 4
[0060] A sintered preformed solder, which is different from Example 1 in that the particle size of the aluminum powder is 100 μm.
[0061] Comparative Example 5
[0062] A sintered preformed solder is different from Example 1 in that the particle size of the copper oxide powder is 100 μm.
[0063] Comparative Example 6
[0064] A sintered preformed solder, which is different from Example 1 in that the particle size of the nickel powder is 1200 nm.
[0065] Comparative Example 7
[0066] A sintered preformed solder, which differs from Example 1 in that the total mass of the mixed powder is 4.329g, of which the mass of the aluminum powder is 1.339g, the mass of the copper oxide powder is 2.75g, and the mass of the nickel powder is 0.24g; the mass of the cesium aluminum fluoroaluminate solder is 0.384g, and its content is still 8% of the total mass of the sintered preformed solder; the mass of the nickel powder is 5% of the total mass of the sintered preformed solder; the thickness of the magnesium film is still 1 / 20 of the total thickness of the sintered preformed solder, that is, the mass of the magnesium film is still 1.9% of the total mass of the sintered preformed solder; the relationship among the mass M1 of the aluminum powder, the mass M2 of the copper oxide powder, and the mass M3 of the nickel powder is (M1-9M2 / 40): M3=3:1.
[0067] Comparative Example 8
[0068] A sintered preformed solder, which differs from Example 1 in that the mass of the aluminum powder is 1.406g, the mass of the copper oxide powder is 2.85g, and the mass of the nickel powder is 0.051g; the mass of the cesium aluminum fluoroaluminate solder is 0.382g, and its content is still 8% of the total mass of the sintered preformed solder; the mass of the nickel powder is 1.1% of the total mass of the sintered preformed solder; the thickness of the magnesium film is still 1 / 20 of the total thickness of the sintered preformed solder, that is, the mass of the magnesium film is still 1.9% of the total mass of the sintered preformed solder; the relationship among the mass M1 of the aluminum powder, the mass M2 of the copper oxide powder, and the mass M3 of the nickel powder is (M1-9M2 / 40): M3=15:1.
[0069] Comparative Example 9
[0070] A sintered preformed solder, which differs from Example 1 in that the thickness of the magnesium film is 10 μm and the mass is 0.036 g, that is, the thickness of the magnesium film is 1 / 50 of the total thickness of the sintered preformed solder, and the mass of the magnesium film is 0.8% of the total mass of the sintered preformed solder.
[0071] Comparative Example 10
[0072] A sintered preformed solder, which differs from Example 1 in that the thickness of the magnesium film is 50 μm and the mass is 0.18 g, that is, the thickness of the magnesium film is 1 / 10 of the total thickness of the sintered preformed solder, and the mass of the magnesium film is 3.9% of the total mass of the sintered preformed solder.
[0073] Comparative Example 11
[0074] A sintered preformed solder, which differs from Example 1 in that the mass of the cesium aluminum fluoroaluminate solder is 0.022 g, and its content is 0.5% of the total mass of the sintered preformed solder.
[0075] Comparative Example 12
[0076] A sintered preformed solder, which differs from Example 1 in that the mass of the cesium aluminum fluoroaluminate solder is 0.769 g, and its content is 15% of the total mass of the sintered preformed solder.
[0077] Comparative Example 13
[0078] The commercially available Al88Si12 brazing filler metal has a size of 10*10*0.5 mm (excluding the aluminum brazing flux part) and a mass of 0.133 g. 0.012 g of cesium aluminum fluoroaluminate brazing flux is coated on its surface, and the mass of cesium aluminum fluoroaluminate brazing flux accounts for 8% of the total mass.
[0079] Performance testing
[0080] In order to further verify the performance of the sintered preformed brazing filler metal of the present application, the brazing materials in Examples 1-9 and Comparative Examples 1-12 were used as the test group, and the brazing material in Comparative Example 13 was used as the control group. Brazing tests were performed respectively. The aluminum parts to be brazed were assembled with the brazing fillers of the test group and the control group, respectively, and laser brazing was performed. The size of the brazing materials in the test group and the control group was 10*10*0.5mm (excluding the brazing agent part), and the following tests were performed:
[0081] 1) Record the temperature required for brazing. The temperature required for brazing is measured with an infrared temperature detector. The lower the temperature, the less likely it is to burn the aluminum parts and the more energy-saving it is.
[0082] 2) After brazing is completed, the shear strength of the overlapped brazed parts is tested by an electronic universal testing machine. The greater the shear strength, the better the brazing strength.
[0083] The test results are shown in Table 1.
[0084] Table 1 Performance test results
[0085]
[0086]
[0087] 1) Comparison of performance test results of Examples 1 to 9 and Comparative Example 13
[0088] From the data in Table 1, it can be seen that the shear strength of Example 1 is increased by about 45% compared with Comparative Example 13 (i.e., the control group), the brazing temperature is reduced from more than 600°C to nearly 500°C, the brazing temperature is reduced by about 110 degrees, and the brazing effect is significantly improved. The other embodiments also have obvious improvements in the effects of increasing shear strength and reducing brazing temperature.
[0089] 2) Comparison of nickel powder modification effects by Example 1, Comparative Example 1, and Comparative Example 13
[0090] From the data in Table 1, it can be seen that Comparative Example 13 is a common solder available on the market, and Comparative Example 1 uses another solder modification material, cobalt, to replace nickel. Through the comparison of performance test results, it can be seen that cobalt modification can effectively reduce the brazing temperature, but the relative shear strength is also reduced. Example 1 has obvious improvements in the effects of increasing shear strength and reducing brazing temperature.
[0091] 3) Comparison of magnesium film modification effects by Example 1, Comparative Example 2, and Comparative Example 3
[0092] From the data in Table 1, it can be seen that comparative example 3 does not use magnesium film, and comparative example 2 uses tin film instead of magnesium film. The tin film has no effect on reducing the brazing temperature and also reduces the shear strength. The magnesium film used in Example 1 has obvious improvements in increasing the shear strength and reducing the brazing temperature.
[0093] 4) Comparison of the effect of aluminum powder particle size modification by Example 1, Example 2, and Comparative Example 4
[0094] From the data in Table 1, it can be seen that as the particle size of aluminum powder decreases from 100μm to 10μm, the shear strength increases and the brazing temperature decreases. The effect improvement brought by reducing the particle size from 100μm to 50μm is higher than that brought by reducing the particle size from 50μm to 10μm. Too large an aluminum powder particle size is not conducive to the full mixing of the powder, the full aluminothermic reaction during brazing, and the full contact of aluminum, copper and nickel to form intermetallic compounds or solid solutions to achieve brazing connection; however, the smaller the aluminum powder particle size, the larger the specific surface area, the easier it is to oxidize, and the smaller the aluminum powder particle size, the higher the manufacturing cost. In summary, when the aluminum powder particle size is in the range of 10μm to 50μm, the product cost is low, and it can be used at a lower brazing temperature and obtain a higher shear strength.
[0095] 5) Comparison of the effect of copper oxide powder particle size modification by Example 1, Example 3, and Comparative Example 5
[0096] From the data in Table 1, it can be seen that as the particle size of copper oxide powder decreases from 100μm to 10μm, the shear strength increases and the brazing temperature decreases. The effect improvement brought by reducing the particle size from 100μm to 50μm is higher than that brought by reducing the particle size from 50μm to 10μm. The particle size of copper oxide powder is too large, which is not conducive to the full mixing of powders, the full aluminothermic reaction during brazing, and the full contact of aluminum, copper and nickel to form intermetallic compounds or solid solutions to achieve brazing connection; however, the smaller the particle size of copper oxide powder, the higher the manufacturing cost. In summary, when the particle size of copper oxide powder is in the range of 10μm to 50μm, the product cost is low, and it can be used at a lower brazing temperature and obtain a higher shear strength.
[0097] 6) Through Example 1, Example 2, Example 3, and Example 4, the effect of simultaneous modification of aluminum powder and copper oxide powder is compared
[0098] From the data in Table 1, it can be seen that the particle sizes of the aluminum powder and the copper oxide powder in Example 4 are both 50 μm. Compared with Example 4, the particle size of the aluminum powder in Example 3 is reduced to 10 μm, and the shear strength is slightly reduced, and the brazing temperature is increased. This may be due to the fact that the aluminum powder particle size is too small, the larger the specific surface area, and the easier it is to oxidize during powder making; compared with Example 4, the particle size of the copper oxide powder in Example 2 is reduced to 10 μm, the brazing temperature is reduced, and the brazing strength is improved. Compared with Example 4, Example 1 reduces the particle size of the aluminum powder and the copper oxide powder to 10 μm at the same time, which can continue to improve the obvious shear strength and significantly reduce the brazing temperature, and the modification effect is better than reducing the copper oxide powder alone.
[0099] 7) Comparison of the effect of nickel powder particle size modification by Example 1, Example 5, and Comparative Example 6
[0100] From the data in Table 1, it can be seen that as the particle size of nickel powder decreases from 1200nm to 200nm, the shear strength increases and the brazing temperature decreases. The effect of reducing the particle size from 1200nm to 800nm on the shear strength is smaller than that of reducing the particle size from 800nm to 200nm, and the difference in the effect of brazing temperature is not much. Nickel has a high melting point. If nickel can be fully fused with aluminum and copper, the particle size of nickel powder needs to be as small as possible; however, the smaller the particle size of nickel powder, the larger the specific surface area, the easier it is to oxidize, and the smaller the particle size, the higher the powder making cost. In summary, when the nickel powder particle size is in the range of 200nm to 800nm, the product cost is low, and it can be used at a lower brazing temperature and obtain a higher shear strength.
[0101] 8) Through Example 1, Example 6, Comparative Example 7 and Comparative Example 8, the modification effect of the mass ratio of aluminum powder, copper oxide powder and nickel powder was compared.
[0102] From the data in Table 1, it can be seen that when the mass M1 of the aluminum powder, the mass M2 of the copper oxide powder, and the mass M3 of the nickel powder meet the ratio of (M1-9M2 / 40): M3 in the range of (3 to 15): 1, as the ratio increases, the degree of improvement in the shear strength and brazing temperature first increases and then decreases, the ratio increases in the range of (3 to 10): 1, and decreases in the range of (10 to 15): 1, and the effect improvement in the range of (3 to 6): 1 is more significant than that in the range of (6 to 10): 1. Therefore, when the mass M1 of the aluminum powder, the mass M2 of the copper oxide powder, and the mass M3 of the nickel powder meet the ratio of (M1-9M2 / 40): M3 in the range of (6 to 10): 1, they can be used at a lower brazing temperature and obtain a higher shear strength.
[0103] 9) Comparison of the modification effects of magnesium film thickness and quality by Example 1, Example 7, Comparative Example 9, and Comparative Example 10
[0104] From the data in Table 1, it can be seen that the magnesium film accounts for the total thickness and total mass of the sintered preformed solder in a proportional relationship. When the magnesium film thickness accounts for 1 / 50 to 1 / 10, that is, when the mass proportion of the magnesium film is in the range of 0.8% to 3.9%, as the proportion of the magnesium film increases, the degree of improvement in the shear strength effect first increases and then decreases. The magnesium film thickness accounts for 1 / 50 to 1 / 20 (that is, the mass proportion is 0.8% to 1.9%), and the magnesium film thickness accounts for 1 / 20 to 1 / 10 (that is, the mass proportion is 1.9% to 3.9%). The effect improvement in the magnesium film thickness in the range of 1 / 50 to 1 / 25 (that is, the mass proportion is 0.8% to 1.5%) is more significant than that in the range of 1 / 25 to 1 / 20 (that is, the mass proportion is 1.5% to 1.9%). The brazing temperature modification effect increases with the increase of the magnesium film thickness, that is, the mass ratio. However, the improvement effect is significantly reduced in the range of 1 / 20 to 1 / 10 (i.e., the mass ratio is 1.9% to 3.9%) compared with other ranges. Moreover, from the effect of brazing of the brazing material of comparative example 10, the magnesium film thickness (i.e., mass) ratio is too large, and there is too much magnesium oxide slag, which affects the brazing strength and appearance. Therefore, from the comprehensive effect, the magnesium film accounts for a proportional relationship between the total thickness and total mass of the sintered preformed brazing material. When the magnesium film thickness accounts for 1 / 25 to 1 / 20 (i.e., the mass ratio is 1.5% to 1.9%), it can be used at a lower brazing temperature and obtain a higher shear strength without affecting the appearance, and the comprehensive effect is optimal.
[0105] 10) Through Example 1, Example 6, Comparative Example 7, and Comparative Example 8, the modification effects of different mass proportions of nickel powder in the sintered preformed solder are compared.
[0106] From the data in Table 1, it can be seen that as the mass proportion of nickel powder increases, the degree of improvement in shear strength and brazing temperature first increases and then decreases. The mass proportion of nickel powder increases in the range of 1.1% to 2.7%, and decreases in the range of 2.7% to 5%. The improvement in the mass proportion of nickel powder in the range of 1.1% to 1.7% is more significant than that in the range of 1.7% to 2.7%. Therefore, when the mass of nickel powder is 1.7%-2.7% of the total mass of the sintered preformed brazing material, it can be used at a lower brazing temperature and obtain a higher shear strength.
[0107] 11) Through Example 1, Example 8, Comparative Example 11, and Comparative Example 12, the modification effect of the mass proportion of cesium aluminum fluoroaluminate brazing flux is compared
[0108] From the data in Table 1, it can be seen that when the proportion of cesium aluminum fluoroaluminate brazing agent in the total mass of the sintered preformed brazing material is in the range of 0.5% to 15%, as the proportion of brazing agent increases, the degree of improvement in the shear strength and brazing temperature first increases and then decreases, increasing in the range of 0.5% to 8%, decreasing in the range of 8% to 15%, and the improvement in the range of 0.5% to 2% is more significant than that in the range of 2% to 8%. After brazing the brazing material of Example 12, when the brazing agent content is too much, too much brazing agent remains after brazing, which affects the brazing effect and appearance. Therefore, it is shown that when the aluminum brazing agent content in the present invention is 2%-8% of the total mass of the sintered preformed brazing material, it can be used at a lower brazing temperature and obtain a higher shear strength without affecting the appearance, and the comprehensive effect is optimal.
[0109] 12) Compare the modification effects of the aluminum brazing flux selected by Example 1 and Example 9
[0110] From the data in Table 1, it can be seen that the effects of the commonly used potassium fluoroaluminate aluminum brazing flux on increasing the shear strength and reducing the brazing temperature are not as obvious as those of the cesium fluoroaluminate aluminum brazing flux.
[0111] From the above comparison, it can be seen that the sintered preformed solder provided by the present invention not only ensures high shear strength, but also effectively reduces the brazing temperature.
[0112] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A sintered preformed brazing material, It is characterized in that The invention comprises a magnesium film, aluminum powder, copper oxide powder and nickel powder attached to the same side of the magnesium film, and an aluminum brazing flux attached to the other side of the magnesium film.
2. The sintered brazing preform according to claim 1, It is characterized in that The mass of the nickel powder is 1.7%-2.7% of the total mass of the sintered preformed solder.
3. The sintered brazing preform according to claim 1, It is characterized in that The mass of the aluminum powder is M 1 , the mass of the copper oxide powder is M 2 , the mass of the nickel powder is M 3 , where (M 1 -9M 2 / 40): M 3 =(6~10):
1.
4. The sintered brazing preform according to claim 1, It is characterized in that The particle sizes of the aluminum powder and the copper oxide powder are 10 μm to 50 μm, and the particle size of the nickel powder is 200 nm to 800 nm.
5. The sintered brazing preform according to claim 1, It is characterized in that The thickness of the magnesium film is 1 / 25 to 1 / 20 of the total thickness of the sintered preformed solder; the mass of the magnesium film is 1.5% to 1.9% of the total mass of the sintered preformed solder.
6. The sintered brazing preform according to claim 1, It is characterized in that In the sintered preform brazing material, the side of the magnesium film to which the aluminum powder, the copper oxide powder and the nickel powder are not attached is coated with an aluminum brazing flux.
7. The sintered brazing preform according to claim 6, It is characterized in that The aluminum brazing flux is a fluoroaluminate aluminum brazing flux.
8. The sintered brazing preform according to claim 7, It is characterized in that The aluminum brazing agent is cesium aluminum fluoroaluminate brazing agent or potassium aluminum fluoroaluminate brazing agent, and the content thereof is 2%-8% of the total mass of the sintered preformed brazing material.
9. A method for preparing a sintered brazing preform according to any one of claims 1 to 8, It is characterized in that The following steps are involved: S1, mixing aluminum powder, copper oxide powder and nickel powder uniformly to obtain a mixed powder; S2, rolling the magnesium strip into a magnesium film of a desired thickness, and cutting it into a desired size; S3, laying the magnesium film prepared in step S2 in the mold cavity of the die-casting machine, and then placing the mixed powder prepared in step S1 on the magnesium film in the mold cavity, and then performing die-casting so that the mixed powder is compacted on the magnesium film to form a solder compact; S4, coating the side of the magnesium film without the mixed powder in the solder compact prepared in step S3 with an aluminum solder flux to form a sintered preformed solder.
10. Use of the sintered preformed brazing filler metal according to any one of claims 1 to 8 or the method for preparing the sintered preformed brazing filler metal according to claim 9 in brazing.
Citation Information
Patent Citations
Method for connecting carbon fiber reinforced aluminum-based composite with metal
CN102658368A
Solder material, solder paste, foam solder, solder joint, and method for controlling solder material
CN107073656A
Air reaction brazing device with multi-field coupling, and method for carrying out air reaction brazing by applying air reaction brazing device with multi-field coupling
CN110039144A
Composite solder and preparation method and application thereof
CN111468857A
Welding powder of stainless steel steel-armored grounding grid suitable for alternate wetting and drying environment
CN111843294A