Production method and device for concrete material modified phosphogypsum admixture

Through the production method of modified phosphogypsum blending materials, combined with drying, fine grinding and heating treatment, the problem of impurities in phosphogypsum affecting strength is solved, the strength of concrete building materials is improved and environmental pollution is reduced, and the efficiency of phosphogypsum is achieved is achieved. Modification and resource utilization.

CN118993608AInactive Publication Date: 2024-11-22GUIZHOU TEMEIDA TECHNOLOGY BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411213960.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-31
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Phosphorus gypsum is rich in impurities such as water-soluble phosphorus and fluorine that affects the strength of concrete building materials, limits its application in building materials, and unscientific emissions pollute the environment.

Method used

A modified phosphogypsum blending method is adopted, including mixed phosphogypsum powder, fly ash, calcium carbide slag, etc., after drying, grinding and heating treatment, combined with the use of a ball mill and a wet grinding device, the impurity content is reduced. Improve the strength of the concrete and add bamboo charcoal during the autoclave aeration process to inhibit hydration.

Benefits of technology

It significantly improves the strength of phosphogypsum concrete building materials, broadens its application scope, reduces environmental pollution, and realizes efficient modification and treatment of phosphogypsum and comprehensive utilization of resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993608A_ABST
    Figure CN118993608A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, in particular to a production method and device of a modified ardealite admixture for a concrete material, and the production method comprises the following steps: S1, preparing a modified ardealite primary material; s2, drying the modified ardealite primary material in a high-temperature environment of 280-350 DEG C until the water content is 7-8%, so as to obtain a modified ardealite dry material; s3, grinding the modified ardealite dried material by adopting a ball mill until particles of 180-220 meshes are obtained, so as to obtain modified ardealite powder; s4, mixing the following component raw materials in parts by weight: 0.25 to 0.4 part of polyaluminum chloride, 0.3 to 0.5 part of calcium formate, 0.25 to 0.4 part of sodium silicate, 0.03 to 0.05 part of rubber powder, 0.08 to 0.1 part of cellulose ether, 0.5 to 0.8 part of a high-efficiency water reducing agent and 98 to 99 parts of the modified phosphogypsum powder, so as to obtain the modified phosphogypsum admixture for the autoclaved aerated concrete blocks. Compared with the prior art, the ardealite is neutralized and modified, so that the technical problem that the strength of the concrete building material taking the ardealite as the raw material is influenced due to the fact that the ardealite is rich in water-soluble phosphorus, fluorine and other impurities is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, in particular to a method and a device for producing a modified phosphogypsum admixture for concrete materials. Background Art

[0002] Phosphogypsum is a byproduct of the production process of phosphoric acid extraction by sulfuric acid method. It is also an industrial waste residue with calcium sulfate dihydrate as the main component. Its main components are resources such as sulfur and calcium, which have many potential uses. It also contains impurities such as phosphorus, fluorine, alkali metal elements, silicon, aluminum, iron, magnesium, etc. that are harmful to the environment and comprehensive utilization. With the rapid development of the phosphate fertilizer industry, the discharge and stockpiling of phosphogypsum have shown a significant year-on-year increase. The unscientific discharge of phosphogypsum not only increases the land area, but also pollutes the environment, becoming an industrial waste residue that urgently needs to be recycled. Therefore, the conversion and consumption of phosphogypsum has become an urgent problem to be solved.

[0003] Using phosphogypsum as an industrial raw material to produce foamed concrete building materials is one of the main conversion and consumption pathways at present. However, phosphogypsum is rich in impurities such as water-soluble phosphorus and fluorine, which seriously affect the hydration reaction of phosphogypsum, resulting in poor use strength of concrete products made from phosphogypsum. Direct use as a building material for building exterior walls will affect the building strength. At the same time, because phosphogypsum contains more water-soluble impurities, after contact with rainwater, the water-soluble impurities enter the water body and pollute the environment. Therefore, foamed concrete building materials made from phosphogypsum can usually only be used as indoor building materials with low strength requirements, which greatly limits the conversion and consumption of phosphogypsum. Therefore, modifying phosphogypsum, reducing the impurity content in phosphogypsum, improving the use strength of concrete products made from phosphogypsum, broadening the conversion pathways of phosphogypsum, and maximizing the value of phosphogypsum have become technical issues that need to be urgently addressed in the industry. Summary of the invention

[0004] The present invention aims to provide a method and device for producing phosphogypsum admixture for modified concrete materials, mainly used to solve the technical problem that phosphogypsum in the prior art is rich in impurities such as water-soluble phosphorus and fluorine, which affects the strength of concrete building materials using phosphogypsum as raw material.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A method for producing a modified phosphogypsum admixture for concrete materials comprises the following steps:

[0007] S1: by weight, 65-80 parts of phosphogypsum powder, 15-30 parts of fly ash, and 8-10 parts of carbide slag are mixed and aged for 40-50 hours to obtain a modified phosphogypsum raw material;

[0008] S2: drying the modified phosphogypsum raw material in a high temperature environment of 280-350° C., and drying the modified phosphogypsum raw material to a moisture content of 7%-8%, thereby obtaining a modified phosphogypsum dry material;

[0009] S3: Grinding the dried modified phosphogypsum material into particles of 180-220 mesh using a ball mill to obtain modified phosphogypsum powder;

[0010] S4: Mix the following raw materials in proportion by weight: 0.25-0.4 parts of polyaluminium, 0.3-0.5 parts of calcium formate, 0.25-0.4 parts of sodium silicate, 0.03-0.05 parts of rubber powder, 0.08-0.1 parts of cellulose ether, 0.5-0.8 parts of high-efficiency water reducing agent and 98-99 parts of modified phosphogypsum powder to obtain modified phosphogypsum admixture for autoclaved aerated concrete blocks.

[0011] Preferably, the preparation of the phosphogypsum powder in step S1 includes the following steps: putting the original phosphogypsum and water into a wet grinding device in a weight ratio of 1:5-10, the wet grinding device synchronously stirs and grinds the mixture of the original phosphogypsum and water for 10-15 minutes, centrifuges and dries to obtain the phosphogypsum powder.

[0012] Preferably, the wet grinding device heats the original phosphogypsum and water under high pressure when stirring and grinding the phosphogypsum and water, and the water temperature is 150-180°C.

[0013] Preferably, in step S4, 5-10 parts of bamboo charcoal particles are also added.

[0014] Working principle and beneficial effects of this solution:

[0015] 1. Calcium carbide slag is added to the modified phosphogypsum admixture of autoclaved aerated concrete blocks. As an alkaline waste residue, calcium carbide slag can integrate the acidity of phosphogypsum, convert the soluble phosphorus in phosphogypsum into insoluble precipitates, change the crystal shape of phosphogypsum, make phosphogypsum easier to hydrate, and the concrete slurry formed after hydration has higher strength.

[0016] 2. If too much precipitation is produced after hydration of phosphogypsum, the hydration of phosphogypsum should be inhibited and the original phosphogypsum should be initialized, including stirring and grinding the phosphogypsum, so that some impurities in the phosphogypsum can enter the water, reducing the precipitation produced when the phosphogypsum is subsequently neutralized with calcium carbide slag, promoting the subsequent hydration of phosphogypsum, and improving the strength of concrete building materials made of phosphogypsum.

[0017] 3. Heating treatment of phosphogypsum can partially convert phosphogypsum into hemihydrated phosphogypsum. Hemihydrated phosphogypsum has good crystallization, is solid, has high fluidity, and requires less water. Compared with untreated original phosphogypsum, it has less impurities and stronger coagulation properties.

[0018] 4. Add bamboo charcoal to the modified phosphogypsum admixture of autoclaved aerated concrete blocks. The bamboo charcoal can absorb a part of the insoluble precipitate during the hydration of the phosphogypsum, prevent the precipitate from adhering to the phosphogypsum crystals, and inhibit the hydration of the phosphogypsum.

[0019] Option 2:

[0020] A production device for concrete material modified phosphogypsum admixture, comprising a wet grinding device, the wet grinding device comprising a tank body, a stirring and grinding device rotatably arranged inside the tank body, the stirring and grinding device comprising a rotatable shaft, a stirring and grinding assembly arranged in an equidistant circular array fixedly mounted on the circumferential surface of the shaft, the stirring and grinding assembly comprising an elastically deformable annular spring piece, one end of the annular spring piece is fixedly connected to the shaft, and the other end is in contact with the inside of the tank body.

[0021] The beneficial effects of this program are as follows:

[0022] The original phosphogypsum and water are added into the tank body at the same time, and the heating plate at the bottom of the tank body heats the mixture of the original phosphogypsum and water. At the same time, the shaft rotates, thereby driving the stirring and grinding assembly to rotate together. The annular springs in the stirring and grinding assembly drive the mixed liquid inside the tank body to move, and the original phosphogypsum and water are stirred evenly. In the stirring process, the original phosphogypsum powder is transported toward the inner wall of the shell along the edge of the annular spring, and the end of the annular spring rubs against the inner wall of the shell to grind the powder.

[0023] This device can heat, stir and grind the original phosphogypsum powder at the same time, and has the following advantages:

[0024] 1. Stir and wash the original phosphogypsum powder once to reduce the phosphorus and fluorine content in the original phosphogypsum;

[0025] 2. Grind the original phosphogypsum powder to increase the contact surface between the original phosphogypsum and water, promote the release of harmful elements such as phosphorus and fluorine in the original phosphogypsum into the water, make the washing more complete, and reduce the water demand for washing the original phosphogypsum;

[0026] 3. Shaping the original phosphogypsum powder so that the admixture made of the original phosphogypsum has higher fluidity after being made into concrete slurry;

[0027] 4. The annular spring piece can be deformed, which has a pressing effect on the inner wall of the tank, making the grinding of the original phosphogypsum powder more efficient. When encountering relatively large pieces of original phosphogypsum particles, the annular spring piece can be deformed to prevent the annular spring piece from being torn and damaged due to forced grinding.

[0028] Preferably, the annular spring sheet comprises an elastically deformable annular spring sheet body, one end of the annular spring sheet body is fixedly connected to the rotating shaft, and the other end is detachably connected to a grinding block, and the end of the grinding block away from the annular spring sheet body is in contact with the inner wall of the tank. In this solution, the grinding block is used to grind the original phosphogypsum powder. After long-term use, the grinding block is severely worn and can be disassembled and replaced.

[0029] Preferably, the end face of the grinding block close to the tank body is processed into an arc surface. In this solution, when the annular spring piece rotates, the grinding block and the inner wall of the tank body will form an inclination angle. The end face of the grinding block is processed into an arc surface so that when the grinding block and the inner wall of the tank body form an inclination angle, the grinding block and the inner wall of the tank body are in line contact, so that the pressure at the contact point between the grinding block and the inner wall is the maximum, and the grinding intensity of the powder is the maximum.

[0030] Preferably, a plurality of stirring blades are installed in an equidistant circular array at one end of the rotating shaft near the bottom of the tank body, and the bottom surface of the stirring blades is arc-shaped. In this solution, the stirring blades with an arc-shaped bottom surface disturb the liquid at the bottom of the tank body to rotate and centrifuge as the rotating shaft rotates, and the liquid flows upward along the inner wall of the tank body and is ground by the annular spring.

[0031] Preferably, a tank cover is sealed and installed at the opening above the tank body, a mounting opening whose axis is consistent with the axis of the tank body is opened in the middle of the tank cover, a mounting sleeve is fixed on the upper surface of the tank cover, the mounting sleeve is coaxially arranged with the mounting opening, the rotating shaft is inserted through the mounting sleeve and is rotatably and sealedly connected with the mounting sleeve; one end of the rotating shaft extending out of the tank body is fixedly connected with a motor that drives the rotating shaft to rotate. In this solution, the mounting sleeve has a certain length, and the rotating shaft passes through the mounting sleeve to ensure that the rotating shaft and the mounting sleeve are stably coaxially arranged; the motor can drive the rotating shaft to rotate.

[0032] Preferably, a heating plate is installed at the bottom of the tank body, and a gas pressure control valve for controlling the internal pressure of the tank body is installed on the tank body cover. In this scheme, the heating plate heats the mixture of original phosphogypsum and water in the tank body. After the original phosphogypsum powder is heated, part of the original phosphogypsum can form α-type semi-hydrated phosphogypsum. α-type semi-hydrated gypsum is well-crystallized, solid, highly fluid, and requires less water. Compared with untreated original phosphogypsum, it has less impurities and stronger coagulation. At the same time, the device can heat, stir, and grind the original phosphogypsum simultaneously, combining the three steps into one and performing them simultaneously, which can improve the initialization processing efficiency of the original phosphogypsum. The gas pressure control valve can adjust the pressure inside the tank body, thereby adjusting the heating temperature of the water body on the original phosphogypsum, and controlling the speed and amount of conversion of the original phosphogypsum into semi-hydrated original phosphogypsum.

[0033] Preferably, a plurality of springs arranged vertically are fixed on the inner surface of the annular spring body, and the axis of the springs intersects with the axis of the shaft and is perpendicular to each other. In this solution, the springs are arranged to increase the strength of the annular spring and to make the grinding block on the annular spring have a greater pressure against the inner wall of the tank. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a three-dimensional structural diagram of the wet grinding device of the present invention;

[0035] Figure 2 It is a three-dimensional internal structure diagram of the wet grinding device of the present invention;

[0036] Figure 3 This is a three-dimensional structural diagram of the stirring device of the wet grinding device of the present invention.

[0037] The reference numerals in the drawings of the specification include: tank body 1, tank body cover 11, air pressure control valve 12, mounting sleeve 13, discharge valve 14, rotating shaft 21, motor 22, annular spring body 23, stirring blade 24, grinding block 231, spring 232. DETAILED DESCRIPTION

[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Embodiment 1:

[0040] A method for producing a modified phosphogypsum admixture for concrete materials comprises the following steps:

[0041] S1: By weight, 70 parts of phosphogypsum powder, 20 parts of fly ash and 9 parts of carbide slag are mixed and aged for 48 hours to obtain a modified phosphogypsum raw material;

[0042] The preparation of phosphogypsum powder comprises the following steps: putting the original phosphogypsum and water into a wet grinding device according to a weight ratio of 1:5-10, the wet grinding device synchronously stirs, grinds and heats the mixture of the original phosphogypsum and water for 10-15 minutes, the heating water temperature is 150°C, stirring, grinding, heating, centrifuging and drying, so as to obtain the phosphogypsum powder;

[0043] S3: drying the modified phosphogypsum raw material at a high temperature of 280° C., and drying the modified phosphogypsum raw material to a moisture content of 7%, thereby obtaining a modified phosphogypsum dry material;

[0044] S4: Grinding the dried modified phosphogypsum material into particles of 200 meshes using a ball mill to obtain modified phosphogypsum powder;

[0045] S5: Mix the following raw materials in proportion by weight: 0.3 part of polyaluminium, 0.4 part of calcium formate, 0.3 part of sodium silicate, 0.04 part of rubber powder, 0.09 part of cellulose ether, 0.6 part of high-efficiency water reducing agent, and the modified phosphogypsum powder obtained in step S4 to obtain modified phosphogypsum admixture for autoclaved aerated concrete blocks.

[0046] The main components of the original phosphogypsum used in this scheme are 91.3% calcium sulfate dihydrate, 3.81% phosphorus pentoxide, 38.11% sulfur trioxide, 24.46% water, and a pH value of 2.24.

[0047] The carbide slag used is a by-product of industrial production of acetylene, wherein calcium oxide is greater than 60%, silicon oxide is greater than 3.5%, aluminum oxide is greater than 2.5%, and the water content is 20-25%.

[0048] Embodiment 2:

[0049] The difference from Example 1 is that the amount of carbide slag added is 8 parts by weight;

[0050] Embodiment 3:

[0051] The difference from Example 1 is that the amount of carbide slag added is 10 parts by weight;

[0052] Embodiment 4:

[0053] Different from Example 1, the phosphogypsum powder in step S1 is prepared by the following steps: original phosphogypsum and water are put into a wet grinding device at a weight ratio of 1:10, the wet grinding device simultaneously stirs, grinds and heats the mixture of original phosphogypsum and water for 10 minutes, and then centrifuges the mixture, and dries the separated original phosphogypsum powder to obtain phosphogypsum powder.

[0054] like Figure 1-Figure 3As shown, the wet grinding device includes a tank body 1, the inner wall of the tank body 1 is roughly arranged, a tank body 1 cover is sealed and installed at the opening above the tank body 1, a mounting opening whose axis line is consistent with the axis line of the tank body 1 is opened in the middle of the tank body 1 cover, a mounting sleeve 13 is fixed on the upper surface of the tank body 1 cover, and the mounting sleeve 13 is coaxially arranged with the mounting opening; a stirring and grinding device is rotatably arranged inside the tank body 1, and the stirring and grinding device includes a rotating shaft 21, the rotating shaft 21 is inserted through the mounting sleeve 13 and is rotatably and sealedly connected with the mounting sleeve 13; one end of the rotating shaft 21 extending out of the tank body 1 is fixedly connected to a motor 22 for driving the rotating shaft 21 to rotate, and the motor 22 is fixed on the frame; and a heating plate is installed at the bottom of the tank body 1, and an air pressure control valve 12 for controlling the internal pressure of the tank body 1 is installed on the tank body 1 cover.

[0055] like Figure 2 As shown, the circumferential surface of the rotating shaft 21 is fixedly mounted with a stirring and grinding assembly arranged in an equidistant circular array, and one end of the rotating shaft 21 close to the bottom of the tank body 1 is also mounted with a plurality of stirring blades 24 in an equidistant circular array;

[0056] The bottom surface of the stirring blade 24 is arc-shaped; when the blade with the arc-shaped bottom surface rotates with the rotating shaft 21, the liquid at the bottom of the tank body 1 is disturbed to rotate and centrifuge, and flows upward along the inner wall of the tank body 1 and is ground by the annular spring sheet.

[0057] like Figure 2 and Figure 3 As shown, the stirring and grinding assembly includes an elastically deformable annular spring sheet, one end of which is fixedly connected to the rotating shaft 21, and the other end is in contact with the inside of the tank body 1; the annular spring sheet includes an annular spring sheet body 23, and three vertically arranged springs 232 are fixed on the inner surface of the annular spring sheet body 23, and the axis of the spring 232 intersects with the axis of the rotating shaft 21 and is perpendicular to each other, and the spring 232 is used to provide support for the annular spring sheet body 23; one end of the outer surface of the annular spring sheet body 23 is fixedly connected to the rotating shaft 21, and the other end is bolted to a grinding block 231, and the end of the grinding block 231 away from the annular spring sheet body 23 is connected to the rotating shaft 21. The inner wall of the tank body 1 is in contact with the grinding block 231; the grinding block 231 is used to grind the original phosphogypsum powder. After long-term use, the grinding block 231 is severely worn and can be disassembled and replaced; the end face of the grinding block 231 close to the tank body 1 is processed into a circular arc surface, and the surface of the circular arc surface is rough. When the annular spring piece rotates, the grinding block 231 and the inner wall of the tank body 1 will form an inclination angle. The end face of the grinding block 231 is processed into an arc surface, so that when the grinding block 231 and the inner wall of the tank body 1 form an inclination angle, the grinding block 231 forms a line contact with the inner wall of the tank body 1, so that the pressure at the contact point between the grinding block 231 and the inner wall is the largest, and the grinding intensity of the powder is the largest.

[0058] In this solution, the pressure inside the tank body 1 is controlled by controlling the air pressure control valve 12, thereby controlling the temperature of the water inside the tank body 1, and the temperature of the water is controlled to be 150°C.

[0059] In this scheme, the wet grinding device is used in combination with the method for producing modified phosphogypsum admixture for autoclaved aerated concrete blocks as follows:

[0060] The original phosphogypsum and water are put into the tank body 1 at a weight ratio of 1:6, and the heating plate at the bottom of the tank body 1 heats the water and the original phosphogypsum in the tank body 1. During the heating process, the motor 22 is started, and the motor 22 drives the rotating shaft 21 to start rotating, stirring the original phosphogypsum and water inside. During the stirring process, the annular spring piece presses against the inner wall of the tank body 1 to rub the original phosphogypsum, and the spring 232 increases the pressure of the annular spring piece on the inner wall of the tank body 1 and provides support force to the annular spring piece. After heating, stirring and grinding for 10 minutes, the motor 22 is turned off, the heating plate is powered off, the air pressure control valve 12 is opened, the pressure inside the tank body 1 is released, and then the discharge valve 14 at the bottom of the tank body 1 is opened to discharge the mixed liquid of water and original phosphogypsum powder from the discharge port at the bottom, and then the mixed liquid is centrifuged to obtain phosphogypsum powder.

[0061] Embodiment 5:

[0062] The difference from Example 1 is that in step S4, 8 portions of bamboo charcoal particles are further added, and the size of the bamboo charcoal particles is 150 meshes.

[0063] Comparative Example 1:

[0064] The difference from Example 1 is that the amount of carbide slag added is 7 parts by weight.

[0065] Comparative Example 2:

[0066] The difference from Example 1 is that the amount of carbide slag added is 6 parts by weight.

[0067] Comparative Example 3:

[0068] The difference from Example 1 is that the amount of carbide slag added is 5 parts by weight.

[0069] Comparative Example 4:

[0070] The difference from Example 1 is that the amount of carbide slag added is 4 parts by weight.

[0071] Comparative Example 5:

[0072] The difference from Example 1 is that the amount of carbide slag added is 11 parts by weight.

[0073] Comparative Example 6:

[0074] The difference from Example 1 is that the amount of carbide slag added is 12 parts by weight.

[0075] Comparative Example 7:

[0076] The difference from Example 1 is that the amount of carbide slag added is 13 parts by weight.

[0077] Comparative Example 8:

[0078] The difference from Example 3 is that the temperature of the water in the tank is 110°C.

[0079] Comparative Example 9:

[0080] The difference from Example 3 is that the temperature of the water in the tank is 120°C.

[0081] Comparative Example 10:

[0082] The difference from Example 3 is that the temperature of the water in the tank is 130°C.

[0083] Comparative Example 11:

[0084] The difference from Example 3 is that the temperature of the water in the tank is 140°C.

[0085] Comparative Example 12:

[0086] The difference from Example 3 is that the temperature of the water in the tank is 160°C.

[0087] Comparative Example 13:

[0088] The difference from Example 3 is that the temperature of the water in the tank is 170°C.

[0089] Comparative Example 14:

[0090] The difference from Example 3 is that the temperature of the water in the tank is 180°C.

[0091] Experimental example preparation:

[0092] S1: 70 parts of the phosphogypsum admixture in the above embodiments and comparative examples are selected, added with 30 parts of cement and 50 parts of water into a stirring device and mixed for 3 minutes to obtain a modified phosphogypsum concrete mixed slurry;

[0093] S2: diluting the composite foaming agent and water in a weight ratio of 1:30 and pouring the mixture into a foam making device to prepare foam, and then feeding the prepared foam into the modified phosphogypsum concrete slurry through a foam control system to fully mix the modified phosphogypsum foam concrete pouring slurry;

[0094] S3: The prepared modified phosphogypsum foam concrete pouring slurry is poured on site or molded through a foam concrete equipment pumping system, and naturally cured to obtain a modified phosphogypsum foam concrete block.

[0095] The modified phosphogypsum admixture of the autoclaved aerated concrete blocks of the above embodiments and comparative examples was used for concrete block casting. The modified phosphogypsum foamed concrete blocks cast were tested for cubic compressive strength according to the provisions of standard GB / T 11969. Six concrete blocks were selected for each sample for testing, and the average value of the test results was recorded as the final test value. The test values ​​are shown in Table 1:

[0096]

[0097]

[0098] Table 1

[0099] Results Analysis

[0100] 1. Generally, the concrete block has a bulk density of 700 kg per cubic meter, and the average compressive strength should not be less than 3.5 MPa. It can be seen from the compressive strength of the concrete blocks of Example 1-Example 3 and Comparative Example 1-Comparative Example 7 that when the amount of carbide slag added is 8%-10% of the total amount of the modified phosphogypsum initial material, the compressive strength is good and meets the requirements. When the amount added is less than 8 parts, the strength of the concrete block is less than 3.5 MPa, which does not meet the requirements. After continuously adding the amount of carbide slag, the compressive strength of the concrete block begins to decrease. After analysis, when the amount of carbide slag added is greater than 10%, the strength does not increase significantly, and even shows a downward trend. This may be due to the fact that carbide slag promotes the soluble phosphorus in the phosphogypsum to form more crystalline calcium phosphate, which adheres to the surface of the phosphogypsum whiskers, inhibits the growth of the phosphogypsum whiskers, thereby reducing the hydration effect of the phosphogypsum and affecting the strength of the final concrete building material;

[0101] 2. From the data of Example 4, the compressive strength of the concrete blocks made of phosphogypsum powder after heating, grinding and one-time water washing is better than the compressive strength of the concrete blocks in Example 1, which proves that heating, grinding and one-time water washing of the original phosphogypsum does have a significant promoting effect on the removal of phosphogypsum impurities and the improvement of the strength of the concrete product;

[0102] 3. According to the test data of Example 4 and Comparative Examples 8 to 14, when the temperature in the tank continues to rise to 180°C, the compressive strength of the concrete block gradually increases, proving that heating and washing the phosphogypsum can indeed remove impurities in the phosphogypsum faster and promote the conversion of the phosphogypsum into more hydratable hemihydrate phosphogypsum. However, when the temperature is greater than 150°C, the strength of the concrete block increases slightly (compared with the strength of the block at 150°C, the strength of the block at 170°C increases by 3.7%, which is almost negligible). Therefore, from the perspective of energy saving, the optimal temperature for heating the phosphogypsum is 150°C;

[0103] 4. It can be seen from the data of Example 5 that the compressive strength of the concrete block of Example 5 is better than that of Example 1, and the compressive strength improvement rate is 16.2%, which proves that adding bamboo charcoal powder to the modified phosphogypsum admixture of autoclaved aerated concrete blocks can effectively improve the strength of concrete products. It is speculated that the mechanism of improving strength is the phosphorus precipitation produced by bamboo charcoal adsorption, which prevents phosphorus precipitation from hindering the growth of phosphogypsum crystal nuclei.

[0104] The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several deformations and improvements can be made without departing from the structure of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A method for producing a modified phosphogypsum admixture for concrete materials, characterized in that: The steps include: S1: by weight, 65-80 parts of phosphogypsum powder, 15-30 parts of fly ash, and 8-10 parts of carbide slag are mixed and aged for 40-50 hours to obtain a modified phosphogypsum raw material; S2: drying the modified phosphogypsum raw material in a high temperature environment of 280-350° C., and drying the modified phosphogypsum raw material to a moisture content of 7%-8%, thereby obtaining a modified phosphogypsum dry material; S3: Grinding the dried modified phosphogypsum material into particles of 180-220 mesh using a ball mill to obtain modified phosphogypsum powder; S4: Mix the following raw materials in proportion by weight: 0.25-0.4 parts of polyaluminium, 0.3-0.5 parts of calcium formate, 0.25-0.4 parts of sodium silicate, 0.03-0.05 parts of rubber powder, 0.08-0.1 parts of cellulose ether, 0.5-0.8 parts of high-efficiency water reducing agent and 98-99 parts of modified phosphogypsum powder to obtain modified phosphogypsum admixture for autoclaved aerated concrete blocks.

2. The method for producing a modified phosphogypsum admixture for concrete materials according to claim 1, characterized in that: The preparation of phosphogypsum powder in step S1 includes the following steps: putting the original phosphogypsum and water into a wet grinding device according to a weight ratio of 1:5-10, the wet grinding device synchronously stirs and grinds the mixture of the original phosphogypsum and water for 10-15 minutes, centrifuges and dries to obtain the phosphogypsum powder.

3. The method for producing a modified phosphogypsum admixture for concrete material according to claim 2, characterized in that: The wet grinding device also heats the original phosphogypsum and water under high pressure when stirring and grinding the phosphogypsum and water, and the water temperature is 150-180°C.

4. The method for producing a modified phosphogypsum admixture for concrete materials according to claim 1, characterized in that: In the step S4, 5-10 parts of bamboo charcoal particles are also added.

5. A device for producing modified phosphogypsum admixture for concrete material, applied to a method for producing modified phosphogypsum admixture for concrete material according to claim 2, characterized in that: The invention comprises a wet grinding device, which comprises a tank body, wherein a stirring and grinding device is rotatably arranged inside the tank body, wherein the stirring and grinding device comprises a rotatable shaft, wherein stirring and grinding components arranged in an equidistant circular array are fixedly mounted on the circumferential surface of the shaft, wherein the stirring and grinding components comprise an elastically deformable annular spring piece, wherein one end of the annular spring piece is fixedly connected to the shaft, and the other end is in contact with the inside of the tank body.

6. The device for producing modified phosphogypsum admixture for concrete material according to claim 5, characterized in that: The annular spring piece comprises an elastically deformable annular spring piece body, one end of which is fixedly connected to the rotating shaft, and the other end of which is detachably connected to a grinding block, wherein one end of the grinding block away from the annular spring piece body contacts the inner wall of the tank body.

7. The device for producing modified phosphogypsum admixture for concrete material according to claim 6, characterized in that: The end surface of one end of the grinding block close to the tank body is processed into an arc surface.

8. The device for producing modified phosphogypsum admixture for concrete material according to claim 7, characterized in that: A plurality of stirring blades are installed in an equidistant circular array at one end of the rotating shaft close to the bottom of the tank body, and the bottom surface of the stirring blades is arc-shaped.

9. The device for producing modified phosphogypsum admixture for concrete material according to claim 8, characterized in that: A tank cover is sealed and installed at the opening above the tank body, and an installation opening is opened in the middle of the tank cover, whose axis line is consistent with the axis line of the tank body. A mounting sleeve is fixed on the upper surface of the tank cover, and the mounting sleeve is coaxially arranged with the mounting opening. The rotating shaft is inserted through the mounting sleeve and is rotatably and sealedly connected to the mounting sleeve; one end of the rotating shaft extending out of the tank body is fixedly connected to a motor that drives the rotating shaft to rotate.

10. The device for producing modified phosphogypsum admixture for concrete material according to claim 9, characterized in that: A heating plate is installed at the bottom of the tank body, and an air pressure control valve for controlling the internal pressure of the tank body is installed on the tank body cover; a plurality of vertically arranged springs are fixed on the inner surface of the annular spring body, and the axis of the spring intersects with the axis of the rotating shaft and is perpendicular to each other.