Large-volume hydrophobic concrete for bridge pier tower column in plateau area
By using high crack resistance and low heat silicate cement, cement-based hydrophobic materials, rice husk ash slag and carbon nanotubes in bridge pier columns in plateau areas, the freeze-thaw cycle of concrete in harsh climates is solved, and the freeze-thaw cycle of concrete is achieved. It has efficient hydrophobicity and frost resistance, and is suitable for large-area engineering applications.
Patent Information
- Application Number
- CN202410951618.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The bridge pier columns in the plateau area are susceptible to freeze-thaw cycle damage in harsh natural climates, resulting in a decrease in the durability of concrete. The existing hydrophobic agents are unevenly distributed in concrete and are harmful to the environment. The operation steps are complicated and not suitable for large-area projects. Promotion.
Large-volume hydrophobic concrete is prepared by high crack resistance and low heat silicate cement, cement-based hydrophobic materials, rice husk ash slag and carbon nanotubes. By controlling the C4AF and C3A content, the dry shrinkage is reduced, and stearic acid and cement-based materials are uniformly ground. Use rice husk ash slag and carbon nanotubes to improve hydrophobicity and frost resistance.
Effectively improve the crack resistance and hydrophobicity of concrete, reduce drying and shrinkage, enhance structural strength and stability, reduce wettability of cement slurry, and the mass loss rate is less than 5% after freeze-thaw cycle, and the mobility elasticity The modulus drop rate is not higher than 20%.
Smart Images

Figure BDA0004947386370000091 
Figure BDA0004947386370000092
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a large-volume hydrophobic concrete for bridge piers and towers in plateau areas. Background Art
[0002] my country's plateau regions have a harsh natural climate with large temperature differences between day and night, frequent snowstorms, thin air, and strong sunshine, which pose a serious threat to the durability of bridge piers and towers. The large temperature difference climate on the plateau, under the condition of the presence of free water, is very likely to cause freeze-thaw cycle damage inside the concrete. Compared with the effect of hydration rate on concrete performance, severe freeze-thaw cycle damage is the most important factor causing the reduction of concrete durability. Concrete contains a large amount of water when mixed, which participates in cement hydration and improves the workability of concrete. After the concrete hardens, the water inside the concrete exists in the pores of the concrete and migrates and exchanges with the water in the environment. In a large temperature difference environment, the free water in the pores of the concrete will freeze at temperatures below freezing, generating expansion stress, which will increase the pores of the concrete, make the structure loose, and cause the aggregate to erode and fall off from the outside to the inside, reducing the durability of the concrete.
[0003] In order to improve the frost resistance and crack resistance of concrete in plateau areas, a self-healing concrete waterproofing agent for plateau areas with application number CN202211718909.1 provides a waterproofing agent with synergistic effects of active components, reinforcing components, hydrophobic components, nano components and expansion components, so that the concrete can self-heal microcracks caused by environmental factors during service, reduce the durability problems caused by cracks, greatly improve the durability of concrete, and is suitable for the protection of concrete building materials under harsh environmental conditions in plateau high-altitude areas. However, the adhesion of the waterproofing agent to the concrete surface is low, and the waterproof layer is easy to fall off. In addition to the hydrophobic treatment of the surface of the concrete structure, there are a large number of studies on the overall hydrophobic modification of concrete. For example, by introducing fluoroalkyl silanes into the fresh cement mixture, an overall super-hydrophobic concrete with super mechanical stability is prepared. The disadvantage of this method is that fluoroalkyl silanes are expensive and harmful to the environment; the introduction of fluoroalkyl silanes will lead to a decrease in the compressive strength of concrete. In addition, when lipophilic hydrophobic substances are added to cement-based materials, due to the presence of water, lipophilic hydrophobic substances are difficult to disperse in cement-based materials. This phenomenon leads to uneven hydrophobicity of cement-based materials. Therefore, hydrophobic substances are usually dispersed in aqueous solution to make emulsions for hydrophobic modification of cement-based materials. However, this method has complicated operation steps and is not suitable for large-scale engineering promotion and application. Summary of the invention
[0004] The purpose of the present invention is to provide a large-volume hydrophobic concrete for bridge piers and towers in plateau areas. The large-volume hydrophobic concrete is prepared by using crack-resistant low-heat silicate cement, cement-based hydrophobic materials, rice husk ash and carbon nanotubes, so as to improve the durability of the bridge piers and towers in plateau areas.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] A large-volume hydrophobic concrete for bridge piers and towers in plateau areas, comprising the following raw materials by weight:
[0007] High crack resistance and low heat silicate cement: 250~350kg / m 3 ;
[0008] Cement-based hydrophobic material: 50-100 kg / m 3 ;
[0009] Rice husk ash: 5-20kg / m 3 ;
[0010] Carbon nanotubes: 0.3~1.5kg / m 3 ;
[0011] Crushed stone: 1000~1150kg / m 3 ;
[0012] Machine-made sand: 700~850kg / m 3 ;
[0013] Powdered polycarboxylate water reducer: 0.5~1.5kg / m 3 ;
[0014] Water: 130~160kg / m 3 .
[0015] Furthermore, the high crack resistance and low heat silicate cement is composed of 95 wt % of high crack resistance and low heat silicate cement clinker and 5 wt % of gypsum.
[0016] Furthermore, the clinker rate values of the high crack resistance and low heat silicate cement clinker are as follows: lime saturation coefficient: 0.80-0.88; silicon rate: 2.50-2.70; aluminum rate: 0.70-0.75.
[0017] Furthermore, in the high crack resistance and low heat silicate cement clinker, C 4 AF content greater than 17%, C 3 The A content is less than 5%, and the MgO content ranges from 2 to 5%.
[0018] Furthermore, the specific surface area of the high crack resistance and low heat silicate cement is 300-350m 2 / kg.
[0019] Furthermore, the cement-based hydrophobic material is prepared by grinding 60-80wt% of high crack-resistant low-heat silicate cement clinker, 10-20wt% of limestone, 10-20wt% of high-titanium slag, and 1-1.5wt% of stearic acid; preferably, the grinding speed is 100-150r / min, and the grinding time is 30-45min.
[0020] Furthermore, in the cement-based hydrophobic material: the content of particles with a particle size of ≤3 μm is 6-9%, the content of particles with a particle size of 3-32 μm is 73-78%, the content of particles with a particle size of 32-65 μm is 12-20%, and the content of particles with a particle size of ≥65 μm is less than 1%.
[0021] Furthermore, the cement-based hydrophobic material has a 45 μm sieve residue of 8 to 10%, a characteristic particle size of 19±0.2 μm, and a uniformity coefficient of 0.93 to 0.95.
[0022] The particle gradation curve of the cement-based hydrophobic material is close to the Fuller curve.
[0023] Furthermore, the preparation method of the rice husk ash is: placing the rice husk in a high-temperature furnace at 500-700° C. and calcining it for 1-3 minutes to obtain particles containing 10-20% carbon residue.
[0024] The rice husk ash is rich in active silicon dioxide.
[0025] Furthermore, the carbon nanotubes are multi-walled carbon nanotubes with a diameter of 8 to 15 nm and a length of 30 to 50 nm.
[0026] The carbon nanotubes have good infrared light absorption and hydrophobic properties.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] (1) By controlling the C content of high crack resistance and low heat silicate cement 4 AF and C 3 A content, thereby reducing concrete shrinkage. 4 AF has the lowest brittleness coefficient and volume shrinkage. When its content is higher than 17% in high crack resistance and low heat silicate cement, it can effectively reduce the shrinkage of concrete. 3 A has a high shrinkage deformation rate. Controlling its content below 5% can reduce the shrinkage of concrete and improve the crack resistance of concrete.
[0029] (2) Stearic acid and high crack resistance and low heat silicate cement clinker, limestone and high titanium slag are ground together to form cement-based hydrophobic materials, so that stearic acid can be evenly distributed on the surface of the material. When concrete is stirred, the cement-based hydrophobic material is evenly distributed, thereby improving the hydrophobicity of the concrete, solving the problem of uneven distribution of hydrophobic agents in concrete in the prior art. In addition, due to the addition of hydrophobic materials, the fluidity of concrete will inevitably deteriorate. For this reason, the present invention utilizes high crack resistance and low heat silicate cement clinker, high titanium slag, limestone with different grindability to prepare a hydrophobic material with a particle gradation close to the ideal distribution. Through the gradation advantage, the water demand is reduced and the mechanical properties of concrete are improved.
[0030] (3) Cement-based hydrophobic materials are filled in order according to particle size. Large particles support each other to form a skeleton, and fine particles are filled in the gaps in the skeleton of large particles. They are intertwined with each other and play a role in rolling lubrication for large particles. On the one hand, the density of cement paste can be improved. On the other hand, the amount of water used in slurry preparation can be reduced, thereby improving the stability and structural strength of cement paste and reducing the drying shrinkage value.
[0031] (4) Due to incomplete combustion of rice husk, the rice husk ash contains amorphous carbon powder, which can refine the pores of concrete, reduce the wettability of cement paste, and improve the hydrophobicity of concrete.
[0032] (5) Since cement-based hydrophobic materials, rice husk ash and carbon nanotubes are all internally mixed into concrete, if the concrete cracks, the fracture surface still has uniform hydrophobicity and moisture will not penetrate into the interior of the concrete through the cracks.
[0033] (6) Multi-walled carbon nanotubes have the ability to absorb infrared light. In winter, the carbon nanotubes inside the concrete absorb infrared rays and convert them into heat, which can increase the temperature inside the concrete and thus improve the concrete's frost resistance. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0035] Example 1
[0036] As a preferred embodiment of the present invention, a large-volume hydrophobic concrete for bridge piers and towers in plateau areas provided in this embodiment includes the following raw materials by weight:
[0037] High crack resistance and low heat silicate cement: 250kg / m3 ;
[0038] Cement-based hydrophobic material: 100kg / m 3 ;
[0039] Rice husk ash: 5kg / m 3 ;
[0040] Carbon nanotubes: 1.5kg / m 3 ;
[0041] Crushed stone: 1150kg / m 3 ;
[0042] Machine-made sand: 733kg / m 3 ;
[0043] Powdered polycarboxylate water reducer: 0.5kg / m 3 ;
[0044] Water: 160kg / m 3 .
[0045] In this embodiment, the high crack resistance and low heat silicate cement is composed of 95 wt % of high crack resistance and low heat silicate cement clinker and 5 wt % of gypsum.
[0046] Furthermore, the clinker rate values of the high crack-resistant and low-heat silicate cement clinker are: lime saturation coefficient: 0.80; silicon rate: 2.70; aluminum rate: 0.73.
[0047] Furthermore, in the high crack resistance and low heat silicate cement clinker: C 4 AF content is 18%, C 3 The A content is 1.5% and the MgO content ranges from 5%.
[0048] Furthermore, the specific surface area of high crack resistance and low heat silicate cement is 320m 2 / kg.
[0049] In this embodiment, the cement-based hydrophobic material is prepared by grinding 60wt% of high crack-resistant low-heat silicate cement clinker, 20wt% of limestone, 20wt% of high-titanium slag, and 1.5wt% of stearic acid in a ball mill at a speed of 150r / min for 30 minutes.
[0050] Furthermore, in the cement-based hydrophobic material: the content of particles with a particle size of ≤3 μm is 9%, the content of particles with a size of 3 to 32 μm is 73%, and the content of particles with a size of 32 to 65 μm is 18%.
[0051] Furthermore, the 45 μm sieve residue of the cement-based hydrophobic material is 9.2%, the characteristic particle size is 18.8 μm, and the uniformity coefficient is 0.93.
[0052] In this embodiment, the rice husk ash is prepared by placing the rice husk in a high-temperature furnace at 500° C. and calcining it for 3 minutes to obtain particles containing 10% carbon residue.
[0053] In this embodiment, the carbon nanotubes are multi-walled carbon nanotubes with a diameter of 8 nm and a length of 50 nm.
[0054] Example 2
[0055] As a preferred embodiment of the present invention, a large-volume hydrophobic concrete for bridge piers and towers in plateau areas provided in this embodiment includes the following raw materials by weight:
[0056] High crack resistance and low heat silicate cement: 350kg / m 3 ;
[0057] Cement-based hydrophobic material: 50kg / m 3 ;
[0058] Rice husk ash: 20kg / m 3 ;
[0059] Carbon nanotubes: 0.5kg / m 3 ;
[0060] Crushed stone: 1150kg / m 3 ;
[0061] Machine-made sand: 700kg / m 3 ;
[0062] Powdered polycarboxylate water reducer: 1.5kg / m 3 ;
[0063] Water: 130kg / m 3 .
[0064] In this embodiment, the high crack resistance and low heat silicate cement is composed of 95 wt % of high crack resistance and low heat silicate cement clinker and 5 wt % of gypsum.
[0065] Furthermore, the clinker rate values of the high crack-resistant and low-heat silicate cement clinker are: lime saturation coefficient: 0.85; silicon rate: 2.60; aluminum rate: 0.70.
[0066] Furthermore, in the high crack resistance and low heat silicate cement clinker: C 4 AF content is 19%, C 3 The A content is 1.0% and the MgO content ranges from 2.0%.
[0067] Furthermore, the specific surface area of high crack resistance and low heat silicate cement is 350m 2 / kg.
[0068] In this embodiment, the cement-based hydrophobic material is prepared by grinding 80wt% of high crack-resistant low-heat silicate cement clinker, 10wt% of limestone, 10wt% of high-titanium slag, and 1.0wt% of stearic acid in a ball mill at a speed of 100r / min for 45 minutes.
[0069] Furthermore, in the cement-based hydrophobic material: the content of particles with a particle size of ≤3 μm is 6%, the content of particles with a size of 3 to 32 μm is 78%, and the content of particles with a size of 32 to 65 μm is 16%.
[0070] Furthermore, the 45 μm sieve residue of the cement-based hydrophobic material is 9.8%, the characteristic particle size is 19.0 μm, and the uniformity coefficient is 0.95.
[0071] In this embodiment, the rice husk ash is prepared by placing the rice husk in a high-temperature furnace at 700° C. and calcining it for 1 minute to obtain particles containing 15% carbon residue.
[0072] In this embodiment, the carbon nanotubes are multi-walled carbon nanotubes with a diameter of 15 nm and a length of 30 nm.
[0073] Example 3
[0074] As a preferred embodiment of the present invention, a large-volume hydrophobic concrete for bridge piers and towers in plateau areas provided in this embodiment includes the following raw materials by weight:
[0075] High crack resistance and low heat silicate cement: 300kg / m 3 ;
[0076] Cement-based hydrophobic material: 75kg / m 3 ;
[0077] Rice husk ash: 13kg / m 3 ;
[0078] Carbon nanotubes: 0.9kg / m 3 ;
[0079] Crushed stone: 1000kg / m 3 ;
[0080] Machine-made sand: 850kg / m 3 ;
[0081] Powdered polycarboxylate water reducer: 1.0kg / m 3 ;
[0082] Water: 150kg / m 3 .
[0083] In this embodiment, the high crack resistance and low heat silicate cement is composed of 95 wt % of high crack resistance and low heat silicate cement clinker and 5 wt % of gypsum.
[0084] Furthermore, the clinker rate values of the high crack-resistant and low-heat silicate cement clinker are: lime saturation coefficient: 0.88; silicon rate: 2.50; aluminum rate: 0.75.
[0085] Furthermore, in the high crack resistance and low heat silicate cement clinker: C 4 AF content is 19%, C 3 The A content is 1.9% and the MgO content ranges from 3.5%.
[0086] Furthermore, the specific surface area of high crack resistance and low heat silicate cement is 330m 2 / kg.
[0087] In this embodiment, the cement-based hydrophobic material is prepared by grinding 70wt% of high crack-resistant low-heat silicate cement clinker, 15wt% of limestone, 15wt% of high-titanium slag, and 1.2wt% of stearic acid in a ball mill at a speed of 125r / min for 45 minutes.
[0088] Furthermore, in the cement-based hydrophobic material: the content of particles with a particle size of ≤3 μm is 8%, the content of particles with a particle size of 3-32 μm is 76%, the content of particles with a particle size of 32-65 μm is 15%, and the content of particles with a particle size of ≥65 μm is less than 1%.
[0089] Furthermore, the 45 μm sieve residue of the cement-based hydrophobic material is 9.0%, the characteristic particle size is 18.9 μm, and the uniformity coefficient is 0.95.
[0090] In this embodiment, the rice husk ash is prepared by placing the rice husk in a high-temperature furnace at 500° C. and calcining it for 2 minutes to obtain particles containing 20% carbon residue.
[0091] In this embodiment, the carbon nanotubes are multi-walled carbon nanotubes with a diameter of 10 nm and a length of 40 nm.
[0092] Comparative Example 1
[0093] The concrete of this comparative example includes the following raw materials by weight:
[0094] Ordinary low heat silicate cement: 250kg / m 3 ;
[0095] First-grade fly ash: 105kg / m 3 ;
[0096] Crushed stone: 1150kg / m 3 ;
[0097] Machine-made sand: 733kg / m 3 ;
[0098] Powdered polycarboxylate water reducer: 0.5kg / m 3 ;
[0099] Water: 160kg / m 3 .
[0100] In this comparative example, the ordinary low-heat Portland cement is composed of 95 wt % of ordinary low-heat Portland cement clinker and 5 wt % of gypsum.
[0101] Furthermore, the clinker rate values of ordinary low-heat Portland cement clinker are: lime saturation coefficient: 0.78; silicon rate: 2.80; aluminum rate: 0.90.
[0102] Furthermore, in ordinary low-heat Portland cement clinker: C 4 AF content is 13.9%, C 3 The A content is 3.8% and the MgO content is 1.0%.
[0103] Furthermore, the specific surface area of ordinary low-heat Portland cement is 343m 2 / kg.
[0104] Comparative Example 2
[0105] The concrete of this comparative example includes the following raw materials by weight:
[0106] Ordinary low-heat silicate cement: 350kg / m 3 ;
[0107] First-grade fly ash: 70kg / m 3 ;
[0108] Crushed stone: 1150kg / m 3 ;
[0109] Machine-made sand: 700kg / m 3 ;
[0110] Powdered polycarboxylate water reducer: 1.5kg / m 3 ;
[0111] Water: 130kg / m 3 .
[0112] In this comparative example, the ordinary low-heat Portland cement is composed of 95 wt % of ordinary low-heat Portland cement clinker and 5 wt % of gypsum.
[0113] Furthermore, the clinker rate values of ordinary low-heat Portland cement clinker are: lime saturation coefficient: 0.78; silicon rate: 2.80; aluminum rate: 0.90.
[0114] Furthermore, in ordinary low-heat Portland cement clinker: C 4AF content is 13.9%, C 3 The A content is 3.8% and the MgO content is 1.0%.
[0115] Furthermore, the specific surface area of ordinary low-heat Portland cement is 343m 2 / kg.
[0116] Comparative Example 3
[0117] The concrete of this comparative example includes the following raw materials by weight:
[0118] Ordinary low-heat silicate cement: 300kg / m 3 ;
[0119] First-grade fly ash: 89kg / m 3 ;
[0120] Crushed stone: 1000kg / m 3 ;
[0121] Machine-made sand: 850kg / m 3 ;
[0122] Powdered polycarboxylate water reducer: 1.0kg / m 3 ;
[0123] Water: 150kg / m 3 .
[0124] In this comparative example, the ordinary low-heat Portland cement is composed of 95 wt % of ordinary low-heat Portland cement clinker and 5 wt % of gypsum.
[0125] Furthermore, the clinker rate values of ordinary low-heat Portland cement clinker are: lime saturation coefficient: 0.78; silicon rate: 2.80; aluminum rate: 0.90.
[0126] Furthermore, in ordinary low-heat Portland cement clinker: C 4 AF content is 13.9%, C 3 The A content is 3.8% and the MgO content is 1.0%.
[0127] Furthermore, the specific surface area of ordinary low-heat Portland cement is 343m 2 / kg.
[0128] The concrete prepared in Examples 1 to 3 and the concrete prepared in Comparative Examples 1 to 3 were tested for basic physical and mechanical properties, hydrophobicity and frost resistance. The test results are shown in Tables 1 and 2.
[0129] Table 1 Basic physical and mechanical properties of concrete
[0130]
[0131] As can be seen from Table 1, the slump of the large-volume hydrophobic concrete prepared using high-crack-resistant low-heat silicate cement, cement-based hydrophobic materials, rice husk ash, carbon nanotubes and other materials is basically the same as that of the ordinary concrete (comparative example), but the air content is slightly increased. Under the same amount of cementitious materials, the strength of each embodiment 3d and 28d is higher than that of the corresponding comparative example.
[0132] Table 2 Concrete hydrophobicity and frost resistance
[0133]
[0134] As can be seen from Table 2, the contact angle of water droplets on the surface of large-volume hydrophobic concrete (Example) can reach more than 130°, which is super hydrophobic; while the contact angle of water droplets on the surface of ordinary concrete (Comparative Example) is about 45°, which is hydrophilic. After immersion for 1 hour, the water absorption rate of the hydrophobic concrete prepared by the present invention is only 1.5%, while the water absorption rate of ordinary concrete is as high as more than 3.5%. After 300 freeze-thaw cycles (quick freezing method), the mass loss rate of the hydrophobic concrete is less than 5%, and the dynamic elastic modulus decrease rate is not higher than 20%.
[0135] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solutions of the present invention, rather than limiting them, and certainly not limiting the patent scope of the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. In other words, any changes or modifications made to the main design concept and spirit of the present invention that have no substantive significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention. In addition, the direct or indirect application of the technical solutions of the present invention in other related technical fields is also included in the patent protection scope of the present invention.
Claims
1. A large volume hydrophobic concrete for bridge piers and towers in plateau areas, characterized in that: Includes the following weights of raw materials: High crack resistance and low heat silicate cement: 250~350kg / m 3 ; Cement-based hydrophobic material: 50-100 kg / m 3 ; Rice husk ash: 5-20kg / m 3 ; Carbon nanotubes: 0.3~1.5kg / m 3 ; Crushed stone: 1000~1150kg / m 3 ; Machine-made sand: 700~850kg / m 3 ; Powdered polycarboxylate water reducer: 0.5~1.5kg / m 3 ; Water: 130~160kg / m 3 .
2. The large-volume hydrophobic concrete for bridge piers and towers in plateau areas according to claim 1 is characterized in that: The high crack resistance and low heat silicate cement consists of 95 wt % of high crack resistance and low heat silicate cement clinker and 5 wt % of gypsum.
3. The large-volume hydrophobic concrete for bridge piers and towers in plateau areas according to claim 2 is characterized in that: The clinker rate values of the high crack resistance and low heat silicate cement clinker are as follows: lime saturation coefficient: 0.80-0.88; silicon rate: 2.50-2.70; aluminum rate: 0.70-0.
75.
4. The large-volume hydrophobic concrete for bridge piers and towers in plateau areas according to claim 2 is characterized in that: In the high crack resistance and low heat silicate cement clinker, the C4AF content is greater than 17%, the C3A content is less than 5%, and the MgO content ranges from 2 to 5%.
5. The large-volume hydrophobic concrete for bridge piers and towers in plateau areas according to claim 1 is characterized in that: The specific surface area of the high crack resistance and low heat silicate cement is 300-350m 2 / kg.
6. The large-volume hydrophobic concrete for bridge piers and towers in plateau areas according to claim 1 is characterized in that: The cement-based hydrophobic material is prepared by grinding 60-80wt% of high crack-resistant low-heat silicate cement clinker, 10-20wt% of limestone, 10-20wt% of high-titanium slag, and 1-1.5wt% of stearic acid; preferably, the grinding speed is 100-150r / min, and the grinding time is 30-45min.
7. The large-volume hydrophobic concrete for bridge piers and towers in plateau areas according to claim 1 is characterized in that: In the cement-based hydrophobic material, the content of particles with a particle size of ≤3 μm is 6-9%, the content of particles with a particle size of 3-32 μm is 73-78%, the content of particles with a particle size of 32-65 μm is 12-20%, and the content of particles with a particle size of ≥65 μm is less than 1%.
8. The large-volume hydrophobic concrete for bridge piers and towers in plateau areas according to claim 1 is characterized in that: The cement-based hydrophobic material has a 45 μm sieve residue of 8-10%, a characteristic particle size of 19±0.2 μm, and a uniformity coefficient of 0.93-0.
95.
9. The large-volume hydrophobic concrete for bridge piers and towers in plateau areas according to claim 1, characterized in that: The method for preparing the rice husk ash is as follows: placing the rice husk in a high-temperature furnace at 500-700° C. and calcining it for 1-3 minutes to obtain particles containing 10-20% carbon residue.
10. The large-volume hydrophobic concrete for bridge piers and towers in plateau areas according to claim 1, characterized in that: The carbon nanotubes are multi-walled carbon nanotubes with a diameter of 8 to 15 nm and a length of 30 to 50 nm.
Citation Information
Patent Citations
Good-fluidity composite powder for 3D (three-dimensional) printing and preparation method of composite powder
CN107805032A
Multiwalled carbon nanotube concrete
CN108558316A
Low-shrinkage anti-freezing mass concrete
CN115159923A
Low-heat low-shrinkage Portland cement and preparation method thereof
CN115784646A
Low-temperature-rise and high-crack-resistance mass concrete as well as preparation method and application thereof
CN116768557A