Recycled asphalt mixture and preparation method thereof

By introducing zinc-aluminum hydrotalcite materials and composite modified polypropylene fibers into the recycled asphalt mixture, the problems of low utilization rate, aging and environmental pollution of the recycled asphalt mixture in the prior art are solved, and its heat resistance is improved Aging and crack resistance achieve more efficient resource utilization and environmental protection effects.

CN118978812APending Publication Date: 2024-11-19QINHUANGDAO HONGYUAN ROAD & BRIDGE ENGINEERING CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411275332.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing recycled asphalt mixture has low utilization rate, aging and agglomeration, high mixing temperature, severe environmental pollution, and insufficient low-temperature crack resistance.

Method used

By pretreating the polypropylene fibers in a mixed acid solution of sulfuric acid and nitric acid, zinc-aluminum hydrotalcite material is generated and is combined with vinyl silane coupling agent, 3-allyloxy-2-hydroxy-1-propanesulfonium sulfonium Sodium acid reacts with the trifluoromethylstyrene to form composite modified polypropylene fibers and is introduced into the regenerated asphalt mixture to improve its heat aging and crack resistance.

Benefits of technology

It improves the heat-aging and low-temperature crack resistance of recycled asphalt mixture, reduces mixing temperature and energy consumption, and enhances the utilization rate and environmental friendliness of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005039990330000141
    Figure BDA0005039990330000141
Patent Text Reader

Abstract

The invention discloses a recycled asphalt mixture and a preparation method thereof.The preparation method comprises the steps that firstly, polypropylene fibers are placed in a mixed acid solution of sulfuric acid and nitric acid to be treated, the chemical activity of the polypropylene fibers is improved, and the polypropylene fibers can be better combined with subsequent hydrotalcite-like materials; then, a hydrotalcite-like compound with a layered double-metal structure is generated on the surface of the pretreated polypropylene fiber, and the zinc-aluminum hydrotalcite-like material is introduced into the recycled asphalt mixture, so that the thermal aging resistance of the recycled asphalt can be improved; according to the present invention, the modified polypropylene fiber is added to the recycled asphalt, the addition reaction between the double bonds is performed to introduce the polymer high molecular chain so as to increase the compatibility between the composite modified polypropylene fiber and the recycled asphalt, and the interaction of the 3-allyloxy-2-hydroxy-1-sodium propanesulfonate and the p-trifluoromethyl styrene jointly improves the low temperature crack resistance and the thermal aging resistance of the recycled asphalt mixture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of recycled asphalt, and in particular to a recycled asphalt mixture and a preparation method thereof. Background Art

[0002] Reclaimed Asphalt Pavement (RAP) is a building material that is made by recycling old asphalt pavement materials and reusing them in new mixtures after proper treatment. This process not only effectively utilizes existing resources, but also reduces the demand for new materials, thereby reducing the environmental burden. It is one of the important means to achieve sustainable development.

[0003] Recycled asphalt mixture mainly consists of several key parts: 1) Recycled asphalt: Recycled asphalt is an asphalt material recovered from the demolished old pavement. To ensure that the performance of recycled asphalt meets the requirements, it usually undergoes multiple processing steps such as crushing, screening and washing to remove impurities and debris and improve its usability. The properties of this material, such as adhesion, fluidity and interlayer bonding, will affect the performance of the final mixture. 2) Aggregate: Recycled asphalt mixture also contains fresh aggregate (such as sand, gravel, etc.). New aggregate provides the necessary skeleton structure and strength support, so that the mixture has sufficient bearing capacity and durability. The type, particle size distribution and quality of aggregate directly affect the final performance of recycled asphalt mixture, so they must be considered in the mix design. 3) New asphalt: Depending on the quality of recycled asphalt and the required mixture performance, a certain proportion of new asphalt is usually added. This helps to improve the fluidity, toughness and anti-aging ability of the mixture. The amount of new asphalt added depends on factors such as the characteristics of the recycled asphalt, environmental conditions and application scenarios.

[0004] The existing recycled asphalt mixture has the following problems: (1) Due to the large variability of the performance of recycled asphalt pavement materials, the proportion of recycled asphalt pavement materials is low. The specification requires that the proportion of recycled materials in the asphalt pavement surface layer should not exceed 30%, so the utilization rate of recycled asphalt pavement materials is low. The result is a large amount of piled up recycled asphalt pavement materials, which not only occupies a large amount of land, but also pollutes the environment and wastes resources. (2) Due to the aging and agglomeration of recycled asphalt mixtures, the mixing temperature of recycled asphalt mixtures is high, the mixing time is long, the heating energy consumption is large, the smoke emission of the mixing plant increases, causing environmental pollution, and excessively high mixing temperatures can easily cause secondary aging of asphalt, reducing the road performance of recycled asphalt mixtures.

[0005] For example, Chinese patent document CN202111119181.6 discloses a modified recycled asphalt mixture and its processing technology, comprising the following components in parts by weight: 50-60 parts of recycled old asphalt; 10-12 parts of new asphalt; 8-10 parts of coarse aggregate; 2-4 parts of filler; 2-3 parts of regeneration agent; 9-12 parts of hydroxymethyl polystyrene resin; 1-3 parts of diallylaminomethoxyacetanilide; 2-3 parts of guar gum; although the anti-rutting performance of the prepared asphalt mixture is improved to a certain extent, its low-temperature crack resistance still needs to be improved. Summary of the invention

[0006] In view of the deficiencies in the prior art, an object of the present invention is to provide a recycled asphalt mixture and a preparation method thereof.

[0007] In order to achieve the above object, the present invention adopts the following technical scheme:

[0008] A method for preparing a recycled asphalt mixture comprises the following steps:

[0009] S1, placing the polypropylene fiber in a mixed acid solution of sulfuric acid and nitric acid, heating and stirring, and then washing and drying to obtain pretreated polypropylene fiber;

[0010] S2, dissolving zinc nitrate, aluminum nitrate and urea in water, stirring and mixing to obtain a mixed salt solution, then adding the pretreated polypropylene fiber obtained in step S1, heating and stirring to react, and then filtering, washing and drying to obtain a composite polypropylene fiber;

[0011] S3, dispersing the composite polypropylene fiber in an ethanol aqueous solution, then adding a vinyl silane coupling agent thereto, heating to react, and after the reaction is completed, filtering, washing, and drying to obtain a double bond modified polypropylene fiber;

[0012] S4, adding the double bond modified polypropylene fiber to an organic solvent, then adding sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, p-trifluoromethylstyrene and an initiator thereto, stirring to react, and after the reaction is completed, filtering, washing and drying to obtain a composite modified polypropylene fiber;

[0013] S5. Heat the recycled asphalt to 120-130°C, add coarse aggregate and fine aggregate, stir evenly, then add mineral powder, composite modified polypropylene fiber, polyethylene wax, asphalt and epoxy soybean oil, stir evenly at 145-160°C to obtain recycled asphalt mixture.

[0014] Preferably, in step S1, the temperature of the heating and stirring treatment is 60-80°C, and the time of the heating and stirring treatment is 2-5h.

[0015] Preferably, in step S2, the mass ratio of zinc nitrate, aluminum nitrate, urea and pretreated polypropylene fiber is 1-3:1-2:3-5:5-10.

[0016] Preferably, in step S2, the temperature of the heating and stirring reaction is 80-90° C., and the time of the heating and stirring reaction is 12-18 h.

[0017] Preferably, in step S3, the mass ratio of the composite polypropylene fiber to the vinyl silane coupling agent is 5-10:1-2, wherein the vinyl silane coupling agent is selected from vinyl trimethoxy silane or vinyl triethoxy silane.

[0018] Preferably, in step S3, the heating reaction temperature is 40-60° C., and the heating reaction time is 2-4 h.

[0019] Preferably, in step S4, the mass ratio of double bond modified polypropylene fiber, sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, p-trifluoromethylstyrene and initiator is 8-12:4-6:3-5:0.5-1, and the initiator is selected from benzoyl peroxide.

[0020] Preferably, in step S4, the stirring reaction temperature is 50-70° C., and the stirring reaction time is 3-5 h.

[0021] Preferably, in step S5, the mass ratio of recovered asphalt, coarse aggregate, fine aggregate, mineral powder, composite modified polypropylene fiber, polyethylene wax, asphalt and epoxidized soybean oil is 75-85:5-10:5-10:5-10:4-6:1-2:6-12:2-4, wherein the coarse aggregate is selected from basalt crushed stone with a particle size of 15-20 mm; the fine aggregate is selected from basalt crushed stone with a particle size of 5-10 mm; and the mineral powder is selected from limestone mineral powder.

[0022] The present invention also provides a regenerated asphalt mixture prepared by the above preparation method.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The present invention first places the polypropylene fiber in a mixed acid solution of sulfuric acid and nitric acid for treatment, which can introduce different types of functional groups, such as carboxyl and hydroxyl groups, on the surface of the polypropylene fiber. The introduction of these functional groups can improve the chemical activity of the polypropylene fiber, so that it can better combine with the subsequent hydrotalcite-like material.

[0025] (2) The present invention generates a layered bimetallic hydrotalcite compound on the surface of the pretreated polypropylene fiber. The zinc-aluminum hydrotalcite material has a relatively large specific surface area and excellent heat and oxygen barrier properties. Introducing the zinc-aluminum hydrotalcite material into the regenerated asphalt mixture can improve the heat aging resistance of the regenerated asphalt.

[0026] (3) In order to improve the compatibility between the composite polypropylene fiber and the recycled asphalt, the present invention first uses a vinyl silane coupling agent to treat the composite polypropylene fiber to obtain a double-bond modified polypropylene fiber, and then reacts with 3-allyloxy-2-hydroxy-1-propanesulfonate sodium and trifluoromethylstyrene through an addition reaction between double bonds to obtain a composite modified polypropylene fiber; by introducing a polymer high molecular chain, the compatibility between the composite modified polypropylene fiber and the recycled asphalt is increased. At the same time, 3-allyloxy-2-hydroxy-1-propanesulfonate sodium contains a sulfonic acid group, which can interact well with the filler, promote the uniform dispersion of the filler in the asphalt, enhance the bonding performance between the filler and the asphalt, and thus improve the crack resistance of the recycled asphalt; trifluoromethylstyrene contains a benzene ring and a fluorine group, which can improve the crack resistance of asphalt under low temperature conditions and the thermal aging performance under high temperature. 3-allyloxy-2-hydroxy-1-propanesulfonate sodium and trifluoromethylstyrene interact with each other to jointly improve the low-temperature crack resistance and heat aging resistance of the recycled asphalt mixture. DETAILED DESCRIPTION

[0027] The present invention is further described in detail below through specific preferred embodiments, but the present invention is not limited to the following embodiments.

[0028] It should be noted that, unless otherwise specified, the chemical reagents involved in the present invention were purchased through commercial channels.

[0029] A method for preparing a recycled asphalt mixture comprises the following steps:

[0030] S1. Preparation of pretreated polypropylene fibers

[0031] The polypropylene fiber is placed in a mixed acid solution of sulfuric acid and nitric acid, heated and stirred, and then washed and dried to obtain the pretreated polypropylene fiber.

[0032] In this step, the usage ratio of the polypropylene fiber and the mixed acid solution is 10-15 g: 100-150 mL, the concentration of sulfuric acid in the mixed acid solution is 2-4 mol / L, and the concentration of nitric acid is 1-2 mol / L.

[0033] In this step, the temperature for heating and stirring treatment is 60-80°C, for example, 60°C, 65°C, 70°C, 75°C, and 80°C can be selected; the time for heating and stirring treatment is 2-5h, for example, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, and 5h can be selected; but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0034] In this step, by treating the polypropylene fiber in a mixed acid solution of sulfuric acid and nitric acid, different types of functional groups, such as carboxyl and hydroxyl groups, can be introduced onto the surface of the polypropylene fiber. The introduction of these functional groups can improve the chemical activity of the polypropylene fiber, enabling it to better combine with the subsequent hydrotalcite-like material.

[0035] S2. Preparation of composite polypropylene fibers

[0036] Dissolve zinc nitrate, aluminum nitrate and urea in water, stir and mix evenly to obtain a mixed salt solution, then add the pretreated polypropylene fiber obtained in step S1, heat and stir to react, then filter, wash and dry to obtain composite polypropylene fiber.

[0037] In this step, the mass ratio of zinc nitrate, aluminum nitrate, urea and pretreated polypropylene fiber is 1-3:1-2:3-5:5-10.

[0038] The temperature of the heating and stirring reaction is 80-90°C, for example, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C, and 90°C can be selected; the time of the heating and stirring reaction is 12-18h, for example, 12h, 13h, 14h, 15h, 16h, 17h, and 18h ​​can be selected; but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0039] In this step, a layered bimetallic hydrotalcite compound is generated on the surface of the pretreated polypropylene fiber. The zinc-aluminum hydrotalcite material has a relatively large specific surface area and excellent heat and oxygen barrier properties. Introducing the zinc-aluminum hydrotalcite material into the recycled asphalt mixture can improve the aging resistance of the recycled asphalt.

[0040] S3. Preparation of double bond modified polypropylene fiber

[0041] The composite polypropylene fiber is dispersed in an ethanol aqueous solution, and then a vinyl silane coupling agent is added thereto for heating reaction. After the reaction is completed, the composite polypropylene fiber is filtered, washed and dried to obtain a double-bond modified polypropylene fiber.

[0042] In this step, the mass ratio of the composite polypropylene fiber and the vinyl silane coupling agent is 5-10:1-2, for example, 5:1, 5:1.5, 5:2, 6:1, 6:2, 8:1, 8:2, 10:1, 10:2 can be selected, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable.

[0043] Wherein, the vinyl silane coupling agent is selected from vinyl trimethoxy silane or vinyl triethoxy silane.

[0044] In this step, the temperature of the heating reaction is 40-60°C, for example, 40°C, 45°C, 50°C, 55°C, and 60°C can be selected; the time of the heating reaction is 2-4h, for example, 2h, 2.5h, 3h, 3.5h, and 4h can be selected, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0045] In this step, the composite polypropylene fiber is treated with a vinyl silane coupling agent to obtain a double-bond modified polypropylene fiber, and carbon-carbon double bonds are introduced on the surface of the composite polypropylene fiber to facilitate subsequent reactions.

[0046] S4. Preparation of composite modified polypropylene fiber

[0047] The double bond modified polypropylene fiber is added into an organic solvent, and then sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, p-trifluoromethylstyrene and an initiator are added thereto, and the mixture is stirred for reaction. After the reaction is completed, the mixture is filtered, washed and dried to obtain a composite modified polypropylene fiber.

[0048] In this step, the mass ratio of double bond modified polypropylene fiber, sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, p-trifluoromethylstyrene and initiator is 8-12:4-6:3-5:0.5-1.

[0049] Wherein, the initiator is selected from benzoyl peroxide.

[0050] In this step, the stirring reaction temperature is 50-70°C, for example, 50°C, 55°C, 60°C, 65°C, 70°C, etc.; the stirring reaction time is 3-5h, for example, 3h, 3.5h, 4h, 4.5h, 5h can be selected; but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0051] In this step, a composite modified polypropylene fiber is obtained by an addition reaction between double bond modified polypropylene fiber, sodium 3-allyloxy-2-hydroxy-1-propanesulfonate and trifluoromethylstyrene; the compatibility between the composite modified polypropylene fiber and the recycled asphalt is increased by introducing a polymer high molecular chain; at the same time, sodium 3-allyloxy-2-hydroxy-1-propanesulfonate contains a sulfonic acid group, which can interact well with the filler, promote the uniform dispersion of the filler in the asphalt, enhance the bonding performance between the filler and the asphalt, and thus improve the anti-cracking performance of the recycled asphalt; trifluoromethylstyrene contains benzene rings and fluorine groups, which can improve the anti-cracking performance of asphalt under low temperature conditions and the thermal aging performance under high temperature; sodium 3-allyloxy-2-hydroxy-1-propanesulfonate and trifluoromethylstyrene interact with each other, and jointly improve the low-temperature anti-cracking performance and aging resistance of the recycled asphalt mixture.

[0052] S5. Preparation of recycled asphalt mixture

[0053] Heat the recycled asphalt to 120-130°C, add coarse aggregate and fine aggregate, stir evenly, then add mineral powder, composite modified polypropylene fiber, polyethylene wax, asphalt and epoxy soybean oil, stir evenly at 145-160°C to obtain recycled asphalt mixture.

[0054] In this step, the mass ratio of recovered asphalt, coarse aggregate, fine aggregate, mineral powder, composite modified polypropylene fiber, polyethylene wax, asphalt and epoxidized soybean oil is 75-85:5-10:5-10:5-10:4-6:1-2:6-12:2-4.

[0055] Wherein, the coarse aggregate is selected from basalt crushed stone with a particle size of 15-20 mm.

[0056] The fine aggregate is selected from basalt crushed stone with a particle size of 5-10 mm.

[0057] The mineral powder is selected from limestone mineral powder.

[0058] The present invention is further illustrated by specific embodiments below, wherein polypropylene fiber is purchased from Shandong Tonghui Glass Fiber Co., Ltd., with a length of 3-5 mm; recycled asphalt: recycled A-70 asphalt obtained after separation of old asphalt material: needle penetration 25℃ / 0.1mm: 48.7, softening point / ℃: 63.1, elongation / cm: 18, 135℃ dynamic viscosity / Pa·s: 1.27; asphalt: A-70 asphalt; limestone ore powder: mesh number 400 mesh; polyethylene wax is purchased from Shandong Baolilai Plastic Additive Co., Ltd.; epoxidized soybean oil CAS number: 8013-07-8.

[0059] Example 1

[0060] A method for preparing a recycled asphalt mixture comprises the following steps:

[0061] S1. 10 g of polypropylene fiber was placed in 100 mL of a mixed acid solution of sulfuric acid and nitric acid, wherein the concentration of the sulfuric acid was 2 mol / L and the concentration of the nitric acid was 1 mol / L, and the mixture was heated and stirred at 60° C. for 5 h, and then washed and dried to obtain pretreated polypropylene fiber;

[0062] S2, dissolving 2g zinc nitrate, 1g aluminum nitrate and 3g urea in 100mL water, stirring and mixing to obtain a mixed salt solution, then adding 8g pretreated polypropylene fiber obtained in step S1, heating and stirring at 80°C for 18h, then filtering, washing and drying to obtain composite polypropylene fiber;

[0063] S3, dispersing 8 g of composite polypropylene fiber in 100 mL of 80 wt% ethanol aqueous solution, then adding 1 g of vinyltrimethoxysilane thereto, heating at 40° C. for 4 h, and after the reaction is completed, filtering, washing, and drying to obtain double bond modified polypropylene fiber;

[0064] S4, adding 8 g of double bond modified polypropylene fiber into 150 mL of organic solvent DMF, and then adding 4 g of sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, 3 g of p-trifluoromethylstyrene and 0.5 g of initiator benzoyl peroxide thereto, stirring and reacting at 60° C. for 5 h, after the reaction is completed, filtering, washing and drying to obtain a composite modified polypropylene fiber;

[0065] S5. Heat 75 parts of recycled asphalt to 120°C, add 8 parts of coarse aggregate and 5 parts of fine aggregate, stir evenly, then add 6 parts of mineral powder, 4 parts of composite modified polypropylene fiber, 2 parts of polyethylene wax, 8 parts of asphalt and 3 parts of epoxidized soybean oil, stir evenly at 145°C to obtain a recycled asphalt mixture.

[0066] Example 2

[0067] A method for preparing a recycled asphalt mixture comprises the following steps:

[0068] S1. Place 15 g of polypropylene fiber in 150 mL of a mixed acid solution of sulfuric acid and nitric acid, wherein the concentration of the sulfuric acid is 4 mol / L and the concentration of the nitric acid is 2 mol / L, and heat and stir at 80° C. for 2 h, and then wash and dry to obtain pretreated polypropylene fiber;

[0069] S2, dissolving 3g zinc nitrate, 2g aluminum nitrate and 5g urea in 100mL water, stirring and mixing to obtain a mixed salt solution, then adding 10g pretreated polypropylene fiber obtained in step S1, heating and stirring at 90°C for 12h, then filtering, washing and drying to obtain composite polypropylene fiber;

[0070] S3, dispersing 10 g of composite polypropylene fiber in 100 mL of 80 wt% ethanol aqueous solution, then adding 2 g of vinyltrimethoxysilane thereto, heating at 60° C. for reaction for 2 h, and after the reaction is completed, filtering, washing, and drying to obtain double bond modified polypropylene fiber;

[0071] S4, adding 12g of double bond modified polypropylene fiber into 150mL of organic solvent DMF, and then adding 6g of sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, 5g of p-trifluoromethylstyrene and 1g of initiator benzoyl peroxide thereto, stirring and reacting at 70°C for 3h, after the reaction is completed, filtering, washing and drying to obtain composite modified polypropylene fiber;

[0072] S5. Heat 85 parts of recycled asphalt to 120°C, add 10 parts of coarse aggregate and 6 parts of fine aggregate, stir evenly, then add 8 parts of mineral powder, 6 parts of composite modified polypropylene fiber, 1 part of polyethylene wax, 10 parts of asphalt and 4 parts of epoxidized soybean oil, stir evenly at 145°C to obtain a recycled asphalt mixture.

[0073] Example 3

[0074] A method for preparing a recycled asphalt mixture comprises the following steps:

[0075] S1. 12 g of polypropylene fiber was placed in a mixed acid solution of 150 mL of sulfuric acid and nitric acid, wherein the concentration of sulfuric acid was 2 mol / L and the concentration of nitric acid was 2 mol / L, and heated and stirred at 75° C. for 3 h, and then washed and dried to obtain pretreated polypropylene fiber;

[0076] S2, dissolving 2g of zinc nitrate, 2g of aluminum nitrate and 4g of urea in 100mL of water, stirring and mixing to obtain a mixed salt solution, then adding 8g of the pretreated polypropylene fiber obtained in step S1, heating and stirring at 85°C for 15h, then filtering, washing and drying to obtain a composite polypropylene fiber;

[0077] S3, dispersing 8 g of composite polypropylene fiber in 100 mL of 80 wt% ethanol aqueous solution, then adding 2 g of vinyl triethoxysilane thereto, heating at 50° C. for reaction for 3 h, and after the reaction is completed, filtering, washing, and drying to obtain double bond modified polypropylene fiber;

[0078] S4, adding 10g of double bond modified polypropylene fiber to 150mL of organic solvent DMF, then adding 5g of sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, 4g of trifluoromethylstyrene and 0.8g of initiator benzoyl peroxide, stirring and reacting at 65°C for 4h, after the reaction is completed, filtering, washing and drying to obtain composite modified polypropylene fiber;

[0079] S5. Heat 80 parts of recycled asphalt to 130°C, add 8 parts of coarse aggregate and 8 parts of fine aggregate, stir evenly, then add 10 parts of mineral powder, 5 parts of composite modified polypropylene fiber, 2 parts of polyethylene wax, 12 parts of asphalt and 3 parts of epoxidized soybean oil, stir evenly at 145°C to obtain a recycled asphalt mixture.

[0080] Example 4

[0081] A method for preparing a recycled asphalt mixture comprises the following steps:

[0082] S1. Place 15 g of polypropylene fiber in 150 mL of a mixed acid solution of sulfuric acid and nitric acid, wherein the concentration of the sulfuric acid is 2 mol / L and the concentration of the nitric acid is 2 mol / L, and heat and stir at 75° C. for 3 h, and then wash and dry to obtain pretreated polypropylene fiber;

[0083] S2, dissolving 3g zinc nitrate, 2g aluminum nitrate and 5g urea in 100mL water, stirring and mixing to obtain a mixed salt solution, then adding 6g pretreated polypropylene fiber obtained in step S1, heating and stirring at 85°C for 15h, then filtering, washing and drying to obtain composite polypropylene fiber;

[0084] S3, dispersing 6 g of composite polypropylene fiber in 100 mL of 80 wt% ethanol aqueous solution, then adding 1.5 g of vinyl triethoxysilane thereto, heating at 45° C. for reaction for 3 h, and after the reaction is completed, filtering, washing, and drying to obtain double bond modified polypropylene fiber;

[0085] S4, adding 10g of double bond modified polypropylene fiber to 150mL of organic solvent DMF, then adding 6g of sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, 5g of p-trifluoromethylstyrene and 1g of initiator benzoyl peroxide, stirring and reacting at 50°C for 5h, after the reaction is completed, filtering, washing and drying to obtain composite modified polypropylene fiber;

[0086] S5. Heat 82 parts of recycled asphalt to 125°C, add 6 parts of coarse aggregate and 10 parts of fine aggregate, stir evenly, then add 8 parts of mineral powder, 5 parts of composite modified polypropylene fiber, 1.5 parts of polyethylene wax, 8 parts of asphalt and 2 parts of epoxidized soybean oil, stir evenly at 145°C to obtain a recycled asphalt mixture.

[0087] Comparative Example 1

[0088] A method for preparing a recycled asphalt mixture comprises the following steps:

[0089] S1. 10 g of polypropylene fiber was placed in 100 mL of a mixed acid solution of sulfuric acid and nitric acid, wherein the concentration of the sulfuric acid was 2 mol / L and the concentration of the nitric acid was 1 mol / L, and the mixture was heated and stirred at 60° C. for 5 h, and then washed and dried to obtain pretreated polypropylene fiber;

[0090] S2, dispersing 8 g of pretreated polypropylene fiber in 100 mL of 80 wt% ethanol aqueous solution, then adding 1 g of vinyltrimethoxysilane thereto, heating at 40° C. for 4 h, and after the reaction is completed, filtering, washing, and drying to obtain double bond modified polypropylene fiber;

[0091] S3, adding 8 g of double bond modified polypropylene fiber into 150 mL of organic solvent DMF, and then adding 4 g of sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, 3 g of p-trifluoromethylstyrene and 0.5 g of initiator benzoyl peroxide thereto, stirring and reacting at 60° C. for 5 h, after the reaction is completed, filtering, washing and drying to obtain a composite modified polypropylene fiber;

[0092] S4. Heat 75 parts of recycled asphalt to 120°C, add 8 parts of coarse aggregate and 5 parts of fine aggregate, stir evenly, then add 6 parts of mineral powder, 4 parts of composite modified polypropylene fiber, 2 parts of polyethylene wax, 8 parts of asphalt and 3 parts of epoxidized soybean oil, stir evenly at 145°C to obtain a recycled asphalt mixture.

[0093] Compared with Example 1, in Comparative Example 1, no zinc-aluminum hydrotalcite was loaded on the pretreated polypropylene fiber.

[0094] Comparative Example 2

[0095] A method for preparing a recycled asphalt mixture comprises the following steps:

[0096] S1. 10 g of polypropylene fiber was placed in 100 mL of a mixed acid solution of sulfuric acid and nitric acid, wherein the concentration of the sulfuric acid was 2 mol / L and the concentration of the nitric acid was 1 mol / L, and the mixture was heated and stirred at 60° C. for 5 h, and then washed and dried to obtain pretreated polypropylene fiber;

[0097] S2, dissolving 2g zinc nitrate, 1g aluminum nitrate and 3g urea in 100mL water, stirring and mixing to obtain a mixed salt solution, then adding 8g pretreated polypropylene fiber obtained in step S1, heating and stirring at 80°C for 18h, then filtering, washing and drying to obtain composite polypropylene fiber;

[0098] S3, dispersing 8 g of composite polypropylene fiber in 100 mL of 80 wt% ethanol aqueous solution, then adding 1 g of vinyltrimethoxysilane thereto, heating at 40° C. for 4 h, and after the reaction is completed, filtering, washing, and drying to obtain double bond modified polypropylene fiber;

[0099] S4, adding 8 g of double bond modified polypropylene fiber to 150 mL of organic solvent DMF, then adding 3 g of p-trifluoromethylstyrene and 0.5 g of initiator benzoyl peroxide, stirring and reacting at 60° C. for 5 h, after the reaction is completed, filtering, washing and drying to obtain composite modified polypropylene fiber;

[0100] S5. Heat 75 parts of recycled asphalt to 120°C, add 8 parts of coarse aggregate and 5 parts of fine aggregate, stir evenly, then add 6 parts of mineral powder, 4 parts of composite modified polypropylene fiber, 2 parts of polyethylene wax, 8 parts of asphalt and 3 parts of epoxidized soybean oil, stir evenly at 145°C to obtain a recycled asphalt mixture.

[0101] Compared with Example 1, Comparative Example 2 did not add sodium 3-allyloxy-2-hydroxy-1-propanesulfonate.

[0102] Comparative Example 3

[0103] A method for preparing a recycled asphalt mixture comprises the following steps:

[0104] S1. 10 g of polypropylene fiber was placed in 100 mL of a mixed acid solution of sulfuric acid and nitric acid, wherein the concentration of the sulfuric acid was 2 mol / L and the concentration of the nitric acid was 1 mol / L, and the mixture was heated and stirred at 60° C. for 5 h, and then washed and dried to obtain pretreated polypropylene fiber;

[0105] S2, dissolving 2g zinc nitrate, 1g aluminum nitrate and 3g urea in 100mL water, stirring and mixing to obtain a mixed salt solution, then adding 8g pretreated polypropylene fiber obtained in step S1, heating and stirring at 80°C for 18h, then filtering, washing and drying to obtain composite polypropylene fiber;

[0106] S3, dispersing 8 g of composite polypropylene fiber in 100 mL of 80 wt% ethanol aqueous solution, then adding 1 g of vinyltrimethoxysilane thereto, heating at 40° C. for 4 h, and after the reaction is completed, filtering, washing, and drying to obtain double bond modified polypropylene fiber;

[0107] S4, adding 8 g of double bond modified polypropylene fiber into 150 mL of organic solvent DMF, then adding 4 g of sodium 3-allyloxy-2-hydroxy-1-propanesulfonate and 0.5 g of initiator benzoyl peroxide thereto, stirring and reacting at 60° C. for 5 h, after the reaction is completed, filtering, washing and drying to obtain composite modified polypropylene fiber;

[0108] S5. Heat 75 parts of recycled asphalt to 120°C, add 8 parts of coarse aggregate and 5 parts of fine aggregate, stir evenly, then add 6 parts of mineral powder, 4 parts of composite modified polypropylene fiber, 2 parts of polyethylene wax, 8 parts of asphalt and 3 parts of epoxidized soybean oil, stir evenly at 145°C to obtain a recycled asphalt mixture.

[0109] Compared with Example 1, Comparative Example 3 does not add trifluoromethylstyrene.

[0110] The regenerated asphalt mixtures prepared in Examples 1-4 and Comparative Examples 1-3 were tested according to the standards of "Testing Procedures for Asphalt and Asphalt Mixtures for Highway Engineering" (JTGE 20-2011);

[0111] The test results are shown in the following table:

[0112]

[0113] Finally, it should be noted that the above embodiments do not limit the present invention in any form. For those skilled in the art, some modifications and improvements can be made to the present invention. Therefore, any modification or improvement made without departing from the spirit of the present invention belongs to the scope of protection claimed in the present invention.

Claims

1. A method for preparing a recycled asphalt mixture, It is characterized in that The steps include: S1, placing the polypropylene fiber in a mixed acid solution of sulfuric acid and nitric acid, heating and stirring, and then washing and drying to obtain pretreated polypropylene fiber; S2, dissolving zinc nitrate, aluminum nitrate and urea in water, stirring and mixing to obtain a mixed salt solution, then adding the pretreated polypropylene fiber obtained in step S1, heating and stirring to react, and then filtering, washing and drying to obtain a composite polypropylene fiber; S3, dispersing the composite polypropylene fiber in an ethanol aqueous solution, then adding a vinyl silane coupling agent thereto, heating to react, and after the reaction is completed, filtering, washing, and drying to obtain a double bond modified polypropylene fiber; S4, adding the double bond modified polypropylene fiber to an organic solvent, then adding sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, p-trifluoromethylstyrene and an initiator thereto, stirring to react, and after the reaction is completed, filtering, washing and drying to obtain a composite modified polypropylene fiber; S5. Heat the recycled asphalt to 120-130°C, add coarse aggregate and fine aggregate, stir evenly, then add mineral powder, composite modified polypropylene fiber, polyethylene wax, asphalt and epoxy soybean oil, stir evenly at 145-160°C to obtain recycled asphalt mixture.

2. The preparation method according to claim 1, It is characterized in that In step S1, the temperature of the heating and stirring treatment is 60-80°C, and the time of the heating and stirring treatment is 2-5h.

3. The preparation method according to claim 1, It is characterized in that In step S2, the mass ratio of zinc nitrate, aluminum nitrate, urea and pretreated polypropylene fiber is 1-3:1-2:3-5:5-10.

4. The preparation method according to claim 1, It is characterized in that In step S2, the temperature of the heating and stirring reaction is 80-90° C., and the time of the heating and stirring reaction is 12-18 hours.

5. The preparation method according to claim 1, It is characterized in that In step S3, the mass ratio of the composite polypropylene fiber to the vinyl silane coupling agent is 5-10:1-2, wherein the vinyl silane coupling agent is selected from vinyl trimethoxy silane or vinyl triethoxy silane.

6. The preparation method according to claim 1, It is characterized in that In step S3, the heating reaction temperature is 40-60° C., and the heating reaction time is 2-4 hours.

7. The preparation method according to claim 1, It is characterized in that In step S4, the mass ratio of double bond modified polypropylene fiber, sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, p-trifluoromethylstyrene and initiator is 8-12:4-6:3-5:0.5-1, and the initiator is selected from benzoyl peroxide.

8. The preparation method according to claim 1, It is characterized in that In step S4, the stirring reaction temperature is 50-70° C., and the stirring reaction time is 3-5 h.

9. The preparation method according to claim 1, It is characterized in that In step S5, the mass ratio of recovered asphalt, coarse aggregate, fine aggregate, mineral powder, composite modified polypropylene fiber, polyethylene wax, asphalt and epoxidized soybean oil is 75-85:5-10:5-10:5-10:4-6:1-2:6-12:2-4, wherein the coarse aggregate is selected from basalt crushed stone with a particle size of 15-20 mm; the fine aggregate is selected from basalt crushed stone with a particle size of 5-10 mm; and the mineral powder is selected from limestone mineral powder.

10. The regenerated asphalt mixture prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Hot-mixed recycled asphalt mixture containing modified reinforcing agent and preparation process of hot-mixed recycled asphalt mixture

    CN120887676A

  • Natural asphalt-doped recycled asphalt mixture and preparation method thereof

    CN122355618A

  • A recycled asphalt mixture doped with natural asphalt and a method for preparing the same