Thermal shock resistant and wear resistant castable and preparation method thereof
Through the combination of modified steel fibers and homemade water reducing agents, the problem of insufficient thermal shock and flexural strength of refractory castables is solved, which significantly improves thermal shock resistance and flow performance, extends service life and reduces safety risks .
Patent Information
- Application Number
- CN202411019870.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-22
AI Technical Summary
The existing refractory castables have poor thermal shock, flush resistance, compressive strength, wear resistance and peel resistance, resulting in a short service life and safety risks.
Using a preparation method of thermal shock-resistant wear-resistant castable material, by using silica micropowder, mullite particles, silicon carbide powder and modified steel fiber as matrix materials, gypsum, aluminum micropowder, silicon micropowder, aluminate salts Cement and homemade water reducing agent are aggregates, and water is added to cure after mixing. The modified steel fibers are treated with zinc sulfate and coated with micro-nanoflake zinc phosphate to form a network structure to improve thermal shock resistance.
It significantly improves thermal shock resistance and flexural strength, extends service life, reduces safety risks, and enhances the flow performance of the castable material.
Abstract
Description
Technical Field
[0001] The invention relates to the field of amorphous refractory materials, in particular to a heat-shock-resistant and wear-resistant castable and a preparation method thereof. Background Art
[0002] Unshaped refractory materials have the advantages of low investment, low energy consumption, good thermal shock stability after being prepared into an integral lining, good air tightness, and the ability to repair the furnace lining. Therefore, compared with shaped refractory materials such as refractory bricks, they are more widely used. Castables belong to unshaped refractory materials and are mainly used in blast furnaces, hot blast furnaces, incinerators, cement preparation and other fields. They can also be used to construct integral structures such as heating furnace linings. At present, the commonly used refractory castables in industry mainly include aluminate castables, water glass castables and phosphate castables.
[0003] However, with the use of castables in the prior art, the corresponding defects of castables have gradually emerged, such as poor thermal shock resistance and erosion resistance, resulting in a short service life, and easy cracking and collapse during use, large changes in thermal shrinkage, which makes the application process have great safety risks; and these defects are caused by the poor erosion resistance, compressive strength, wear resistance, thermal shock resistance and spalling resistance of the castable. Therefore, it is an urgent problem for those skilled in the art to study and prepare a castable that is resistant to thermal shock and wear. Summary of the invention
[0004] The object of the present invention is to provide a heat-shock-resistant and wear-resistant castable and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a thermal shock resistant and wear resistant castable, which is prepared by adding water to a mixture, stirring evenly and then solidifying; the mixture comprises a matrix material and an aggregate; the matrix material comprises silica powder, mullite particles, silicon carbide powder and modified steel fiber; the aggregate comprises gypsum, aluminum powder, silicon powder, aluminate cement, sodium hexametaphosphate and a homemade water reducer.
[0006] Preferably, the iron oxide content in the mullite particles is 1-1.2% and the particle size is 6-8 mm.
[0007] Preferably, the particle size of the silicon dioxide powder is 8-10 mm, the particle size of the silicon carbide powder is 6-8 mm, the particle size of the aluminum powder is 6-8 mm, and the particle size of the silicon powder is 6-8 mm.
[0008] Preferably, the modified steel fiber is prepared by treating the steel fiber with zinc sulfate and then coating the surface of the steel fiber with polydopamine to form micro-nano flaky zinc phosphate; the length of the modified steel fiber is 4 to 6 mm.
[0009] Preferably, the homemade water reducer is a modified polyurethane; the modified polyurethane is prepared by polycondensing dimethylolbutyric acid, hydroxyl monomers of polyethylene glycol ether and isocyanate monomers to form a long-chain polyurethane, which is then cross-linked with a terminal hydroxyl hyperbranched polyester.
[0010] Preferably, the method for preparing the thermal shock resistant and wear resistant castable comprises the following specific steps: S1. Mix zinc oxide, 70-80% by mass phosphoric acid, citric acid, calcium nitrate, zinc nitrate and deionized water in a mass ratio of 5-8:30:1:20:20:100, heat to 72-77°C, immerse the steel fiber, phosphate for 15-25 minutes, filter and wash with deionized water for 3-5 times, and dry to obtain a modified steel fiber base material; S2. 3-5 g / L dopamine solution and micro-nano flaky zinc phosphate were mixed in a mass ratio of 20-30:1-6, the pH was adjusted to 7.6-7.8 with tris(hydroxymethyl)aminomethane, 6-10 times the mass of micro-nano flaky zinc phosphate was added to the modified steel fiber base material, and the mixture was soaked for 6-12 hours, filtered and rinsed with deionized water, and dried after water control to obtain modified steel fiber; S3. A polyethylene glycol ether with a molecular weight of 350, toluene diisocyanate and dimethylolbutyric acid are mixed in a mass ratio of 1:5:0.08~0.12, the temperature is raised to 60~65°C, dibutyltin dilaurate is added in an amount of 0.03~0.06 times the mass of toluene diisocyanate, the temperature is raised to 83~85°C, the mixture is stirred at 200~400rpm for reaction for 3~5h, the temperature is lowered to 38~42°C, acetone in an amount of 2~4 times the mass of toluene diisocyanate and a terminal hydroxyl hyperbranched polyester in an amount of 0.2~0.6 times the mass of toluene diisocyanate are added, the temperature is raised to 90~92°C, the mixture is stirred at 200~400rpm for reaction for 2~4h, and a modified polyurethane is obtained, which is a homemade water reducing agent; S4. The silica powder, mullite particles, silicon carbide powder and modified steel fiber are mixed to obtain a matrix material; gypsum, aluminum powder, silica powder, aluminate cement, sodium hexametaphosphate and a homemade water reducing agent are mixed to obtain an aggregate; S5. The matrix material and the aggregate are mixed in a mass ratio of 1:1-1.5 to obtain a mixture, and the mixture is mixed with water in a mass ratio of 20:0.9-1.1 to solidify to obtain a heat-shock-resistant and wear-resistant castable.
[0011] Preferably, in the above step S2., the preparation method of micro-nano flaky zinc phosphate is: ammonium carbonate, 5-8% ammonia water and zinc oxide are mixed in a mass ratio of 5:20:1-2, stirred to dissolve and then filtered, heated to 50-80°C, magnetically stirred at 200-400rpm for 4-6h, added with 4-6 times the total volume of deionized water, aged for 4-6h, filtered and washed with deionized water for 3-5 times, then added with 4-6 times the mass of ammonium carbonate and a mass fraction of 20-40% ethanol solution, stirred evenly, and then added dropwise with 0.2-0.4 times the mass of ammonium carbonate phosphoric acid at a rate of 1-3ml / min, reacted at room temperature for 25-35min, filtered with a circulating water vacuum pump, and finally dried and ground to obtain micro-nano flaky zinc phosphate.
[0012] Preferably, in the above step S3., the preparation method of the terminal hydroxyl hyperbranched polyester is: under a nitrogen atmosphere, 2,2-dihydroxymethylpropionic acid, trimethylolpropane and catalyst p-toluenesulfonic acid are mixed in a mass ratio of 40:13:0.1~0.2, the temperature is raised to 135~145°C, refluxed for 2~4h, and then 6~8 times the mass of trimethylolpropane 2,2-dihydroxymethylpropionic acid and 0.5~0.6 times the mass of trimethylolpropane p-toluenesulfonic acid are added, and after reacting for 2~4h, the temperature is kept and a vacuum pump is connected to reduce pressure and remove water, and finally cooled to room temperature, dissolved with acetone, recrystallized with toluene, filtered and dried to obtain the terminal hydroxyl hyperbranched polyester.
[0013] Preferably, in the above step S4., the mass ratio of silica powder, mullite particles, silicon carbide powder and modified steel fiber is 1~6:60~70:1~4:0.2~0.8; the mass ratio of gypsum, aluminum powder, silica powder, aluminate cement, sodium hexametaphosphate and homemade water reducer is 10~20:1~4:2~4:6:2:1~2.
[0014] Preferably, in the above step S5., during curing, the temperature is raised to 30-40°C and cured for 16-20 hours, and the temperature is raised to 100-110°C and cured for 16-20 hours.
[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: The heat-shock-resistant and wear-resistant castable prepared by the present invention is prepared by adding water to a mixture, stirring evenly and then solidifying the mixture, wherein the mixture includes a matrix material and an aggregate; The matrix material includes silicon dioxide micropowder, mullite particles, silicon carbide powder and modified steel fiber; the modified steel fiber is prepared by treating the steel fiber with zinc sulfate and then coating the surface of the steel fiber with micro-nano flaky zinc phosphate with polydopamine; the steel fiber is treated with zinc sulfate to increase the surface roughness and form zinc phosphate linking sites on the surface, and then the surface of the steel fiber is coated with micro-nano flaky zinc phosphate with polydopamine to fix the micro-nano flaky zinc phosphate on the surface of the steel fiber, and the modified steel fiber is added to the mixture and evenly dispersed, and the network structure formed by the micro-nano flaky zinc phosphate can increase the number of microcracks and the size of large cracks in the system, thereby improving the thermal shock resistance; Aggregates include gypsum, aluminum micropowder, silicon micropowder, aluminate cement, sodium hexametaphosphate and a homemade water reducer; the homemade water reducer is a modified polyurethane, which is prepared by polycondensing dimethylolbutyric acid, hydroxyl monomers of polyethylene glycol ether and isocyanate monomers to form a long-chain polyurethane, which is then cross-linked with a terminal hydroxyl hyperbranched polyester; the homemade water reducer formed by cross-linking the long-chain polyurethane and the terminal hydroxyl hyperbranched polyester has abundant polar groups, which enhances the dispersion of particles in the raw material and aggregate in water, and has a stable structure, which enters into a network structure formed by micro-nano flaky zinc phosphate on the modified steel fiber, reduces the flocculation tendency of the water reducer, and enables the castable to have good flow properties, thereby enhancing the flexural strength. DETAILED DESCRIPTION
[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0017] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the heat shock and wear resistant castables prepared in the examples and comparative examples as follows: Flexural strength: The thermal shock and wear resistant castables prepared in the same embodiment and comparative example were measured for flexural strength with reference to GB / T3001.
[0018] Thermal shock resistance: The thermal shock and wear-resistant castables prepared in the examples and comparative examples were re-fired at 1550°C for 3 h, then kept at 1100°C for 30 min, and then air-cooled for 20 min. The flexural strength before and after re-firing was tested, and the flexural residual rate was calculated. Example 1
[0019] S1. Mix zinc oxide, 70% by mass phosphoric acid, citric acid, calcium nitrate, zinc nitrate and deionized water in a mass ratio of 5:30:1:20:20:100, heat to 72°C, immerse the steel fiber, phosphate for 15 minutes, filter and wash with deionized water three times, and dry to obtain a modified steel fiber base material; S2. ammonium carbonate, 5% ammonia water and zinc oxide were mixed in a mass ratio of 5:20:1, stirred and dissolved, filtered, heated to 50 ° C, magnetically stirred at 200 rpm for 4 hours, deionized water 4 times the total volume was added, aged for 4 hours, filtered and washed with deionized water 3 times, and then 4 times the mass of ammonium carbonate was added. 20% ethanol solution was added, stirred evenly, and phosphoric acid 0.2 times the mass of ammonium carbonate was added dropwise at a rate of 1 ml / min, reacted at room temperature for 25 minutes, and then filtered with a circulating water vacuum pump, and finally dried and ground to obtain micro-nano flaky zinc phosphate; 3g / L dopamine solution and micro-nano flaky zinc phosphate were mixed in a mass ratio of 20:1, the pH was adjusted to 7.6 with trishydroxymethylaminomethane, and 6 times the mass of micro-nano flaky zinc phosphate was added. Modified steel fiber base material, soaked for 6 hours, filtered and rinsed with deionized water, controlled water and dried to obtain modified steel fiber; S3. Under a nitrogen atmosphere, 2,2-dimethylolpropionic acid, trimethylolpropane and p-toluenesulfonic acid as a catalyst were mixed in a mass ratio of 40:13:0.1, heated to 135°C, refluxed for 2h, and then 6 times the mass of trimethylolpropane 2,2-dimethylolpropionic acid and 0.5 times the mass of trimethylolpropane p-toluenesulfonic acid were added. After reacting for 2h, the mixture was kept warm and connected to a vacuum pump to reduce pressure and remove water, and finally cooled to room temperature, dissolved in acetone, recrystallized in toluene, filtered and dried to obtain a terminal hydroxyl hyperbranched polyester; a molecular weight of 350 Polyethylene glycol ether, toluene diisocyanate and dimethylolbutyric acid were mixed in a mass ratio of 1:5:0.08, heated to 60°C, dibutyltin dilaurate in an amount of 0.03 times the mass of toluene diisocyanate was added, heated to 83°C, stirred at 200rpm for reaction for 3h, cooled to 38°C, acetone in an amount of 2 times the mass of toluene diisocyanate and terminal hydroxyl hyperbranched polyester in an amount of 0.2 times the mass of toluene diisocyanate were added, heated to 90°C, stirred at 200rpm for reaction for 2h, and a modified polyurethane was obtained, which was a homemade water reducer; S4. The silica powder, mullite particles, silicon carbide powder and modified steel fiber were mixed in a mass ratio of 1:60:1:0.2 to obtain a matrix material; gypsum, aluminum powder, silica powder, aluminate cement, sodium hexametaphosphate and a homemade water reducing agent were mixed in a mass ratio of 10:1:2:6:2:1 to obtain an aggregate; S5. Mix the matrix material and aggregate in a mass ratio of 1:1 to obtain a mixture, mix the mixture with water in a mass ratio of 20:0.9 and solidify, raise the temperature to 30°C during solidification, solidify for 16 hours, raise the temperature to 100°C, solidify for 16 hours, and obtain a heat-shock-resistant and wear-resistant castable. Example 2
[0020] S1. Mix zinc oxide, 75% by mass phosphoric acid, citric acid, calcium nitrate, zinc nitrate and deionized water in a mass ratio of 7:30:1:20:20:100, heat to 74°C, immerse the steel fiber, phosphate for 20 minutes, filter and wash with deionized water 4 times, and dry to obtain a modified steel fiber base material; S2. ammonium carbonate, 7% ammonia water and zinc oxide were mixed in a mass ratio of 5:20:1.5, stirred and dissolved, filtered, heated to 60 ° C, magnetically stirred at 300 rpm for 5 hours, deionized water was added in an amount of 5 times the total volume, aged for 5 hours, filtered and washed with deionized water 4 times, and then a 30% ethanol solution with a mass fraction of 5 times the mass of ammonium carbonate was added. After stirring, phosphoric acid with a mass fraction of 0.3 times the mass of ammonium carbonate was added dropwise at a rate of 2 ml / min, reacted at room temperature for 30 minutes, and then filtered with a circulating water vacuum pump. Finally, dried and ground to obtain micro-nano flaky zinc phosphate; 4g / L dopamine solution and micro-nano flaky zinc phosphate were mixed in a mass ratio of 25:4, the pH was adjusted to 7.7 with trishydroxymethylaminomethane, and 8 times the mass of micro-nano flaky zinc phosphate was added. Modified steel fiber base material, soaked for 9 hours, filtered and rinsed with deionized water, controlled water and dried to obtain modified steel fiber; S3. Under a nitrogen atmosphere, 2,2-dimethylolpropionic acid, trimethylolpropane and p-toluenesulfonic acid as a catalyst were mixed in a mass ratio of 40:13:0.15, heated to 140°C, refluxed for 3h, and then 7 times the mass of trimethylolpropane 2,2-dimethylolpropionic acid and 0.55 times the mass of trimethylolpropane p-toluenesulfonic acid were added. After reacting for 3h, the mixture was kept warm and connected to a vacuum pump to reduce pressure and remove water, and finally cooled to room temperature, dissolved in acetone, recrystallized in toluene, filtered and dried to obtain a hydroxyl-terminated hyperbranched polyester; a molecular weight of 35 0 polyethylene glycol ether, toluene diisocyanate and dimethylolbutyric acid are mixed in a mass ratio of 1:5:0.1, heated to 62°C, dibutyltin dilaurate (0.04 times the mass of toluene diisocyanate) is added, heated to 84°C, stirred at 300rpm for reaction for 4h, cooled to 40°C, acetone (3 times the mass of toluene diisocyanate) and terminal hydroxyl hyperbranched polyester (0.4 times the mass of toluene diisocyanate) are added, heated to 91°C, stirred at 300rpm for reaction for 3h to obtain modified polyurethane, which is a homemade water reducer; S4. The silica powder, mullite particles, silicon carbide powder and modified steel fiber were mixed in a mass ratio of 4:65:3:0.5 to obtain a matrix material; gypsum, aluminum powder, silica powder, aluminate cement, sodium hexametaphosphate and a homemade water reducing agent were mixed in a mass ratio of 15:2.5:3:6:2:1.5 to obtain an aggregate; S5. Mix the matrix material and aggregate in a mass ratio of 1:1.2 to obtain a mixture, mix the mixture with water in a mass ratio of 20:1 and solidify, raise the temperature to 35°C during solidification, solidify for 18 hours, raise the temperature to 105°C, solidify for 18 hours, and obtain a heat-shock-resistant and wear-resistant castable. Example 3
[0021] S1. Mix zinc oxide, 80% by mass phosphoric acid, citric acid, calcium nitrate, zinc nitrate and deionized water in a mass ratio of 8:30:1:20:20:100, heat to 77°C, immerse the steel fiber, phosphate for 25 minutes, filter and wash with deionized water 5 times, and dry to obtain a modified steel fiber base material; S2. ammonium carbonate, 8% ammonia water and zinc oxide were mixed in a mass ratio of 5:20:2, stirred and dissolved, filtered, heated to 80 ° C, magnetically stirred at 400 rpm for 6 hours, deionized water 6 times the total volume was added, aged for 6 hours, filtered and washed with deionized water 5 times, and then 6 times the mass of ammonium carbonate was added. 40% ethanol solution was added, stirred evenly, and phosphoric acid 0.4 times the mass of ammonium carbonate was added dropwise at a rate of 3 ml / min, reacted at room temperature for 35 minutes, and then filtered with a circulating water vacuum pump, and finally dried and ground to obtain micro-nano flaky zinc phosphate; 5g / L dopamine solution and micro-nano flaky zinc phosphate were mixed in a mass ratio of 30:6, the pH was adjusted to 7.8 with trishydroxymethylaminomethane, and 10 times the mass of micro-nano flaky zinc phosphate was added. Modified steel fiber base material, soaked for 12 hours, filtered and rinsed with deionized water, controlled water and dried to obtain modified steel fiber; S3. Under a nitrogen atmosphere, 2,2-dimethylolpropionic acid, trimethylolpropane and p-toluenesulfonic acid as a catalyst were mixed in a mass ratio of 40:13:0.2, heated to 145°C, refluxed for 4 hours, and then 8 times the mass of trimethylolpropane 2,2-dimethylolpropionic acid and 0.6 times the mass of trimethylolpropane p-toluenesulfonic acid were added. After reacting for 4 hours, the mixture was kept warm and connected to a vacuum pump to reduce pressure and remove water, and finally cooled to room temperature, dissolved in acetone, recrystallized in toluene, filtered and dried to obtain a hydroxyl-terminated hyperbranched polyester; a molecular weight of 350 Polyethylene glycol ether, toluene diisocyanate and dimethylolbutyric acid were mixed in a mass ratio of 1:5:0.12, heated to 65°C, dibutyltin dilaurate in an amount of 0.06 times the mass of toluene diisocyanate was added, heated to 85°C, stirred at 400rpm for reaction for 5h, cooled to 42°C, acetone in an amount of 4 times the mass of toluene diisocyanate and terminal hydroxyl hyperbranched polyester in an amount of 0.6 times the mass of toluene diisocyanate were added, heated to 92°C, stirred at 400rpm for reaction for 4h to obtain modified polyurethane, i.e., a homemade water reducer; S4. The silica powder, mullite particles, silicon carbide powder and modified steel fiber were mixed in a mass ratio of 6:70:4:0.8 to obtain a matrix material; gypsum, aluminum powder, silica powder, aluminate cement, sodium hexametaphosphate and a homemade water reducing agent were mixed in a mass ratio of 20:4:4:6:2:2 to obtain an aggregate; S5. Mix the matrix material and aggregate in a mass ratio of 1:1.5 to obtain a mixture, mix the mixture with water in a mass ratio of 20:1.1 and solidify, raise the temperature to 40°C during solidification, solidify for 20 hours, raise the temperature to 110°C, solidify for 20 hours, and obtain a heat-shock-resistant and wear-resistant castable.
[0022] Comparative Example 1 The composition of Comparative Example 1 is the same as that of Example 2. The difference between the preparation method of the heat shock and wear resistant castable and Example 2 is that the modified steel fiber is prepared by treating the steel fiber with zinc sulfate.
[0023] Comparative Example 2 The composition of Comparative Example 2 is the same as that of Example 2. The difference between the preparation method of the heat shock and wear resistant castable and Example 2 is that the matrix material includes silicon dioxide powder, mullite particles, silicon carbide powder and steel fiber.
[0024] Comparative Example 3 The composition of comparative example 3 is the same as that of example 2. The difference between the preparation method of the heat shock and wear resistant castable and example 2 is that the homemade water reducing agent is modified polyurethane, and the modified polyurethane is a long-chain polyurethane formed by polycondensation of dimethylolbutyric acid, hydroxyl monomer of polyethylene glycol ether and isocyanate monomer.
[0025] Comparative Example 4 The composition of Comparative Example 4 is the same as that of Example 2. The difference between the preparation method of the heat shock and wear resistant castable and Example 2 is that the aggregate includes gypsum, aluminum powder, silicon powder, aluminate cement, sodium hexametaphosphate and water reducing agent polyurethane.
[0026] Effect example Table 1 below shows the performance analysis results of the thermal shock and wear resistant castables prepared by using Examples 1 to 3 of the present invention and Comparative Examples 1 to 4: Table 1 Flexural strength (MPa) Flexural Residue (%) Example 1 29.5 55 Example 2 30.1 58 Example 3 29.4 52 Comparative Example 1 23.5 48 Comparative Example 2 24.3 45 Comparative Example 3 21.6 50 Comparative Example 4 20.9 49 By comparing the experimental data of the examples and the comparative examples in Table 1, it can be clearly found that the thermal shock and wear-resistant castables prepared using Examples 1, 2, and 3 have excellent thermal shock resistance and flexural strength.
[0027] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 1, Comparative Example 2, it can be found that the modified steel fiber prepared by treating the steel fiber with zinc sulfate and then coating the steel fiber surface with polydopamine with micro-nano flaky zinc phosphate, treating the steel fiber with zinc sulfate to increase the surface roughness, forming zinc phosphate linking sites on the surface, and then coating the steel fiber surface with polydopamine with micro-nano flaky zinc phosphate, fixing the micro-nano flaky zinc phosphate on the steel fiber surface, adding the modified steel fiber to the mixture, and uniformly dispersing it, the network structure formed by the micro-nano flaky zinc phosphate can increase the number of microcracks and the size of large cracks in the system, thereby improving the thermal shock resistance.
[0028] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 3, Comparative Example 4, it can be found that the self-made water reducer formed by cross-linking the long-chain polyurethane formed by condensing the hydroxyl monomer of dimethylolbutyric acid and polyethylene glycol ether and the isocyanate monomer with the terminal hydroxyl hyperbranched polyester has abundant polar groups, which enhances the dispersion performance of the particles in the raw material and aggregate in water, and has a stable structure, which reduces the flocculation tendency of the water reducer, so that the castable has good flow properties, thereby enhancing the flexural strength.
[0029] Obviously, the above embodiments are merely examples for clearly illustrating the embodiments of the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. However, these obvious changes or modifications derived from the spirit of the present invention are still within the scope of protection of the present invention.
Claims
1. A heat-shock-resistant and wear-resistant castable. It is characterized in that The heat-shock-resistant and wear-resistant castable is prepared by adding water to a mixture, stirring evenly and then solidifying; the mixture comprises a matrix material and an aggregate; the matrix material comprises silica powder, mullite particles, silicon carbide powder and modified steel fiber; the aggregate comprises gypsum, aluminum powder, silicon powder, aluminate cement, sodium hexametaphosphate and a homemade water reducer.
2. A thermal shock and wear resistant castable according to claim 1, It is characterized in that The mullite particles have an iron oxide content of 1-1.2% and a particle size of 6-8 mm.
3. A thermal shock and wear resistant castable according to claim 1, It is characterized in that The particle size of the silicon dioxide powder is 8-10 mm, the particle size of the silicon carbide powder is 6-8 mm, the particle size of the aluminum powder is 6-8 mm, and the particle size of the silicon powder is 6-8 mm.
4. A thermal shock and wear resistant castable according to claim 1, It is characterized in that The modified steel fiber is prepared by treating the steel fiber with zinc sulfate and then coating the surface of the steel fiber with polydopamine to form micro-nano flaky zinc phosphate; the length of the modified steel fiber is 4-6 mm.
5. The heat-shock-resistant and wear-resistant castable according to claim 1, It is characterized in that The self-made water reducing agent is a modified polyurethane; the modified polyurethane is prepared by polycondensing dimethylolbutyric acid, hydroxyl monomers of polyethylene glycol ether and isocyanate monomers to form a long-chain polyurethane, which is then cross-linked with terminal hydroxyl hyperbranched polyester.
6. A method for preparing the thermal shock and wear resistant castable as claimed in claim 1, It is characterized in that The specific steps include: S1. Mix zinc oxide, 70-80% by mass phosphoric acid, citric acid, calcium nitrate, zinc nitrate and deionized water in a mass ratio of 5-8:30:1:20:20:100, heat to 72-77°C, immerse the steel fiber, phosphate for 15-25 minutes, filter and wash with deionized water for 3-5 times, and dry to obtain a modified steel fiber base material; S2. 3-5 g / L dopamine solution and micro-nano flaky zinc phosphate were mixed in a mass ratio of 20-30:1-6, the pH was adjusted to 7.6-7.8 with tris(hydroxymethyl)aminomethane, 6-10 times the mass of micro-nano flaky zinc phosphate was added to the modified steel fiber base material, and the mixture was soaked for 6-12 hours, filtered and rinsed with deionized water, and dried after water control to obtain modified steel fiber; S3. A polyethylene glycol ether with a molecular weight of 350, toluene diisocyanate and dimethylolbutyric acid are mixed in a mass ratio of 1:5:0.08~0.12, the temperature is raised to 60~65°C, dibutyltin dilaurate is added in an amount of 0.03~0.06 times the mass of toluene diisocyanate, the temperature is raised to 83~85°C, the mixture is stirred at 200~400rpm for reaction for 3~5h, the temperature is lowered to 38~42°C, acetone in an amount of 2~4 times the mass of toluene diisocyanate and a terminal hydroxyl hyperbranched polyester in an amount of 0.2~0.6 times the mass of toluene diisocyanate are added, the temperature is raised to 90~92°C, the mixture is stirred at 200~400rpm for reaction for 2~4h, and a modified polyurethane is obtained, which is a homemade water reducing agent; S4. The silica powder, mullite particles, silicon carbide powder and modified steel fiber are mixed to obtain a matrix material; gypsum, aluminum powder, silica powder, aluminate cement, sodium hexametaphosphate and a homemade water reducing agent are mixed to obtain an aggregate; S5. The matrix material and the aggregate are mixed in a mass ratio of 1:1-1.5 to obtain a mixture, and the mixture is mixed with water in a mass ratio of 20:0.9-1.1 to solidify to obtain a heat-shock-resistant and wear-resistant castable.
7. A method for preparing a thermal shock and wear-resistant castable according to claim 6, It is characterized in that In the above step S2., the preparation method of micro-nano flaky zinc phosphate is as follows: ammonium carbonate, 5-8% ammonia water and zinc oxide are mixed in a mass ratio of 5:20:1-2, stirred to dissolve and then filtered, heated to 50-80°C, magnetically stirred at 200-400rpm for 4-6h, deionized water 4-6 times the total volume is added, aged for 4-6h, filtered and washed with deionized water 3-5 times, and then 4-6 times the mass of ammonium carbonate and 20-40% ethanol solution is added, stirred evenly, and phosphoric acid 0.2-0.4 times the mass of ammonium carbonate is added dropwise at a rate of 1-3ml / min, reacted at room temperature for 25-35min, filtered with a circulating water vacuum pump, and finally dried and ground to obtain micro-nano flaky zinc phosphate.
8. A method for preparing a heat-shock-resistant and wear-resistant castable according to claim 6, It is characterized in that In the above step S3., the preparation method of the terminal hydroxyl hyperbranched polyester is: under a nitrogen atmosphere, 2,2-dihydroxymethylpropionic acid, trimethylolpropane and catalyst p-toluenesulfonic acid are mixed in a mass ratio of 40:13:0.1~0.2, the temperature is raised to 135~145°C, refluxed for 2~4h, and then 2,2-dihydroxymethylpropionic acid with a mass of 6~8 times that of trimethylolpropane and p-toluenesulfonic acid with a mass of 0.5~0.6 times that of trimethylolpropane are added. After reacting for 2~4h, the mixture is kept warm and connected to a vacuum pump to reduce pressure and remove water, and finally cooled to room temperature, dissolved with acetone, recrystallized with toluene, filtered and dried to obtain the terminal hydroxyl hyperbranched polyester.
9. The method for preparing a thermal shock and wear-resistant castable according to claim 6, It is characterized in that In the above step S4., the mass ratio of silica powder, mullite particles, silicon carbide powder and modified steel fiber is 1~6:60~70:1~4:0.2~0.8; the mass ratio of gypsum, aluminum powder, silica powder, aluminate cement, sodium hexametaphosphate and homemade water reducer is 10~20:1~4:2~4:6:2:1~2.
10. The method for preparing a thermal shock and wear-resistant castable according to claim 6, It is characterized in that In the above step S5., during curing, the temperature is raised to 30-40°C and cured for 16-20 hours, and then the temperature is raised to 100-110°C and cured for 16-20 hours.
Citation Information
Patent Citations
Mullite castable and preparation method thereof
CN102557676A
Steel fiber reinforced wear-resisting castable for fluidized bed boiler
CN103539471A
Preparation method of nanometer sheet-shaped zinc phosphate
CN104495776A
Lightweight refractory castable suitable for doors and windows and preparation method of lightweight refractory castable
CN109627018A
Steel fiber surface modification treatment method
CN117245086A