Stain-resistant gypsum-based decorative plate as well as manufacturing method and application thereof
By applying a specific coating combination on the surface of the gypsum-based decorative board, the problem of insufficient stain resistance is solved, the adhesion and cleaning convenience are improved, and the service life is extended.
Patent Information
- Application Number
- CN202411053367.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-01
AI Technical Summary
Gypsum-based decorative boards are prone to stains during use and are difficult to clean. The existing technology has failed to effectively solve their stain resistance problem.
The surface of the gypsum-based decorative sheet is coated with a first coating including an acrylic copolymer, a hydrophobic nanoSiO2 and a wetting agent, and a second coating including a silicone hydrophobic agent, a silane coupling agent and a hydrophobic nanoSiO2, respectively. Improve its dirt and stain resistance.
Enhance the adhesion of the coating, simplifies the cleaning process, and extends the service life of gypsum-based decorative sheets.
Smart Images

Figure BDA0004976484330000061
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of building boards, and specifically relates to a stain-resistant gypsum-based decorative board, a manufacturing method thereof, and an application thereof. Background Art
[0002] Under the guidance of the national strategic policy of vigorously promoting prefabricated buildings, local governments have stepped up efforts to promote construction, and have explicitly required the delivery of fine decoration for affordable housing and public rental housing invested and built by the state, bringing greater market development space for various types of indoor dry-process finishing panels.
[0003] Gypsum-based decorative panels are decorative panels that replace wall cloth, wallpaper, paint and other on-site wet construction methods. They have the advantages of personalized design, factory production, all-dry assembly construction, fast installation, environmental protection and pollution-free, and ready-to-move-in. They are widely used in indoor partitions, ceilings and other fields. However, as decorative panels, they are inevitably stained for various reasons, and cleaning becomes a very practical problem. Summary of the invention
[0004] The following is an overview of the subject matter described in detail herein. This overview is not intended to limit the scope of protection of this application.
[0005] The present application provides a stain-resistant gypsum-based decorative board, a manufacturing method thereof, and an application thereof. The present application increases the dirt and stain resistance of the gypsum-based decorative board, improves the adhesion of the coating, makes cleaning more convenient, and increases the service life by coating a first coating comprising an acrylic copolymer, hydrophobic nano-SiO2, and a wetting agent and a second coating comprising an organic silicon hydrophobic agent, a silane coupling agent, and hydrophobic nano-SiO2 on the surface of the gypsum-based decorative board.
[0006] In one aspect, the present application provides a stain-resistant gypsum-based decorative board, comprising:
[0007] Gypsum-based decorative panels;
[0008] A first coating layer applied on the surface of the gypsum-based decorative board; and
[0009] A second coating layer is applied on the first coating layer,
[0010] The first coating layer comprises an acrylic copolymer, hydrophobic nano-SiO2 and a wetting agent, and the second coating layer comprises an organic silicon hydrophobic agent, a silane coupling agent and hydrophobic nano-SiO2.
[0011] In an embodiment of the present application, the first coating comprises 98.5-99.5 parts by weight of an acrylic copolymer, 0.3-0.8 parts by weight of hydrophobic nano-SiO2 and 0.2-0.7 parts by weight of a wetting agent. Preferably, the first coating comprises 99 parts by weight of an acrylic copolymer, 0.6 parts by weight of hydrophobic nano-SiO2 and 0.4 parts by weight of a wetting agent.
[0012] In an embodiment of the present application, the second coating contains 75-90 parts by weight of an organosilicon hydrophobic agent, 8-20 parts by weight of a silane coupling agent and 2-5 parts by weight of hydrophobic nano-SiO2. Preferably, the second coating contains 82 parts by weight of an organosilicon hydrophobic agent, 15 parts by weight of a silane coupling agent and 3 parts by weight of hydrophobic nano-SiO2.
[0013] In an embodiment of the present application, the acrylic copolymer is formed by reacting monomers of butyl acrylate, ethyl acrylate, methyl methacrylate or acrylic acid in the presence of an initiator, an emulsifier and a reducing agent. The acrylic copolymer has a solid content of 40%-50%, a pH of 9-9.5 and a minimum film-forming temperature of 5°C-15°C.
[0014] In the embodiment of the present application, the average particle size of the hydrophobic nano-SiO2 is 10-30nm, and the specific surface area is 200-300m 2 / g.
[0015] In an embodiment of the present application, the wetting agent is an alkylphenol polyoxyethylene ether type nonionic surfactant.
[0016] In an embodiment of the present application, the silicone hydrophobizing agent is a solvent-free silane / siloxane-based silicone concentrate.
[0017] In an embodiment of the present application, the silane coupling agent is an epoxy functional silane, preferably γ-glycidoxypropyltrimethoxysilane.
[0018] In another aspect, the present application provides a method for manufacturing the stain-resistant gypsum-based decorative board as described above, comprising the following steps:
[0019] Provide gypsum-based decorative panels;
[0020] Applying a first coating layer on a surface of the gypsum-based decorative board; and
[0021] applying a second coating on the first coating,
[0022] The first coating layer comprises an acrylic copolymer, hydrophobic nano-SiO2 and a wetting agent, and the second coating layer comprises an organic silicon hydrophobic agent, a silane coupling agent and hydrophobic nano-SiO2.
[0023] In an embodiment of the present application, a solution for the first coating is prepared by pouring 0.3-0.8 parts by weight of hydrophobic nano-SiO2 and 0.2-0.7 parts by weight of a wetting agent into 98.5-99.5 parts by weight of an acrylic copolymer, dispersing at a high speed of 1200-1800 rpm for 10-20 minutes, and dispersing uniformly;
[0024] The solution for the second coating is prepared by pouring 8-20 parts by weight of a silane coupling agent into 75-90 parts by weight of an organosilicon hydrophobic agent, dispersing at a high speed of 1000-1500 rpm for 5-15 minutes, then adding 2-5 parts by weight of hydrophobic nano-SiO2, continuing to disperse at 1000-1500 rpm for 15-25 minutes, and dispersing evenly.
[0025] In an embodiment of the present application, the solution of the first coating is applied on the surface of the gypsum-based decorative board at 10-20 g / m2 and baked at 30°C-50°C for 10-20 minutes, and the solution of the second coating is applied on the first coating at 20-30 g / m2 and baked at 60°C-80°C for 10-30 minutes to obtain a stain-resistant gypsum-based decorative board.
[0026] In yet another aspect, the present application provides the use of the stain-resistant gypsum-based decorative board as described above or the stain-resistant gypsum-based decorative board manufactured by the method as described above in indoor partition walls or suspended ceilings.
[0027] The present application increases the dirt and stain resistance of the gypsum-based decorative board, improves the adhesion of the coating, makes cleaning more convenient, and increases the service life by respectively coating the surface of the gypsum-based decorative board with a first coating comprising an acrylic copolymer, hydrophobic nano-SiO2 and a wetting agent, and a second coating comprising an organosilicon hydrophobic agent, a silane coupling agent and hydrophobic nano-SiO2.
[0028] Other features and advantages of the present application will be described in the following description, and partly become apparent from the description, or be understood by implementing the present application. Other advantages of the present application can be realized and obtained by the schemes described in the description. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the present application more clear, the embodiments of the present application will be described in detail below. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other arbitrarily without conflict.
[0030] The present application provides a stain-resistant gypsum-based decorative board, comprising:
[0031] Gypsum-based decorative panels;
[0032] A first coating layer applied on the surface of the gypsum-based decorative board; and
[0033] A second coating layer is applied on the first coating layer,
[0034] The first coating layer comprises an acrylic copolymer, hydrophobic nano-SiO2 and a wetting agent, and the second coating layer comprises an organic silicon hydrophobic agent, a silane coupling agent and hydrophobic nano-SiO2.
[0035] In an embodiment of the present application, the first coating comprises 98.5-99.5 parts by weight of an acrylic copolymer, 0.3-0.8 parts by weight of hydrophobic nano-SiO2 and 0.2-0.7 parts by weight of a wetting agent. Preferably, the first coating comprises 99 parts by weight of an acrylic copolymer, 0.6 parts by weight of hydrophobic nano-SiO2 and 0.4 parts by weight of a wetting agent.
[0036] In an embodiment of the present application, the second coating contains 75-90 parts by weight of an organosilicon hydrophobic agent, 8-20 parts by weight of a silane coupling agent and 2-5 parts by weight of hydrophobic nano-SiO2. Preferably, the second coating contains 82 parts by weight of an organosilicon hydrophobic agent, 15 parts by weight of a silane coupling agent and 3 parts by weight of hydrophobic nano-SiO2.
[0037] In an embodiment of the present application, the acrylic copolymer is formed by reacting monomers of butyl acrylate, ethyl acrylate, methyl methacrylate or acrylic acid in the presence of an initiator, an emulsifier and a reducing agent. The acrylic copolymer has a solid content of 40%-50%, a pH of 9-9.5 and a minimum film-forming temperature of 5°C-15°C.
[0038] In the embodiment of the present application, the average particle size of the hydrophobic nano-SiO2 is 10-30nm, and the specific surface area is 200-300m 2 / g.
[0039] In an embodiment of the present application, the wetting agent is an alkylphenol polyoxyethylene ether type nonionic surfactant.
[0040] In an embodiment of the present application, the organosilicon hydrophobic agent is a solvent-free silane / siloxane-based organosilicon concentrate.
[0041] In an embodiment of the present application, the silane coupling agent is an epoxy functional silane, preferably γ-glycidyloxypropyltrimethoxysilane.
[0042] The present application also provides a method for manufacturing the stain-resistant gypsum-based decorative board as described above, comprising the following steps:
[0043] Provide gypsum-based decorative panels;
[0044] Applying a first coating layer on a surface of the gypsum-based decorative board; and
[0045] A second coating is applied on the first coating to obtain a stain-resistant gypsum-based decorative board.
[0046] The first coating layer comprises an acrylic copolymer, hydrophobic nano-SiO2 and a wetting agent, and the second coating layer comprises an organic silicon hydrophobic agent, a silane coupling agent and hydrophobic nano-SiO2.
[0047] In an embodiment of the present application, a solution for the first coating layer is prepared by pouring 0.3-0.8 parts by weight of hydrophobic nano-SiO2 and 0.2-0.7 parts by weight of a wetting agent into 98.5-99.5 parts by weight of an acrylic copolymer, dispersing at a high speed of 1200-1800 rpm for 10-20 minutes, and dispersing uniformly;
[0048] The solution for the second coating is prepared by pouring 8-20 parts by weight of a silane coupling agent into 75-90 parts by weight of an organosilicon hydrophobic agent, dispersing at a high speed of 1000-1500 rpm for 5-15 minutes, then adding 2-5 parts by weight of hydrophobic nano-SiO2, continuing to disperse at 1000-1500 rpm for 15-25 minutes, and dispersing evenly.
[0049] In an embodiment of the present application, the solution of the first coating is applied on the surface of the gypsum-based decorative board at 10-20 g / m2 and baked at 30-50°C for 10-20 minutes, and the solution of the second coating is applied on the first coating at 20-30 g / m2 and baked at 60-80°C for 10-30 minutes to obtain a stain-resistant gypsum-based decorative board.
[0050] The embodiments of the present application also provide the use of the stain-resistant gypsum-based decorative board as described above or the stain-resistant gypsum-based decorative board manufactured by the method as described above in indoor partition walls or suspended ceilings.
[0051] The acrylic copolymer used in the examples and comparative examples of the present application was purchased from Dow, brand MAINCOTE IC-1002, with a solid content of 42%, a pH of 9.4, and a minimum film-forming temperature of 9°C. The average particle size of the hydrophobic nano-SiO2 is 20 nm, and the specific surface area is 240 m 2 / g. The wetting agent is LF 7100. The silicone hydrophobic agent is purchased from Wacker BS290. The silane coupling agent is KH560 (γ-glycidyloxypropyltrimethoxysilane).
[0052] Embodiment 1:
[0053] 0.3 parts by weight of hydrophobic nano-SiO2 and 0.2 parts by weight of a wetting agent were poured into 99.5 parts by weight of an acrylic copolymer, and dispersed at a high speed of 1200 rpm for 10 minutes to obtain a first coating solution after uniform dispersion.
[0054] Pour 8 parts by weight of silane coupling agent into 90 parts by weight of silicone hydrophobic agent, disperse at a high speed of 1000 rpm for 5 minutes, then add 2 parts by weight of hydrophobic nano-SiO2, continue to disperse at 1000 rpm for 15 minutes, and obtain a second coating solution after uniform dispersion.
[0055] The solution of the first coating is applied on the surface of the gypsum-based decorative board at 10 g / m2 and baked at 30°C for 10 minutes. Then, the solution of the second coating is applied on the dried first coating at 20 g / m2 and baked at 60°C for 10 minutes to obtain a stain-resistant gypsum-based decorative board.
[0056] Embodiment 2:
[0057] 0.6 parts by weight of hydrophobic nano-SiO2 and 0.4 parts by weight of a wetting agent were poured into 99 parts by weight of an acrylic copolymer, and dispersed at a high speed of 1500 rpm for 15 minutes to obtain a first coating solution after uniform dispersion.
[0058] Pour 15 parts by weight of silane coupling agent into 82 parts by weight of silicone hydrophobic agent, disperse at a high speed of 1200 rpm for 10 minutes, then add 3 parts by weight of hydrophobic nano-SiO2, and continue to disperse at 1200 rpm for 20 minutes to obtain a second coating solution after uniform dispersion.
[0059] The solution of the first coating is applied on the surface of the gypsum-based decorative board at 15 g / m2 and baked at 40°C for 15 minutes. Then, the solution of the second coating is applied on the dried first coating at 25 g / m2 and baked at 70°C for 20 minutes to obtain a stain-resistant gypsum-based decorative board.
[0060] Embodiment 3:
[0061] 0.8 parts by weight of hydrophobic nano-SiO2 and 0.7 parts by weight of a wetting agent were poured into 98.5 parts by weight of an acrylic copolymer, and dispersed at a high speed of 1800 rpm for 20 minutes to obtain a first coating solution after uniform dispersion.
[0062] Pour 20 parts by weight of silane coupling agent into 75 parts by weight of silicone hydrophobic agent, disperse at a high speed of 1500 rpm for 15 minutes, then add 5 parts by weight of hydrophobic nano-SiO2, and continue to disperse at 1500 rpm for 25 minutes to obtain a second coating solution after uniform dispersion.
[0063] The solution of the first coating is applied on the surface of the gypsum-based decorative board at 20 g / m2 and baked at 50°C for 20 minutes. Then, the solution of the second coating is applied on the dried first coating at 30 g / m2 and baked at 80°C for 30 minutes to obtain a stain-resistant gypsum-based decorative board.
[0064] Comparative Example 1:
[0065] Pour 15 parts by weight of silane coupling agent into 82 parts by weight of silicone hydrophobic agent, disperse at a high speed of 1200 rpm for 10 minutes, then add 3.6 parts by weight of hydrophobic nano-SiO2 and 0.4 parts by weight of wetting agent, continue to disperse at 1500 rpm for 15 minutes, finally add 99 parts by weight of acrylic copolymer, continue to disperse at 1200 rpm for 20 minutes to obtain the coating material.
[0066] The coating material was coated on a gypsum-based decorative board at 25 g / m2 and baked at 70°C for 20 minutes to obtain a stain-resistant gypsum-based decorative board.
[0067] Comparative Example 2:
[0068] The organic silicon hydrophobic agent was coated on the gypsum-based decorative board at 25 g / m2 and baked at 70°C for 20 minutes to obtain the stain-resistant gypsum-based decorative board.
[0069] Comparison of implementation effects:
[0070] The water contact angle, adhesion and stain resistance of the stain-resistant gypsum-based decorative panels manufactured in Examples 1-3 and Comparative Example 1 were tested, and the results are shown in Table 1 below.
[0071] Table 1
[0072]
[0073] Since the decorative material on the gypsum-based decorative board is a PVC material, the surface is smooth and the permeability is poor, and the organosilicon hydrophobic agent is directly applied thereon, the problem of poor adhesion will occur. The embodiments 1-3 of the present application are respectively coated on the surface of the gypsum-based decorative board with an acrylic copolymer, a hydrophobic nano-SiO2 and a first coating of a wetting agent and a second coating comprising an organosilicon hydrophobic agent, a silane coupling agent and a hydrophobic nano-SiO2, which not only improves the adhesion of the coating, but also further improves the anti-fouling performance of the gypsum-based decorative board. In addition, in Comparative Example 1, by directly mixing the organosilicon hydrophobic agent with an acrylic copolymer, a silane coupling agent, a wetting agent, and a hydrophobic nano-SiO2 and applying it on the surface of the gypsum-based decorative board, the problem of the coating becoming sticky will occur, and it is easy to get dusty, which affects the anti-fouling effect. In Examples 1-3 of the present application, the problem of coating stickiness is avoided by first applying a first coating layer comprising an acrylic copolymer, hydrophobic nano-SiO2 and a wetting agent on the surface of a gypsum-based decorative board and drying it, and then applying a second coating layer comprising a silicone hydrophobic agent, a silane coupling agent and hydrophobic nano-SiO2 on the first coating layer and drying it.
[0074] Although the embodiments disclosed in this application are as above, the contents described are only embodiments adopted to facilitate understanding of this application and are not intended to limit this application. Any technician in the field to which this application belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in this application, but the scope of patent protection of this application shall still be based on the scope defined in the attached claims.
Claims
1. A stain-resistant gypsum-based decorative board, comprising: Gypsum-based decorative panels; A first coating layer applied on the surface of the gypsum-based decorative board; as well as A second coating layer is applied on the first coating layer, The first coating layer comprises an acrylic copolymer, hydrophobic nano-SiO2 and a wetting agent, and the second coating layer comprises an organic silicon hydrophobic agent, a silane coupling agent and hydrophobic nano-SiO2.
2. The stain-resistant gypsum-based decorative board according to claim 1, wherein: The first coating comprises 98.5-99.5 parts by weight of acrylic copolymer, 0.3-0.8 parts by weight of hydrophobic nano-SiO2 and 0.2-0.7 parts by weight of wetting agent. Preferably, the first coating comprises 99 parts by weight of acrylic copolymer, 0.6 parts by weight of hydrophobic nano-SiO2 and 0.4 parts by weight of wetting agent.
3. The stain-resistant gypsum-based decorative board according to claim 1, wherein: The second coating contains 75-90 parts by weight of an organosilicon hydrophobic agent, 8-20 parts by weight of a silane coupling agent and 2-5 parts by weight of hydrophobic nano-SiO2. Preferably, the second coating contains 82 parts by weight of an organosilicon hydrophobic agent, 15 parts by weight of a silane coupling agent and 3 parts by weight of hydrophobic nano-SiO2.
4. The stain-resistant gypsum-based decorative board according to any one of claims 1 to 3, wherein: The acrylic copolymer is prepared by reacting monomers of butyl acrylate, ethyl acrylate, methyl methacrylate or acrylic acid in the presence of an initiator, an emulsifier and a reducing agent; the acrylic copolymer has a solid content of 40%-50%, a pH of 9-9.5 and a minimum film-forming temperature of 5°C-15°C.
5. The stain-resistant gypsum-based decorative board according to any one of claims 1 to 3, wherein: The average particle size of the hydrophobic nano-SiO2 is 10-30nm, and the specific surface area is 200-300m 2 / g.
6. The stain-resistant gypsum-based decorative board according to any one of claims 1 to 3, wherein: The wetting agent is an alkylphenol polyoxyethylene ether type nonionic surfactant.
7. The stain-resistant gypsum-based decorative board according to any one of claims 1 to 3, wherein: The silicone hydrophobic agent is a solvent-free silane / siloxane-based silicone concentrate.
8. The stain-resistant gypsum-based decorative board according to any one of claims 1 to 3, wherein: The silane coupling agent is an epoxy functional silane, preferably γ-glycidoxypropyltrimethoxysilane.
9. A method for manufacturing the stain-resistant gypsum-based decorative board according to any one of claims 1 to 8, comprising the following steps: Provide gypsum-based decorative panels; Applying a first coating to a surface of the gypsum-based decorative board; as well as applying a second coating on the first coating, The first coating layer comprises an acrylic copolymer, hydrophobic nano-SiO2 and a wetting agent, and the second coating layer comprises an organic silicon hydrophobic agent, a silane coupling agent and hydrophobic nano-SiO2.
10. The method according to claim 9, wherein: The first coating solution is prepared by pouring 0.3-0.8 parts by weight of hydrophobic nano-SiO2 and 0.2-0.7 parts by weight of a wetting agent into 98.5-99.5 parts by weight of an acrylic copolymer, dispersing at a high speed of 1200-1800 rpm for 10-20 minutes, and dispersing uniformly; The solution for the second coating is prepared by pouring 8-20 parts by weight of a silane coupling agent into 75-90 parts by weight of an organosilicon hydrophobic agent, dispersing at a high speed of 1000-1500 rpm for 5-15 minutes, then adding 2-5 parts by weight of hydrophobic nano-SiO2, continuing to disperse at 1000-1500 rpm for 15-25 minutes, and dispersing evenly.
11. The method according to claim 10, wherein: The solution of the first coating is applied on the surface of the gypsum-based decorative board at 10-20 g / m2, and baked at 30°C-50°C for 10-20 minutes. The solution of the second coating is applied on the first coating at 20-30 g / m2, and baked at 60°C-80°C for 10-30 minutes to obtain a stain-resistant gypsum-based decorative board.
12. Use of the stain-resistant gypsum-based decorative board according to any one of claims 1 to 8 or the stain-resistant gypsum-based decorative board manufactured by the method according to any one of claims 9 to 11 in indoor partition walls or suspended ceilings.
Citation Information
Patent Citations
Decorative gypsum board with self-cleaning function and production process thereof
CN105507529A
Organic silicon coating super-hydrophobic coating and preparation method thereof
CN116804132A
Easy-to-clean material, preparation method and application thereof
CN117247586A