Crystal material, preparation method thereof and application of crystal material in high-selectivity capture of lead (II) in water body
The synthesis of Ba-Zn-Sb oxygen cluster-based materials by a solvothermal method solves the problems of poor selectivity and low reusability of lead(II) ions in existing technologies, and achieves highly selective adsorption and separation of lead(II) ions, which is suitable for the treatment of heavy metal waste liquid.
Patent Information
- Application Number
- CN202410930861.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-22
AI Technical Summary
Existing technologies have poor selectivity and low reusability when removing lead(II) ions from wastewater. Furthermore, commonly used materials pose a risk of secondary pollution, and their adsorption effect is affected by pH value and salinity.
Ba-Zn-Sb oxygen cluster-based materials were synthesized by a solvothermal method, and a three-dimensional framework structure was formed through in-situ synthesis. Ba-Zn-Sb oxygen cluster-based materials were used as highly selective adsorbents to adsorb and separate lead(II) ions.
It achieves highly selective adsorption and separation of lead(II) ions, has a wide applicable pH range, is simple to prepare, low in cost, and easy to reuse, making it suitable for the treatment of heavy metal waste liquid.
Smart Images

Figure CN118994264A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a crystal material and a preparation method thereof and application in the highly selective capture of lead (II) in water bodies, belonging to the field of materials. Background Art
[0002] Lead is widely used in battery manufacturing, coatings, cosmetics and other industries due to its excellent physical and chemical properties (Ann. Rev. Med. 2004, 55, 209-222). In particular, the manufacture and use of lead-acid batteries consumes about 80% of the total industrial lead, and the waste generated is an important source of lead pollution. The large amount of wastewater generated during the manufacture of lead-acid batteries has complex components and contains Cu 2+ 、Ni 2+ and Cd 2+ Other transition metal ions such as lead (II) and lead ions (II) are present in the environment for a long time. It is reported that one in five children in India is a victim of lead poisoning. According to the World Health Organization, about 600,000 children suffer from intellectual disabilities due to lead exposure every year.
[0003] At present, the removal of Pb from wastewater 2+ The main methods are precipitation (Sep. Purif. Technol. 2007, 54, 373-381), ion exchange (Micropor. Mesopor. Mater. 1999, 28, 315-324) and adsorption (Rev. Environ. Sci. Biotechnol. 2019, 18, 231-269). Although precipitation and adsorption are more commonly used, they are often affected by the pH value and salt content of the wastewater, resulting in poor selectivity for removing target metal ions, and there is also a risk of secondary pollution when using precipitation. At present, ion exchange resin is the most widely used method for removing Pb 2+ The most commonly used ion exchange material, but its further application is limited due to resin scaling and adsorption of organic matter. Therefore, more and more other ion exchange materials have been developed and applied, such as polymetallic oxygen compounds (J.Environ.2017,5,1866-1873) and metal organic frameworks (Chem.Eur.J.2020,26,1355-1362) and their composites (ACS Sustainable Chem.Eng.2018,6,3176-3186). These materials have a great influence on the degradation of Pb 2+ However, when there are other competing ions (such as Cu 2 + 、Ni 2+ and Cd 2+ ), their selectivity will be greatly disturbed.
[0004] High-nuclear metal oxygen clusters have attracted much attention in the field of ion exchange due to their abundant active sites on the cluster surface. For example, H3PW is filled in the pores of the Cu3(btc)2 framework (H3btc = 1,3,5-benzenetricarboxylic acid). 12 O 40 Composite material HKUST-1-@H3PW formed by clusters 12 O 40 , can adsorb up to 98.18 mg / g of Pb 2+ However, competing ion experiments showed that Pb 2 + With a lot of Cr 3+ and Cd 2+ was adsorbed at the same time, which indicates that its 2+ The selectivity of molybdate compounds (4-Hap)4[Mo8O 16 ](BUC-14, 4-ap=4-aminopyridine) and [δ-Mo8O 26 ](L)2-2H2O (BUC-77, L = 1,10-bis(4-carboxybenzyl)-4,4'-bipyridyl dichloride) also showed 2+ The high adsorption capacity of BUC-14 can separate Cu 2+ and Pb 2+ Although only metal oxide cluster-based materials have shown 2+ However, its clear and precise adsorption mechanism has not been revealed at the atomic level. Therefore, it is necessary to design and construct new crystalline materials based on metal oxygen clusters to capture Pb with high selectivity. 2+ It has important scientific significance and application prospects. Summary of the invention
[0005] The present application utilizes in-situ synthesized Ba-Zn-Sb oxygen cluster-based materials to solve the shortcomings of poor selectivity and low reuse rate of the materials when removing lead (II) ions in water.
[0006] According to one aspect of the present application, a crystalline material is provided, wherein the chemical formula of the crystalline material is C 24 H 59.03 Ba 2.485 O 70 Sb 12 Zn2.
[0007] The crystalline material crystallizes in the triclinic system, and the space group is
[0008] The unit cell parameters of the crystal material are: α=69.57~69.67°, β=70.19~70.29°, γ=88.93~89.03°, Z=2.
[0009] Optionally, the unit cell parameters of the crystal material are:
[0010] , α=69.5710(10)°, β=70.1960(10)°, γ=88.9380(10)°, Z=2.
[0011] The structure of the crystalline material is as follows:
[0012] The anion clusters [Zn2Sb 12 (μ3-O)8(μ4-O)3(tta)6] 6- (Htta = tartaric acid) as the main framework, each anion cluster is connected to six Ba 2+ ions, four of which are fully occupied Ba(1), and one partially occupied Ba(2) and Ba(3). Each Ba(1) ion connects four adjacent anion clusters, thereby partially forming a wavy layer of the anion cluster. The partially occupied Ba(2) and Ba(3) are connected to each other in a common edge manner by sharing oxygen atoms, and then Ba(3) self-aggregates through oxygen atom edge sharing to form a "z"-shaped scaffold of a four-core cluster. The "z"-shaped scaffold further connects adjacent wavy layers along the c-axis direction to form a three-dimensional framework structure. In addition, there is also partially occupied Ba(4) that is connected to Ba(2) and Ba(3) in a common point manner, turning the original four-core cluster into a six-core cluster, but Ba(4) is not directly connected to the wavy layer formed by Ba(1), but is only suspended in the pores of the anion framework.
[0013] According to another aspect of the present application, a method for preparing the above-mentioned crystalline material is provided, using a solvothermal method, comprising the following steps:
[0014] In a sealed container, raw materials containing an antimony source, a zinc source and a barium source are mixed with a solvent and reacted to obtain the crystalline material.
[0015] The antimony source is selected from potassium antimony tartrate;
[0016] The zinc source is selected from zinc nitrate; it can be zinc nitrate hexahydrate.
[0017] The barium source is selected from barium nitrate, and may be barium nitrate hexahydrate.
[0018] The mass ratio of the antimony source, the zinc source and the barium source is 0.11-0.12: 0.108-0.115: 0.1-0.11.
[0019] The mass ratio of the antimony source in the raw material to the volume ratio of the solvent is 0.11 g: 3-4 mL.
[0020] The solvent contains N,N'-dimethylformamide and water, wherein the volume ratio of N,N'-dimethylformamide to water is 1:3.
[0021] The reaction temperature is 80-100°C;
[0022] The reaction time is 3 to 5 days.
[0023] Specifically,
[0024] First, potassium antimony tartrate purchased from commercial channels is mixed with zinc nitrate and barium nitrate in a solvent containing a mixture of N,N'-dimethylformamide and water, sealed in an 8mL glass bottle, and then transferred to a preheating furnace at 80-100°C for continuous heating reaction for 4 days. After cooling to room temperature, ultrasonic cleaning is performed, and then the obtained Ba-Zn-Sb oxygen cluster-based material is repeatedly washed with water and anhydrous ethanol for several times, and then filtered and dried to obtain the Ba-Zn-Sb oxygen cluster-based material, that is, the crystalline material.
[0025] According to another aspect of the present application, there is provided a use of the above-mentioned crystal material in the highly selective capture of lead (II) in water.
[0026] Specifically, the above-mentioned crystalline material is first ground and passed through a 100-mesh sieve so that it can fully expand its specific surface area and increase the adsorption active sites to maximize its adsorption amount, and then contacted with a solution containing the lead (II) element. After adsorption, the crystalline material can dynamically / statically separate and / or extract the lead (II) element.
[0027] The contact methods include:
[0028] 1. contacting the crystalline material with a solution containing lead (II) ions;
[0029] 2. Passing a solution containing lead (II) ions through an adsorption column, separating and / or extracting the lead (II) ions in the solution in the adsorption column; the adsorption column is filled with the crystalline material.
[0030] The temperature at which the crystalline material adsorbs the lead (II) ions is 20 to 25° C.; the contact time for the crystalline material to adsorb the lead (II) ions is 6 to 10 hours;
[0031] Optionally, the temperature at which the crystalline material adsorbs the lead (II) ions is 25°C; and the contact time is 10 hours.
[0032] The solution containing lead (II) ions also includes interfering ions such as cadmium (II) ions and nickel (II) ions.
[0033] The beneficial effects of the technical solution of the present invention are:
[0034] (1) The preparation method of the Ba-Zn-Sb oxygen cluster-based material provided in the present application is simple to operate, easy to repeat, and the raw materials are cheap and easy to obtain, and the cost is low;
[0035] (2) The synthesis reaction conditions of the Ba-Zn-Sb oxygen cluster-based material prepared in this application are mild, the equipment requirements are not high, and it belongs to a low-energy consumption processing process;
[0036] (3) The preparation method provided in this application can solve the problems of small powder particles, difficulty in recovery and recycling when oxygen cluster-based materials are used as ion adsorbents;
[0037] (4) This application applies to Pb 2+ The adsorption of ions is applicable to aqueous solution environments with a wide pH range;
[0038] (5) Pb passing through the system 2+ Ion adsorption experiments including kinetics, concentration dependence, acid and alkali resistance, and application of adsorption columns have confirmed that the prepared material is an efficient adsorption material for Pb 2+ Ionic materials have broad application prospects in the field of heavy metal waste liquid treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 The crystal structure diagram of the Ba-Zn-Sb oxygen cluster-based material obtained in Example 1, after exchange of lead (II) and after elution of lead (II).
[0040] Figure 2 This is a comparison chart of X-ray powder diffraction of the Ba-Zn-Sb oxygen-based material obtained in Example 1, after exchange of lead (II) and after elution of lead (II).
[0041] Figure 3 This is the kinetic diagram of the removal of lead (II) ions by the Ba-Zn-Sb oxygen cluster-based material obtained in Example 1.
[0042] Figure 4 This is the adsorption model diagram of the Ba-Zn-Sb oxygen cluster-based material obtained in Example 1 for removing lead (II) ions.
[0043] Figure 5 a is a graph showing the removal rate and distribution coefficient of lead (II) ions of the Ba-Zn-Sb oxygen-based material obtained in Example 1 in a wide pH range, Figure 5 b is a comparison diagram of X-ray powder diffraction of the Ba-Zn-Sb oxygen cluster-based material obtained in Example 1 over a wide pH range.
[0044] Figure 6 This is a diagram showing the removal rate and distribution coefficient of lead (II) ions by the Ba-Zn-Sb oxygen cluster-based material obtained in Example 1 in the presence of different competing ions.
[0045] Figure 7 a is a graph showing the adsorption / desorption rate of lead (II) ions by the Ba-Zn-Sb oxygen cluster-based material obtained in Example 1 during three cycles, Figure 7 b is a comparison diagram of X-ray powder diffraction of the Ba-Zn-Sb oxygen cluster-based material obtained in Example 1 after three cycles.
[0046] Figure 8 This is a comparison chart of the removal rates of lead (II) ions, nickel (II) ions, and cadmium (II) ions by the Ba-Zn-Sb oxygen-based material obtained in Example 1 in a column experiment. DETAILED DESCRIPTION
[0047] The present application is further described below in conjunction with the examples. It should be understood that these examples are only used to illustrate the present application and are not used to limit the scope of the present application.
[0048] Unless otherwise specified, the test conditions for the samples in the examples are as follows:
[0049] Inductively coupled plasma mass spectrometry (ICP-MS) and inductively coupled plasma optical emission spectroscopy (ICP-OES) were performed on XSerise II and Thermo 7400 instruments, respectively.
[0050] Energy dispersive X-ray spectroscopy (EDS) tests were performed on a JEOL JSM-6700F scanning electron microscope and a HITACHI FE-SEMSU8010 machine.
[0051] X-ray powder diffraction phase analysis (XRD) was carried out on a Rigaku Miniflex II X-ray diffractometer at 30 kV and 15 mA, using a Cu target and a K α Radiation Source
[0052] The removal rate in the examples of this application is calculated by the following method:
[0053]
[0054] In the examples of the present application, the adsorption amount is calculated by the following method:
[0055]
[0056] The distribution coefficient in the embodiments of the present application is calculated by the following method:
[0057]
[0058] In the above formula, C0 and C e represents the initial concentration and equilibrium concentration of the lead solution, respectively. Where b is the Langmuir constant related to the adsorption free energy. b is a constant related to the adsorption free energy, and n is the Freundlich constant. k F is the Freundlich adsorption equilibrium constant.
[0059] Example 1. Preparation of Ba-Zn-Sb oxygen cluster-based materials
[0060] 113.6 mg of potassium antimony tartrate, 178.5 mg of zinc nitrate hexahydrate, 100.0 mg of barium nitrate hexahydrate, 3 mL of water and 1 mL of N,N'-dimethylformamide were sealed in an 8 mL glass bottle, heated at 100°C for 4 days, and then cooled to room temperature. The sample was ultrasonically cleaned with water and anhydrous ethanol for multiple times, and 56.1 mg of colorless block crystalline Ba-Zn-Sb oxygen cluster-based material was obtained by filtration. The colorless block crystalline Ba-Zn-Sb oxygen cluster-based material obtained in this example was used below.
[0061] Example 2: Characterization of Ba-Zn-Sb oxygen cluster-based materials
[0062] The crystalline Ba-Zn-Sb oxygen cluster-based materials and the eluted crystalline Ba-Zn-Sb oxygen cluster-based materials were measured on a Rigaku XtaLAB Synergy diffractometer. The recording temperature is 295(2)K. The crystalline Pb-Zn-Sb oxygen cluster-based material after exchange is measured on the Rigaku XtaLAB Synergy diffractometer. The single crystal structure is recorded above, and the recording temperature is 100(2)K.
[0063] The unit cell parameters are α=69.5710(10)°, β=70.1960(10)°, γ=88.9380(10)°,
[0064] The chemical formula of the crystalline material is C 24 H 59.03 Ba 2.485 O 70 Sb 12 Zn2.
[0065] Chemical formula after exchange: C 24 H 58.13 O 69.5 Pb 2.435 Sb 12 Zn2.
[0066] Chemical formula C after elution 24 H 59.41 Ba 2.445 O 70.25 Pb 0.1 Sb 12 Zn2.
[0067] The test results are as follows Figure 1 and Figure 2 The prepared crystalline material was crystallized in the triclinic system before and after adsorption and after elution. Space group, belongs to isostructural compounds, anion clusters [Zn2Sb 12 (μ3-O)8(μ4-O)3(tta)6] 6- (Htta = tartaric acid) as the main framework, each anion cluster is connected to six Ba 2+ ions, four of which are fully occupied Ba(1), and one partially occupied Ba(2) and Ba(3). Each Ba(1) ion connects four adjacent anion clusters, thereby partially forming a wavy layer of the anion cluster. The partially occupied Ba(2) and Ba(3) are connected to each other in a common edge manner by sharing oxygen atoms, and then Ba(3) self-aggregates through oxygen atom edge sharing to form a "z"-shaped scaffold of a four-core cluster. The "z"-shaped scaffold further connects adjacent wavy layers along the c-axis direction to form a three-dimensional framework structure. In addition, there is also partially occupied Ba(4) that is connected to Ba(2) and Ba(3) in a common point manner, turning the original four-core cluster into a six-core cluster, but Ba(4) is not directly connected to the wavy layer formed by Ba(1), but is only suspended in the pores of the anion framework.
[0068] After adsorbing lead, the original Ba(1) site splits into Pb(1) and Pb(1B); the Ba(3) site splits into Pb(3), Pb(3B) and Pb(3C). Ba(2), Ba(2B) and Ba(4) are occupied by Pb(2), Pb(2B) and Pb(4), respectively. The difference is that there are two additional partially occupied Pb sites, Pb(5) and Pb(6). Pb(5) is connected to Pb(1) or Pb(1B) by corner sharing; Pb(6) is connected to Pb(4) by edge sharing. Pb(5) and Pb(6) are not directly connected to the anion clusters, but are suspended in the channels of the 3-D framework.
[0069] The material after elution has changed relatively little compared to before the exchange. The original Ba(1) position is now occupied by Ba(1) and Pb(1); the positions of Ba(2) and Ba(2B) are now occupied by Ba(2) and Pb(2), and there is no obvious change in other positions.
[0070] In addition, since most of the metal ions in the three compounds are partially occupied, the counter cation H + The number of ions and the number of coordinated water and crystallographic water molecules also vary slightly.
[0071] Example 3: Adsorption kinetics of lead (II) on Ba-Zn-Sb oxygen cluster-based materials
[0072] The Ba-Zn-Sb oxygen-based material was mixed with a lead (II) solution of a certain initial concentration, and stirred at room temperature according to the condition of V (solution volume): m (exchanger mass) = 1000 mL / g. A small amount of the supernatant was taken at a certain interval, and the ion concentration was measured by inductively coupled plasma mass spectrometry. The test results are as follows: Figure 3 As shown in Table 1, the adsorption of lead by the crystalline Ba-Zn-Sb oxygen-cluster-based material gradually reaches equilibrium in 20 minutes.
[0073] Table 1 Removal of Pb by Ba-Zn-Sb oxygen-based materials 2+ Ion kinetic test results
[0074] Time (min) <![CDATA[C e Pb (mg / L)]]> Removal rate (%) 0 100.65 0 1 49.90 50.42 5 34.48 65.75 10 28.90 71.29 20 25.69 74.48 30 24.92 75.24 60 24.45 75.71 120 23.54 76.62 300 24.75 75.41 600 25.80 74.37 720 26.04 74.13
[0075] Example 4. Isothermal adsorption model test of Ba-Zn-Sb oxygen cluster-based materials for lead (II)
[0076] The Ba-Zn-Sb oxygen-based material was mixed with aqueous solutions of different initial lead nitrate concentrations. The mixture was stirred at room temperature for 10 hours under the condition of V (solution volume): m (exchange agent mass) = 1000 mL / g. After the adsorption was completed, the supernatant and the initial solution were taken and the lead concentration was determined by inductively coupled plasma mass spectrometry. The experimental results are shown in Figure 2. Figure 4 As shown in Table 2, the adsorption capacity of Ba-Zn-Sb oxygen cluster-based material for lead is 199.29±5.86 mg / g.
[0077] Table 2 Removal of Pb by Ba-Zn-Sb oxygen-based materials 2+ Isothermal adsorption model test of ions
[0078]
[0079]
[0080] Example 5: Testing of the Ability of Ba-Zn-Sb Oxygen Cluster-Based Materials to Enrich and Recover Lead (II) at Different pH Values
[0081] The Ba-Zn-Sb oxygen-based material was mixed with a lead solution of different pH values, and stirred at room temperature for 10 hours under the condition of V (solution volume): m (exchange agent mass) = 1000 mL / g. After the adsorption was completed, the supernatant and the initial solution were taken and the lead concentration was determined by inductively coupled plasma mass spectrometry. The results are shown in Figure 2. Figure 5 As shown in Table 3, the Ba-Zn-Sb oxygen cluster-based material can maintain the removal activity for uranium in the pH range of 3.94 to 7.20. The method for removing lead from water provided in the present application has a strong removal ability for lead in a wide pH activity range.
[0082] Table 3 Test of the ability of Ba-Zn-Sb oxygen-based materials to remove lead (II) at different pH values
[0083]
[0084] Example 6: Test of the ability of Ba-Zn-Sb oxygen cluster-based materials to remove lead (II) in a solution rich in competitive ions
[0085] The Ba-Zn-Sb oxygen cluster-based materials were mixed with single competitive ions M (M = Mn 2+ 、Co 2+ 、Ni 2+ , Cu 2+ 、Cd 2+ ) was mixed with a lead solution and stirred at room temperature for 10 hours under the condition of V (solution volume): m (exchange agent mass) = 1000 mL / g. After the adsorption was completed, the supernatant and the initial solution were taken and the lead concentration was determined by inductively coupled plasma mass spectrometry. The experimental results are shown in Table 4 and Figure 6 As shown. When the competing ion M in the solution 2+ When the molar ratio of ions is 1:1, the compound has a 2+ The ion removal rate is greater than 66.65%, and the distribution coefficient is greater than 1.999×10 3 g / mL, and the maximum distribution coefficient for competing ions is only about 0.16×10 3 g / mL. When the molar ratio is 10:1, the compound has an 2+ ions still have a removal rate of about 50%, K d The values are all within 1.000×10 3 g / mL, and the K d The value is only 0.083×10 3 Even when the molar ratio was 50:1, although the competitive ions had a greater impact on the adsorption of lead ions, the removal rate was still about 20%, K dThe value also remains greater than 0.200×10 3 The above experimental results fully prove that Ba-Zn-Sb oxygen cluster-based materials have a strong 2+ Ions have excellent selectivity.
[0086] Table 4 Test of the ability of Ba-Zn-Sb oxygen cluster-based materials to remove lead (II) in the presence of single competitive ions at different molar ratios
[0087]
[0088]
[0089] At the same time, the Ba-Zn-Sb oxygen cluster-based material was mixed with lead solutions of different types of competitive ions at different molar ratios. The adsorbent still had a strong affinity for Pb. 2+ The ions were captured with high selectivity. The experimental results are shown in Table 5 and Figure 6 As shown. When the ions in the solution are 2+ When the molar ratio of ions is 1:1, the compound maintains a removal rate of 66.82% for lead ions. d The value remains at 2.012×10 3 g / mL. When each ion is combined with Pb 2+ When the molar ratio of ions is 2:1, R Pb Still 63.28%, K d The value is 1.724×10 3 g / mL. Even when the molar ratio was 5:1, the removal rate of lead ions remained at 49.95%, K d The value can still be maintained at 0.998×10 3 Through the mixed competitive ion experiment, it can also be determined that the affinity of Ba-Zn-Sb oxygen cluster-based materials to each ion is roughly in the order of Pb 2+ >Cu 2+ >Cd 2+ >Ni 2+ >Co 2+ >Mn 2+ In summary, whether from the results of single competitive ion or mixed competitive ion experiments, even when the competitive ions are present in excess, the Ba-Zn-Sb oxygen cluster-based materials still maintain excellent selectivity for lead ions.
[0090] Table 5 shows the test of the removal of lead (II) by Ba-Zn-Sb oxygen cluster-based materials in the presence of various competitive ions at different molar ratios.
[0091]
[0092]
[0093] Example 7: Cyclic test of Ba-Zn-Sb oxygen cluster-based materials
[0094] After grinding, Ba-Zn-Sb oxygen cluster-based materials adsorb Pb 2+ The product after the adsorption of ions is recorded as Pb-Zn-Sb. The Ba-Zn-Sb oxygen-based material is mixed with a lead nitrate solution, the mixture is stirred at room temperature for 10 hours, centrifuged, and the supernatant is filtered with a filter to determine the lead ion concentration in the solution. The sample is washed several times with deionized water and anhydrous ethanol and then dried at room temperature to obtain the adsorbed Pb 2+ ion products.
[0095] The obtained sample was immersed in a 0.1M barium nitrate solution, V (volume of solution): m (mass of exchange agent) = 1000mL / g, and stirred at room temperature for 10 hours. After the reaction was completed, the suspension was taken, and the concentration of lead ions in the solution was determined after filtration. Three adsorption-elution cycle experiments were carried out in this way. As shown in the figure, the removal rate of the sample was higher than 70% in three cycles. It shows that the crystalline material provided by this application can be recycled.
[0096] Example 8: Application of simulated ion adsorption column
[0097] 0.1 g of Ba-Zn-Sb oxygen cluster-based material sample was filled in the ion exchange column, and the column volume was measured to be about 0.047 cm -3 According to the literature, a simulated lead-acid battery waste solution was prepared. The mixed solution contained Pb 2+ 、Ni 2+ and Cd 2+ ions, and the initial concentrations of each ion were 55.75 mg / L, 0.935 mg / L and 0.915 mg / L, respectively. The mixed solution was passed through the adsorption column at a flow rate of 1 mL / min by a peristaltic pump. Liquid samples were collected every 5 minutes using an automatic collection device.
[0098] The experimental results are as follows Figure 8 As shown. Testing the concentration of each ion in the liquid sample collected in the first test tube (i.e., the bed volume is about 26.60) shows that: at this time, the ion exchange column has a high removal rate for each ion, but the removal rate for lead ions is still the highest among the three ions, reaching 99.924%. As the volume of the treated wastewater continues to increase, the removal rate of each ion is gradually decreasing, but Ni 2+ and Cd 2+ The downward trend of ions is particularly obvious. When the treatment bed volume increases to 106.38, the removal rate is only 35.294% (Ni 2+ ) and 56.284% (Cd 2+), and the removal rate of lead ions is still 98.655%. When the bed volume increases to 265.96, the removal rate of lead ions is still maintained at 95.614%, and at this time Ni 2+ and Cd 2+ The removal rates of lead ions were only 9.626% and 19.126% respectively. When the bed volume increased to 611.20, the removal rate of lead ions was still greater than 90%, while the removal rates of the other two ions were less than 10%. When the treatment bed volume increased to 984.04, the removal rate of lead was still 84.09%, while the removal rates of nickel ions and cadmium ions were only 4.278% and 1.093%. In summary, with the continuous increase of the volume of the wastewater bed, the removal rates of the three compounds will decrease accordingly. As of 984.04 column volumes, the removal rate of lead ions was still greater than 84%, while the removal rates of the other two ions were less than 5%, which fully proved that Ba-Zn-Sb oxygen cluster-based materials have excellent selectivity for lead ions. It shows that Ba-Zn-Sb oxygen cluster-based materials have the potential for selective extraction of lead ions in actual industrial wastewater environments.
[0099] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A crystalline material, characterized in that: The chemical formula of the crystalline material is C 24 H 59.03 Ba 2.485 O 70 Sb 12 Zn2.
2. The crystalline material according to claim 1, characterized in that The crystal material is a triclinic system, and the space group is The unit cell parameters of the crystal material are: α=69.57~69.67°, β=70.19~70.29°, γ=88.93~89.03°, Z=2.
3. The crystal material according to claim 1, characterized in that The unit cell parameters of the crystal material are: α=69.5710(10)°, β=70.1960(10)°, γ=88.9380(10)°, 4. The crystalline material according to claim 1, characterized in that The structure of the crystalline material is: Anion cluster [Zn2Sb 12 (μ3-O)8(μ4-O)3(tta)6] 6- (H4tta=tartaric acid) as the main framework, each anion cluster is connected to six Ba 2+ ions, four of which are fully occupied Ba(1), and one each of partially occupied Ba(2) and Ba(3); Each Ba(1) ion connects four adjacent anion clusters, so that the anion clusters partially form a wavy layer; the partially occupied Ba(2) and Ba(3) are connected to each other in an edge-sharing manner by sharing oxygen atoms, and then Ba(3) self-aggregates through oxygen atom edge sharing to form a "z"-shaped scaffold of a tetranuclear cluster; Preferably, the "z"-shaped bracket connects adjacent wave layers along the c-axis direction to form a three-dimensional frame structure; The partially occupied Ba(4) is connected to Ba(2) and Ba(3) in a co-point manner, turning the original four-core cluster into a six-core cluster. Ba(4) is not directly connected to the wavy layer formed by Ba(1) but is suspended in the pores of the anion framework.
5. A method for preparing the crystalline material according to any one of claims 1 to 4, characterized in that: The following steps are involved: In a sealed container, raw materials containing an antimony source, a zinc source and a barium source are mixed with a solvent and reacted to obtain the crystalline material.
6. The preparation method according to claim 5, characterized in that: The antimony source is selected from potassium antimony tartrate; The zinc source is selected from zinc nitrate; The barium source is selected from barium nitrate.
7. The preparation method according to claim 5, characterized in that: The mass ratio of the antimony source, the zinc source and the barium source is 0.11-0.12: 0.108-0.115: 0.1-0.
11.
8. The preparation method according to claim 5, characterized in that: The mass ratio of the antimony source in the raw material to the volume ratio of the solvent is 0.11 g: 3-4 mL.
9. The preparation method according to claim 5, characterized in that: The reaction temperature is 80-100°C; The reaction time is 3 to 5 days.
10. Use of the crystal material according to any one of claims 1 to 4 for highly selective capture of lead (II) ions in water.