Linear low-density metallocene polyethylene resin, linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bag and preparation method of linear low-density metallocene polyethylene resin
The linear low-density metallocene polyethylene resin was prepared through the gas-phase polymerization process, which solved the problems of insufficient puncture resistance and polyethylene impurity pollution of polycrystalline silicon packaging bags, and achieved a high-purity and puncture-resistant packaging film, which was suitable for efficient packaging of polycrystalline silicon.
Patent Information
- Application Number
- CN202411489359.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-10-24
AI Technical Summary
The existing polysilicon packaging bags have insufficient puncture resistance, and polyethylene raw materials may contain impurities, resulting in polysilicon contamination.
The linear low-density metallocene polyethylene resin was prepared by gas-phase polymerization. By adjusting the comonomer and reaction conditions, controlling the molecular structure and density, improving puncture resistance and reducing impurity content, high-purity linear low-density metallocene polyethylene was prepared. Vinyl packaging film.
It significantly improves the puncture resistance and cleanliness of polycrystalline silicon packaging bags, reduces the content of surface impurities and bulk impurities, improves the electrostatic performance and thermal strength, and is suitable for packaging of high-purity polycrystalline silicon.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of petrochemical industry, and specifically relates to a linear low-density metallocene polyethylene resin, a linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags and a preparation method thereof. Background Art
[0002] At present, polysilicon is widely used in the semiconductor and solar energy industries. Due to the extreme fear of contamination, it needs to be packaged before transportation. At present, polyethylene packaging bags are generally used to package polysilicon. For example, a Chinese patent document with publication number CN105017601A discloses a polysilicon packaging film, which is prepared from raw materials including three LDPEs with different melt indexes and lubricants; the raw materials may also include a polyimide oligomer mixture and 1,3,5-triaminobenzene. However, due to the low puncture resistance of the packaging bag, the polysilicon block is vibrated and bumped during transportation and storage, and the packaging bag is cut and punctured by the sharp-edged polysilicon block, exposing the polysilicon block to the air, resulting in contamination of the polysilicon block.
[0003] At present, in order to improve the puncture resistance of polysilicon packaging bags, the existing technology generally improves the performance of polysilicon packaging bags by changing the shape of the packaging bags, adding processing aids and formulas, etc.
[0004] The Chinese patent document with the authorization announcement number CN219707743U discloses a clean PE bag for polysilicon packaging, which includes a first bag body and a second bag body, wherein the first bag body is placed inside the second bag body, and a bubble film is arranged inside the first bag body, with the bubble side of the bubble film facing inward. By laying the bubble film inside the first bag body and making the bubble film face inward, the contact surface between the polysilicon and the first bag body is reduced, thereby reducing the risk of the polysilicon piercing the first bag body; by installing Velcro on the upper end and the middle part of one side of the second bag body, the first bag body is tightened by the second bag body, thereby preventing the first bag body from moving inside the second bag body, reducing the friction between the polysilicon, and further reducing the risk of the polysilicon piercing the first bag body.
[0005] A Chinese patent document with authorization announcement number CN220683315U discloses a high-purity polysilicon packaging bag, including an inner bag and an outer bag, both of which have a first side, a second side, a first edge, a second edge and a third edge, and a chamber is formed between the two side surfaces by sealing the edges, the inner bag is placed in the outer bag with a gap, the chamber of the inner bag is the first space, and the space between the inner bag and the outer bag is the second space; the inner bag also has a mesh, and the mesh distribution density is between 10% and 90%; high-purity polysilicon is placed in the first space, and silicon powder that falls is collected in the second space; a high-purity polysilicon packaging bag is formed by sealing the edges of the two side surfaces, and mesh holes are provided on the inner bag to facilitate the falling of silicon powder generated by friction between the high-purity polysilicon.
[0006] The Chinese patent document with the publication number CN113232393A discloses an electronic-grade polysilicon packaging bag and a production method thereof, wherein the electronic-grade polysilicon packaging bag comprises an inner layer, an intermediate layer and an outer layer, wherein the inner layer comprises 100% LLDPE by weight, the intermediate layer comprises 68-72% metallocene PE and 32-28% LLDPE by weight, and the outer layer comprises 85% LLDPE and 15% auxiliary materials by weight, wherein the auxiliary materials contain conductive materials; and the thickness ratio between the inner layer, the intermediate layer and the outer layer is 2:4:4. The electronic-grade polysilicon packaging bag of this structure makes full use of the tensile, penetration, impact and tear resistance of LLDPE, as well as the penetration resistance of metallocene PE, and adopts a structure of pure LLDPE in the inner layer, which can effectively reduce the surface metal precipitation rate and is very suitable for the packaging of polysilicon.
[0007] However, the polyethylene used in the prior art may contain a certain amount of impurities. For polysilicon used in the electronics industry, the impurity concentration on the surface of the packaging bag is too high, which will directly lead to polysilicon contamination. Therefore, it is necessary to improve the production process and formula to obtain polyethylene raw materials with excellent puncture resistance and extremely low impurity content for the preparation of polysilicon packaging film. Summary of the invention
[0008] In order to solve the above-mentioned problems existing in the prior art, the purpose of the present invention is to provide a linear low-density metallocene polyethylene resin, a linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags and a preparation method thereof, so as to improve the performance of polycrystalline silicon packaging bags by improving the cleanliness and mechanical properties of the linear low-density metallocene polyethylene used as the raw material of the polycrystalline silicon packaging bags.
[0009] In order to achieve the above object, the present invention adopts the following technical solutions.
[0010] In a first aspect, the present invention provides a linear low-density metallocene polyethylene resin, wherein the melt flow rate (or melt index or melt flow index) of the linear low-density metallocene polyethylene resin is 0.7 g / 10 min to 1.3 g / 10 min (test conditions: 190° C., 2.16 kg), and the linear low-density metallocene polyethylene resin is obtained according to the following preparation method: 1) In a gas phase polymerization process, using materials including ethylene, hydrogen, comonomer, nitrogen and condensing agent as raw materials, adjusting the gas phase components in the reactor, and using a metallocene catalyst to complete the polymerization reaction to obtain a linear low-density metallocene polyethylene powder; wherein the comonomer is a blend of hexene and octene, and the molar ratio of the hexene to the octene is 3:2 to 4:1; 2) The linear low-density metallocene polyethylene powder, antioxidant and auxiliary antioxidant are mixed and then kneaded and melted to obtain a linear low-density metallocene polyethylene resin.
[0011] The linear low-density metallocene polyethylene resin, the molecular weight of the linear low-density metallocene polyethylene powder obtained in step 1) is 60000 g / mol to 350000 g / mol, and the molecular weight distribution index is 1 to 4; the density of the linear low-density metallocene polyethylene powder is 0.910 g / cm 3 Up to 0.928 g / cm 3 .
[0012] In the above linear low-density metallocene polyethylene resin, in step 1), the total molar concentration of hexene and octene accounts for 1.4% to 18% of the molar concentration of ethylene. That is, the total molar concentration of hexene and octene is 1.4% to 18% of the molar concentration of ethylene.
[0013] The present invention adopts a blend of hexene and octene as a comonomer to control the molecular structure of a metallocene polyethylene resin (mPE) (specifically, the present invention controls the density of a linear low-density metallocene polyethylene resin by controlling the ratio of the comonomers (hexene and octene) to ethylene), thereby obtaining a linear low-density metallocene polyethylene resin (mLLDPE) having a linear molecular structure, which is beneficial to improving the puncture resistance of mLLDPE.
[0014] In the above linear low-density metallocene polyethylene resin, in step 1), the ethylene partial pressure in the gas phase component is 2500 KPa to 2700 KPa.
[0015] In the above linear low-density metallocene polyethylene resin, in step 1), the molar ratio of hydrogen to ethylene in the gas phase component is 0.0001 to 0.0003:1.
[0016] The present invention controls the melt flow ratio (MFR) of the product by the ratio of hydrogen to ethylene, thereby controlling the molecular weight distribution index of the linear low-density metallocene polyethylene powder. In addition, the present invention can appropriately improve the reaction activity by adjusting the gas phase components in the reactor so that the ethylene partial pressure in the gas phase components is 2500 KPa to 2700 KPa and the molar ratio of hydrogen to ethylene is 0.0001 to 0.0003:1, and obtains puncture-resistant linear low-density metallocene polyethylene powder through polymerization reaction.
[0017] In the above-mentioned linear low-density metallocene polyethylene resin, in step 2), the antioxidant includes 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (molecular formula C 35 H 62 O 3) and pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate].
[0018] The above-mentioned linear low-density metallocene polyethylene resin, the auxiliary antioxidant includes tris[2,4-di-tert-butylphenyl]phosphite (molecular formula C 42 H 63 O 3 P), at least one of tris(nonylphenyl)phosphite and distearyl pentaerythritol diphosphite.
[0019] In the present invention, the linear low-density metallocene polyethylene powder only uses common antioxidants and auxiliary antioxidants, and does not use processing aids such as zinc stearate or calcium stearate, thereby ensuring that the obtained linear low-density metallocene polyethylene resin does not contain any metal element impurities and has high purity. This high purity is conducive to the linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags prepared later having very low static electricity content, so the linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags has no effect on the resistivity of the polycrystalline silicon stored therein.
[0020] The linear low-density metallocene polyethylene resin (mLLDPE) prepared by the present invention has tensile strength, puncture resistance, impact resistance and tear resistance, and also has the characteristic of high purity, so that the linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags produced by using the mLLDPE of the present invention as a raw material has low static electricity content, low surface impurities and volume impurity content, high tensile properties, puncture strength and heat sealing properties, and is more suitable as a polycrystalline silicon packaging bag than conventional packaging films.
[0021] In the above-mentioned linear low-density metallocene polyethylene resin, in step 2), based on the mass of the linear low-density metallocene polyethylene powder, the mass fraction of the antioxidant is 0.001% to 0.5%, and the mass fraction of the auxiliary antioxidant is 0.01% to 0.5%.
[0022] In the above-mentioned linear low-density metallocene polyethylene resin, in step 2), the mass fraction of the antioxidant is 0.005% to 0.1% based on the mass of the linear low-density metallocene polyethylene powder.
[0023] In the above-mentioned linear low-density metallocene polyethylene resin, in step 2), based on the mass of the linear low-density metallocene polyethylene powder, the mass fraction of the auxiliary antioxidant is 0.05% to 0.3%.
[0024] In the above-mentioned linear low-density metallocene polyethylene resin, in step 2), based on the mass of the linear low-density metallocene polyethylene powder, the mass fraction of the antioxidant is 0.01% to 0.05%, and the mass fraction of the auxiliary antioxidant is 0.1% to 0.2%.
[0025] In the above linear low-density metallocene polyethylene resin, in step 2), the mixing and melting is carried out by a twin-screw extruder.
[0026] In the present invention, the melt flow rate of the linear low-density metallocene polyethylene resin is tested according to the standard in GB / T 3682. At a temperature of 190° C. and a load of 2.16 kg, the melt flow rate is 0.7 g / 10 min to 1.3 g / 10 min.
[0027] The puncture strength of the linear low-density metallocene polyethylene resin is ≥5N when the film thickness is 0.3 mm.
[0028] In the present invention, during the extrusion process of a twin-screw extruder, a linear low-density metallocene polyethylene powder, an antioxidant and an auxiliary antioxidant are mixed and added to the barrel of the extruder in a certain proportion for mixing and melting. By adjusting the content of the antioxidant and the auxiliary antioxidant, a linear low-density metallocene polyethylene resin (mLLDPE) with a melt flow rate of 0.7 g / 10 min to 1.3 g / 10 min (190° C., 2.16 kg), a molecular weight distribution index of 2 to 4, and a puncture strength of ≥5N (when the film thickness is 0.3 mm) with high purity and puncture resistance is obtained.
[0029] The present invention produces a linear low-density metallocene polyethylene powder with super strong puncture resistance by adjusting the production process; reduces impurities in the linear low-density metallocene polyethylene powder by changing the reaction conditions and the auxiliary agent formula, and finally obtains a linear low-density metallocene polyethylene resin with high purity and puncture resistance. The linear low-density metallocene polyethylene resin of the present invention is used as a raw material for polycrystalline silicon packaging bags, and the processed polycrystalline silicon packaging bags have excellent puncture resistance and extremely low surface impurity concentration.
[0030] In a second aspect, the present invention provides a method for preparing a linear low-density metallocene polyethylene resin.
[0031] In a third aspect, the present invention provides a linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags, wherein the linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags comprises an inner layer, a middle layer and an outer layer, wherein the mass ratio of the inner layer, the middle layer and the outer layer is 1:(0.9 to 1.1):(0.9 to 1.1); wherein, The inner layer comprises mLLDPE and a lubricant, and the mass ratio of the mLLDPE to the lubricant is 8:1.8 to 2.2; The middle layer includes mLLDPE and a lubricant, and the mass ratio of the mLLDPE to the lubricant is 8.9 to 9.1:1; The outer layer includes mLLDPE; The mLLDPE is a linear low-density metallocene polyethylene resin, which is prepared by the above-mentioned method for preparing the linear low-density metallocene polyethylene resin.
[0032] Since the mLLDPE is prepared by the preparation method of the linear low-density metallocene polyethylene resin, the mLLDPE has the characteristics and properties of linear low-density metallocene polyethylene powder, especially the puncture resistance. In order to make the puncture resistance of the linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags more excellent, in the present invention, the amount of mLLDPE raw materials used in the inner layer, middle layer to outer layer film is increased in sequence.
[0033] The linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags, the lubricant includes one of erucamide and oleamide.
[0034] The linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags has a thickness ratio of 1:2:1 among the inner layer, the middle layer and the outer layer.
[0035] In the present invention, the middle layer thickness of the linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags is designed to be thicker, and more mLLDPE raw materials can be added to the middle layer, so as to increase the film thickness and stiffness while reducing the cost; then, the inner layer and the outer layer to which a lubricant is added are combined on the basis of the mLLDPE raw materials, so that the prepared linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags has better mechanical properties and puncture resistance, and is more suitable for the storage of polycrystalline silicon.
[0036] The linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags has a total thickness of the inner layer, the middle layer and the outer layer of 180 μm to 300 μm.
[0037] The above-mentioned linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags has the following properties: film tensile strength (longitudinal / transverse) ≥46 MPa, film yield stress (longitudinal / transverse) ≥12 MPa, film right-angle tear strength (longitudinal / transverse) ≥110 kN / m, film dart impact strength ≥1370 g, and puncture strength ≥5N.
[0038] In the present invention, the performance of the linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags is tested according to the national standard GB / T 1040, and the film thickness of the linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags is 0.3 mm during the test.
[0039] In a fourth aspect, the present invention provides a method for preparing a linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags, comprising the following steps: (1) Obtaining linear low-density metallocene polyethylene powder; (2) obtaining a linear low-density metallocene polyethylene resin (the linear low-density metallocene polyethylene resin is a pellet); (3) According to the above-mentioned linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags, a linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags is prepared by three-layer co-extrusion blown film.
[0040] In the method for preparing the linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags, in the step (3), before the three-layer co-extrusion blown film is performed, the required amount of mLLDPE is mixed with a lubricant.
[0041] In the method for preparing the linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags, the film blowing is performed using a three-layer co-extrusion film blowing machine.
[0042] According to the technical solution of the present invention, firstly, in the gas phase polymerization process, materials including ethylene, hydrogen, comonomer, nitrogen and condensing agent are used as raw materials, and a metallocene catalyst is used to complete the polymerization reaction. The molecular structure of the linear low-density metallocene polyethylene powder is controlled by adjusting the type of comonomer (using a blend of hexene and octene as a comonomer) and the ratio; based on the ethylene feed amount, the total molar ratio of hexene and octene is controlled to be 1.4% to 18%, and the molar ratio of hexene and octene is 3:2 to 4:1, so as to obtain a puncture-resistant linear low-density metallocene polyethylene powder. Secondly, by adjusting the polymerization reaction parameters (ethylene partial pressure, hydrogen / ethylene molar ratio), the reaction activity is improved and the metal residue of the linear low-density metallocene polyethylene powder is fully reduced. Furthermore, by changing the additive component, the content of metals and impurities in the linear low-density metallocene polyethylene resin is reduced, and finally a high-purity linear low-density metallocene polyethylene resin is obtained. Finally, the linear low-density metallocene polyethylene resin is mixed with a certain amount of lubricant, and a linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags is produced by blowing film through a three-layer co-extrusion film blowing machine.
[0043] In the present invention, the above technical features can be freely combined to form a new technical solution without conflicting with each other.
[0044] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects: (1) The present invention changes the molecular chain structure of the linear low-density metallocene polyethylene powder by changing the comonomer of the polymerization reaction, thereby greatly improving the puncture resistance of the linear low-density metallocene polyethylene powder; (2) The present invention optimizes the gas phase components of the polymerization reaction, improves the reaction activity, reduces the amount of catalyst residue in the resin, and thus significantly reduces the content of metal elements in the resin; at the same time, by optimizing the additive components, the introduction of impurities is reduced, thereby further reducing the content of metal elements in the resin product, and obtaining a high-purity, puncture-resistant linear low-density metallocene polyethylene resin; (3) The present invention adopts the above-mentioned high-purity puncture-resistant linear low-density metallocene polyethylene resin to prepare a linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags, wherein the surface impurity concentration is ≤25 ppbw, the volume impurity concentration is ≤800, the puncture strength is greater than 11 N, the heat sealing strength is ≥30 N, the tensile force is ≥30 N / 15 mm, the elongation at break is ≥900%, and the static electricity content is ≤0.05 kv. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0046] Some embodiments of the present invention provide a method for preparing a linear low-density metallocene polyethylene resin, comprising the following steps: S1: In a gas phase polymerization process, materials including ethylene, hydrogen, comonomer, nitrogen and condensing agent are used as raw materials, the gas phase components in the reactor are adjusted, and a polymerization reaction is completed using a metallocene catalyst to obtain a linear low-density metallocene polyethylene powder; wherein the comonomer is a blend of hexene and octene, and the molar ratio of the hexene to the octene is 3:2 to 4:1; S2: The linear low-density metallocene polyethylene powder prepared in step S1 is mixed with an antioxidant and an auxiliary antioxidant, and then kneaded and melted to obtain a linear low-density metallocene polyethylene resin.
[0047] In some embodiments, in step S1, the total molar concentration of hexene and octene is 1.4% to 18% of the molar concentration of ethylene. That is, the total molar concentration of hexene and octene is 1.4% to 18% (e.g., 2%, 5%, 8%, 10%, 12%, 15% or 17%) of the molar concentration of ethylene.
[0048] In some embodiments, in step S1, the ethylene partial pressure in the gas phase component is 2500 KPa to 2700 KPa (eg, 2550 KPa, 2600 KPa, 2650 KPa, or 2680 KPa).
[0049] In some embodiments, in step S1, the molar ratio of hydrogen to ethylene in the gas phase component is 0.0001 to 0.0003:1 (eg, 0.0002:1).
[0050] In some embodiments, in step S1, the molecular weight of the linear low-density metallocene polyethylene powder is 60,000 g / mol to 350,000 g / mol (e.g., 80,000 g / mol, 100,000 g / mol, 150,000 g / mol, 200,000 g / mol, 250,000 g / mol, 300,000 g / mol or 330,000 g / mol), the molecular weight distribution index is 1 to 4 (e.g., 2 or 3), and the density of the linear low-density metallocene polyethylene powder is 0.910 g / cm 3 Up to 0.928 g / cm 3 (For example, 0.920 g / cm 3 ).
[0051] In some embodiments, in step S2, based on the mass of the linear low-density metallocene polyethylene powder, the mass fraction of the antioxidant is 0.001% to 0.5% (e.g., 0.005%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3% or 0.4%), and the mass fraction of the auxiliary antioxidant is 0.01% to 0.5% (e.g., 0.03%, 0.05%, 0.1%, 0.2%, 0.3% or 0.4%); preferably, the mass fraction of the antioxidant is 0.005% to 0.1% (e.g., 0.006%, 0.007%, 0.010%, 0.011%, 0.012%, 0.013%, 0.014%, 0.015%, 0.016%, 0.017%, 0.018%, 0.019%, 0.1011%, 0.112%, 0.123%, 0.13%, 0.143%, 0.154%, 0.165%, 0.176%, 0.187%, 0.198%, 0.199%, 1010%, 1020%, 1030%, 1040%, 1050%, 1060%, 1070%, 1080%, 1090%, 1110%, 1120%, 1130%, 1140%, 1150%, 8%, 0.01%, 0.03%, 0.05% or 0.08%), the mass fraction of the auxiliary antioxidant is 0.05% to 0.3% (for example, 0.06%, 0.08%, 0.10%, 0.15%, 0.20%, 0.25% or 0.28%); more preferably, the mass fraction of the antioxidant is 0.01% to 0.05% (for example, 0.02%, 0.03% or 0.04%), and the mass fraction of the auxiliary antioxidant is 0.1% to 0.2% (for example, 0.12%, 0.14%, 0.15%, 0.17% or 0.19%).
[0052] In some embodiments, in step S2, the antioxidant includes 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (molecular formula: C 35 H 62 O 3 ) and at least one of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester; the auxiliary antioxidant includes tris[2,4-di-tert-butylphenyl] phosphite (molecular formula C 42 H 63 O 3 P), at least one of tris(nonylphenyl)phosphite and distearyl pentaerythritol diphosphite.
[0053] In some embodiments, in step S2, the mixing and melting is performed using a twin-screw extruder.
[0054] Some embodiments of the present invention further provide a linear low-density metallocene polyethylene resin, which is prepared by the above-mentioned preparation method.
[0055] In some embodiments, the melt flow rate (or melt index or melt flow index) of the linear low density metallocene polyethylene resin is 0.7 g / 10 min to 1.3 g / 10 min (e.g., 0.8 g / 10 min, 0.9 g / 10 min, 1.0 g / 10 min or 1.23 g / 10 min), and the puncture strength of the linear low density metallocene polyethylene resin at a film thickness of 0.3 mm is ≥5N.
[0056] In the present invention, during the extrusion process of a twin-screw extruder, a linear low-density metallocene polyethylene powder, an antioxidant and an auxiliary antioxidant are mixed and added to the barrel of the extruder in a certain proportion for mixing and melting. By adjusting the content of the antioxidant and the auxiliary antioxidant, a linear low-density metallocene polyethylene resin with a melt flow rate of 0.7 g / 10 min to 1.3 g / 10 min (190° C., 2.16 kg), a molecular weight distribution index of 2 to 4, and a puncture strength of ≥5N (when the film thickness is 0.3 mm) with high purity and puncture resistance is obtained.
[0057] Some embodiments of the present invention further provide a linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags, wherein the linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags comprises an inner layer, a middle layer and an outer layer, wherein the mass ratio of the inner layer, the middle layer and the outer layer is 1:0.9 to 1.1:0.9 to 1.1 (for example, 1:1:1); wherein, The inner layer includes mLLDPE and a lubricant, and the mass ratio of the mLLDPE to the lubricant is 8:1.8 to 2.2 (for example, 8:2); The middle layer includes mLLDPE and a lubricant, and the mass ratio of the mLLDPE to the lubricant is 8.9 to 9.1:1 (for example, 9:1); The outer layer includes mLLDPE; The mLLDPE is a linear low-density metallocene polyethylene resin, which is prepared by the above-mentioned method for preparing the linear low-density metallocene polyethylene resin.
[0058] In some embodiments, the lubricant includes at least one of erucamide and oleamide.
[0059] In some embodiments, the thickness ratio of the inner layer, the middle layer, and the outer layer is 1:2:1, and the total thickness of the inner layer, the middle layer, and the outer layer is 180 μm to 300 μm (eg, 200 μm, 220 μm, 250 μm, or 280 μm).
[0060] In some embodiments, the properties of the linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags are: film tensile strength (longitudinal / transverse) ≥46 MPa, film yield stress (longitudinal / transverse) ≥12 MPa, film right-angle tear strength (longitudinal / transverse) ≥110 kN / m, film dart impact strength ≥1370 g, and puncture strength ≥5N.
[0061] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods. The experimental methods in the following examples that do not specify specific conditions are usually measured in accordance with national standards. If there is no corresponding national standard, it is carried out in accordance with the general international standards, conventional conditions, or the conditions recommended by the manufacturer. For example, the melt flow rate of linear low-density metallocene polyethylene resin is tested in accordance with the standard in GB / T 3682; the performance of linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags is tested in accordance with the standard GB / T1040 "Determination of tensile properties of plastics".
[0062] Example 1 A method for preparing a linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags comprises the following steps: S1: In a gas phase polymerization process, ethylene, hydrogen, comonomer, nitrogen, condensing agent, etc. are used as raw materials, and a metallocene catalyst is used to complete the polymerization reaction. Specifically, during the polymerization reaction, the gas phase components in the reactor are adjusted to appropriately increase the reaction activity, wherein the ethylene partial pressure in the gas phase components is 2500 KPa, the molar ratio of hydrogen to ethylene is 0.00025:1, the reaction activity is 8200 kg / kg, and the comonomer is a blend of hexene and octene, the total molar amount of hexene and octene is 1.5% of the molar amount of ethylene, and the molar ratio of hexene and octene is 4:1; a linear low-density metallocene polyethylene powder is obtained through polymerization reaction; S2: During the extrusion process of the twin-screw extruder, the linear low-density metallocene polyethylene powder is fully mixed with the composite antioxidant, wherein the composite antioxidant includes an antioxidant (3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate) and an auxiliary antioxidant (tris[2,4-di-tert-butylphenyl]phosphite), and the addition amounts of the antioxidant and the auxiliary antioxidant are 0.03% and 0.15% of the mass of the linear low-density metallocene polyethylene powder, respectively; after mixing, the mixture is sent into the barrel of the extruder for mixing and melting, and a melt flow rate of 1.03 g / 10 min (190 ° C, 2.16 kg) and a density of 0.9190 g / cm 3 , linear low-density metallocene polyethylene resin with a molecular weight distribution index of 2.3 and a puncture strength ≥5.7N (when the film thickness is 0.3mm).
[0063] S3: The linear low-density metallocene polyethylene resin obtained in step S2 is mixed with a certain amount of lubricant, and a single layer of single material is blown by a three-layer co-extrusion film blowing machine to produce a linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags. Specifically, The three layers of raw materials are prepared according to the following raw material ratios in parts by weight: Inner layer: 10 parts, of which the mass ratio of mLLDPE to lubricant is 8:2; Middle layer: 10 parts, of which the mass ratio of mLLDPE to lubricant is 9:1; Outer layer: mLLDPE 10 parts; The thickness ratio of the inner layer, middle layer and outer layer in the three layers is 1:2:1, and the total thickness is 200 μm.
[0064] Example 2 A method for preparing a linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags comprises the following steps: S1: In a gas phase polymerization process, ethylene, hydrogen, comonomer, nitrogen, condensing agent, etc. are used as raw materials, and a metallocene catalyst is used to complete the polymerization reaction. Specifically, during the polymerization reaction, the gas phase components in the reactor are adjusted to appropriately increase the reaction activity, wherein, in the gas phase components, the ethylene partial pressure is 2600 KPa, the hydrogen / ethylene molar ratio is 0.0002:1, the reaction activity is 8300 kg / kg, the comonomer is a blend of hexene and octene, and the total molar amount of hexene and octene is 1.7% of the molar amount of ethylene; the molar ratio of hexene to octene is 3:2; and a linear low-density metallocene polyethylene powder is obtained through polymerization reaction; S2: During the extrusion process of the twin-screw extruder, the linear low-density metallocene polyethylene powder is fully mixed with the composite antioxidant, wherein the composite antioxidant includes an antioxidant (3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate) and an auxiliary antioxidant (tris[2,4-di-tert-butylphenyl]phosphite), and the addition amounts of the antioxidant and the auxiliary antioxidant are 0.025% and 0.18% of the mass of the linear low-density metallocene polyethylene powder, respectively. Afterwards, the mixture is sent into the barrel of the extruder for mixing and melting to obtain a melt flow rate of 1.01 g / 10 min (190°C, 2.16 kg) and a density of 0.9189 g / cm 3 , linear low-density metallocene polyethylene resin with a molecular weight distribution index of 2.5 and a puncture strength of ≥6.2N (when the film thickness is 0.3mm); S3: The linear low-density metallocene polyethylene resin obtained in step S2 is mixed with a certain amount of lubricant, and a single layer of single material is blown by a three-layer co-extrusion film blowing machine to produce a linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags. Specifically, The three layers of raw materials are prepared according to the following raw material ratios in parts by weight: Inner layer: 10 parts, of which the mass ratio of mLLDPE to lubricant is 8:2; Middle layer: 10 parts, of which the mass ratio of mLLDPE to lubricant is 9:1; Outer layer: mLLDPE 10 parts; The thickness ratio of the inner layer, the middle layer and the outer layer in the three layers is 1:2:1, and the total thickness is 200 μm.
[0065] Comparative Example 1 A method for preparing a polyethylene packaging film suitable for polycrystalline silicon packaging bags comprises the following steps: Low-density polyethylene resins (LDPE-A, LDPE-B and LDPE-C) with melt indexes of 0.9 g / 10 min to 1 g / 10 min, 2.1 g / 10 min to 2.9 g / 10 min, and 0.2 g / 10 min to 0.5 g / 10 min, respectively, were uniformly mixed in a mass ratio of 90:5:20, and a single-layer polycrystalline silicon packaging film with a thickness of 250 μm was prepared by a plastic film casting method; wherein, The density of LDPE-A is 0.910 g / cm 3 Up to 0.925 g / cm 3 , molecular weight distribution index is 4 to 15; The density of LDPE-B is 0.910 g / cm 3 Up to 0.925 g / cm 3 , molecular weight distribution index is 4 to 15; The density of LDPE-C is 0.910g / cm 3 Up to 0.925 g / cm 3 , the molecular weight distribution index is 4 to 15.
[0066] Comparative Example 2 A method for preparing a polyethylene packaging film suitable for polycrystalline silicon packaging bags comprises the following steps: The inner layer is made of metallocene polyethylene resin with a melt index of 0.9 g / 10 min to 1 g / 10 min, LLDPE of 2.1 g / 10 min to 2.9 g / 10 min, and LDPE of 0.2 g / 10 min to 0.5 g / 10 min. The density of the metallocene polyethylene resin is 0.910 g / cm 3 Up to 0.925 g / cm 3 , molecular weight distribution index is 2 to 5; the density of LLDPE is 0.910 g / cm 3 Up to 0.925 g / cm 3 , molecular weight distribution index 2 to 5; LDPE density is 0.910 g / cm 3 Up to 0.925 g / cm 3 , molecular weight distribution index is 4 to 15; The middle layer is made of metallocene polyethylene resin with a melt index of 0.9 g / 10 min to 1 g / 10 min (using the same metallocene polyethylene resin as the inner layer) and LLDPE with a melt index of 2.1 g / 10 min to 2.9 g / 10 min (using the same LLDPE raw material as the inner layer) as the middle layer formula, wherein the mass ratio of the metallocene polyethylene resin to the LLDPE is (60 to 70): (40 to 30); The outer layer is made of LDPE (using the same LDPE raw material as the inner layer) and is co-extruded in three layers. The film thickness is 220 μm, and the thickness ratio of the inner layer, the middle layer and the outer layer in the three layers is 1:2:1.
[0067] Comparative Example 3 A method for preparing a linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags comprises the following steps: S1: preparing a metallocene polyethylene base powder by a conventional method; in a gas phase polymerization process, using ethylene, hydrogen, comonomer, nitrogen, condensing agent, etc. as raw materials, using a metallocene catalyst to complete a polymerization reaction, specifically, in the polymerization process, wherein, in the gas phase component, the ethylene partial pressure is 2200KPa, the molar ratio of hydrogen to ethylene is 0.00024:1, the reaction activity is 6000kg / kg to 7000 kg / kg, the comonomer is hexene, and the total molar amount of hexene is 1.0% to 1.8% of the molar amount of ethylene; obtaining a conventional metallocene polyethylene powder through a polymerization reaction; S2: Preparation of metallocene polyethylene resin: During the extrusion process of the twin-screw extruder, the metallocene polyethylene powder and the composite antioxidant are fully mixed, wherein the composite antioxidant includes an antioxidant (3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate), an auxiliary antioxidant (tris[2,4-di-tert-butylphenyl]phosphite) and a processing aid (zinc stearate), and the addition amounts of the antioxidant, the auxiliary antioxidant and the processing aid are 0.03%, 0.15% and 0.04% of the mass of the metallocene polyethylene powder, respectively; after mixing, the mixture is sent into the barrel of the extruder for mixing and melting to obtain a melt flow rate of 1.01 g / 10 min (test conditions: 190°C, 2.16 kg) and a density of 0.9200 g / cm 3 , a conventional metallocene polyethylene resin with a molecular weight distribution index of 2.5 and a puncture strength of 3N (when the film thickness is 0.3 mm).
[0068] S3: The conventional metallocene polyethylene resin obtained in step S2 is mixed with a certain amount of lubricant, and a single layer of single material is blown by a three-layer co-extrusion film blowing machine to produce a linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags. Specifically, The three layers of raw materials are prepared according to the following raw material ratios in parts by weight: Inner layer: comprising metallocene polyethylene resin and lubricant, with a total weight of 10 parts, wherein the weight ratio of metallocene polyethylene resin to lubricant is 8:2; Middle layer: including metallocene polyethylene resin and lubricant, with a total mass of 10 parts, wherein the mass ratio of metallocene polyethylene resin to lubricant is 9:1; Outer layer: 10 parts of metallocene polyethylene resin; The thickness ratio of the inner layer, the middle layer and the outer layer in the three layers is 1:2:1, and the total thickness is 200 μm.
[0069] Comparative Example 4 A method for preparing a linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags comprises the following steps: S1: preparing metallocene polyethylene powder by conventional method; in a gas phase polymerization process, using ethylene, hydrogen, comonomer, nitrogen, condensing agent and the like as raw materials, using a metallocene catalyst to complete the polymerization reaction, specifically, in the polymerization reaction process, wherein, in the gas phase component, the ethylene partial pressure is 2150 KPa, the molar ratio of hydrogen to ethylene is 0.00023:1, the reaction activity is 5800kg / kg to 6500 kg / kg, the comonomer is hexene, and the total molar amount of hexene is 1.0% to 1.8% of the molar amount of ethylene; obtaining conventional metallocene polyethylene powder by polymerization reaction; S2: preparing metallocene polyethylene resin; specifically, in the process of extrusion by a twin-screw extruder, the metallocene polyethylene powder is fully mixed with a composite antioxidant, wherein the composite antioxidant includes an antioxidant (n-octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate), an auxiliary antioxidant (tris[2,4-di-tert-butylphenyl]phosphite) and a processing aid, and the addition amounts of the antioxidant, the auxiliary antioxidant and the processing aid (zinc stearate) are 0.03%, 0.15% and 0.04% of the mass of the metallocene polyethylene powder, respectively; after mixing, the mixture is sent into the barrel of an extruder for mixing and melting to obtain a melt flow rate of 1.03 g / 10 min (test conditions: 190°C, 2.16 kg) and a density of 0.9198 g / cm 3 , metallocene polyethylene resin mPE with a molecular weight distribution index of 2.4 and a puncture strength of 3.2N (when the film thickness is 0.3mm).
[0070] S3: The metallocene polyethylene resin mPE obtained in step S2 is mixed with a certain amount of conventional LLDPE and a lubricant, and a single layer of single material is blown by a three-layer co-extrusion film blowing machine to produce a metallocene polyethylene packaging film suitable for polysilicon packaging bags. Specifically, The three layers of raw materials are prepared according to the following raw material ratios in parts by weight: Inner layer: LLDPE, mPE and lubricant, with a total mass of 10 parts, wherein the mass ratio of the total mass of LLDPE and mPE to the lubricant is 8:2; the mass ratio of LLDPE to mPE is 1:1; Middle layer: LLDPE, mPE and lubricant, with a total mass of 10 parts, wherein the mass ratio of the total mass of LLDPE and mPE to the lubricant is 9:1; the mass ratio of LLDPE to mPE is 1:1; Outer layer: LLDPE and mPE, with a total mass of 10 parts, of which the mass ratio of LLDPE to mPE is 1:1; The thickness ratio of the inner layer, middle layer and outer layer in the three layers is 1:2:1, and the total thickness is 200 μm.
[0071] Performance Testing: The properties of the polysilicon films prepared in the above examples and comparative examples were tested according to the method in GB / T 1040 "Determination of tensile properties of plastics". The results are shown in Table 1 below.
[0072] It can be seen from Table 1 that, compared with conventional metallocene polyethylene packaging films suitable for polycrystalline silicon packaging bags (Comparative Examples 1 and 2), the linear low-density metallocene polyethylene packaging films suitable for polycrystalline silicon packaging bags prepared by using Examples 1 and 2 of the present invention have very excellent mechanical properties, and the surface impurities, volume impurities and static electricity content are significantly reduced. The lower surface impurities and volume impurities content indicate that the linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags has high purity; the lower static electricity content indicates that the linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags will not have an adverse effect on the resistivity of the polycrystalline silicon stored therein; the higher heat-sealing strength is conducive to better storage of the polycrystalline silicon stored in the packaging film, otherwise, the low heat-sealing strength is easy to cause the seal of the packaging bag to be easily damaged, thereby causing the polycrystalline silicon to be exposed or leaked to the outside and contaminated by external impurities.
[0073] In addition, the difference between Comparative Example 3 and Example 1 is that the metallocene polyethylene resin prepared by conventional methods (firstly preparing metallocene polyethylene powder by conventional methods, and then mixing the metallocene polyethylene powder with antioxidants, auxiliary antioxidants and processing aids to obtain resin) is used to prepare the metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags. The surface impurity and volume impurity content and static electricity content of the obtained metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags are higher than those of the packaging films of Examples 1 and 2, and the heat sealing strength and puncture resistance are lower. In Comparative Example 4, the metallocene polyethylene resin prepared by conventional methods is combined with conventional LLDPE to prepare the metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags. The performance of the obtained metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags is not as good as the performance of the metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags obtained in Examples 1 and 2.
[0074] Therefore, the linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags prepared by the technical solution of the present invention has lower surface impurities and volume impurities content, excellent performance, high heat sealing strength and puncture resistance, low static electricity content, and is more suitable for use as polycrystalline silicon packaging bags.
[0075] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0076] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically directions. In addition, in the description of the present application specification, the terms "include", "comprise", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following (individuals)" or similar expressions thereof refer to any combination of these items, including any combination of singular (individuals) or plural (individuals).
[0077] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
[0078] Table 1 .
Claims
1. A linear low-density metallocene polyethylene resin, characterized in that The melt flow rate of the linear low-density metallocene polyethylene resin is 0.7 g / 10 min to 1.3 g / 10 min, and the linear low-density metallocene polyethylene resin is obtained according to the following preparation method: 1) In a gas phase polymerization process, using materials including ethylene, hydrogen, comonomer, nitrogen and condensing agent as raw materials, adjusting the gas phase components in the reactor, and using a metallocene catalyst to complete the polymerization reaction to obtain a linear low-density metallocene polyethylene powder; wherein the comonomer is a blend of hexene and octene, and the molar ratio of the hexene to the octene is 3:2 to 4:1; 2) The linear low-density metallocene polyethylene powder, antioxidant and auxiliary antioxidant are mixed and then kneaded and melted to obtain a linear low-density metallocene polyethylene resin.
2. The linear low density metallocene polyethylene resin according to claim 1, characterized in that The molecular weight of the linear low-density metallocene polyethylene powder obtained in step 1) is 60,000 g / mol to 350,000 g / mol, and the molecular weight distribution index is 1 to 4; the density of the linear low-density metallocene polyethylene powder is 0.910 g / cm 3 Up to 0.928 g / cm 3 .
3. The linear low density metallocene polyethylene resin according to claim 1 or 2, characterized in that In step 1), the total molar concentration of hexene and octene is 1.4% to 18% of the molar concentration of ethylene; or In step 1), the ethylene partial pressure in the gas phase component is 2500 KPa to 2700 KPa; or / and In step 1), the molar ratio of hydrogen to ethylene in the gas phase component is 0.0001 to 0.0003:
1.
4. The linear low density metallocene polyethylene resin according to claim 3, characterized in that In step 2), the antioxidant includes at least one of 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate; The auxiliary antioxidant includes at least one of tris[2,4-di-tert-butylphenyl]phosphite, tris(nonylphenyl)phosphite and dioctadecyl pentaerythritol diphosphite.
5. The linear low density metallocene polyethylene resin according to claim 1, 2 or 4, characterized in that: In step 2), based on the mass of the linear low-density metallocene polyethylene powder, the mass fraction of the antioxidant is 0.001% to 0.5%, and the mass fraction of the auxiliary antioxidant is 0.01% to 0.5%.
6. The linear low-density metallocene polyethylene resin according to claim 5, characterized in that In step 2), based on the mass of the linear low-density metallocene polyethylene powder, the mass fraction of the antioxidant is 0.005% to 0.1%; the mass fraction of the auxiliary antioxidant is 0.05% to 0.3%.
7. The linear low-density metallocene polyethylene resin according to claim 1, 2, 4 or 6, characterized in that: In step 2), the mixing and melting is carried out using a twin-screw extruder.
8. A method for preparing a linear low-density metallocene polyethylene resin according to any one of claims 1 to 7, characterized in that: The following steps are involved: 1) In a gas phase polymerization process, using materials including ethylene, hydrogen, comonomer, nitrogen and condensing agent as raw materials, adjusting the gas phase components in the reactor, and using a metallocene catalyst to complete the polymerization reaction to obtain a linear low-density metallocene polyethylene powder; wherein the comonomer is a blend of hexene and octene, and the molar ratio of the hexene to the octene is 3:2 to 4:1; 2) The linear low-density metallocene polyethylene powder, antioxidant and auxiliary antioxidant are mixed and then kneaded and melted to obtain a linear low-density metallocene polyethylene resin.
9. A linear low-density metallocene polyethylene packaging film suitable for polysilicon packaging bags, characterized in that: The linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags comprises an inner layer, a middle layer and an outer layer, wherein the mass ratio of the inner layer, the middle layer and the outer layer is 1:0.9 to 1.1:0.9 to 1.1; wherein, The inner layer comprises mLLDPE and a lubricant, and the mass ratio of the mLLDPE to the lubricant is 8:1.8 to 2.2; The middle layer includes mLLDPE and a lubricant, and the mass ratio of the mLLDPE to the lubricant is 8.9 to 9.1:1; The outer layer includes mLLDPE; The mLLDPE is the linear low-density metallocene polyethylene resin, which is prepared by the preparation method of the linear low-density metallocene polyethylene resin as claimed in claim 8.
10. The linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags according to claim 9, characterized in that: The lubricant includes at least one of erucamide and oleamide.
11. The linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags according to claim 10, characterized in that: The thickness ratio of the inner layer, the middle layer and the outer layer is 1:2:
1.
12. The linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags according to any one of claims 9 to 11, characterized in that: The total thickness of the inner layer, the middle layer and the outer layer is 180 μm to 300 μm.
13. A method for preparing a linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags as claimed in claim 12, characterized in that: The method for preparing the linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags comprises the following steps: (1) Obtaining linear low-density metallocene polyethylene powder; (2) obtaining a linear low-density metallocene polyethylene resin; (3) A linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags according to any one of claims 9 to 12 is prepared by three-layer co-extrusion blown film.
14. The method for preparing a linear low-density metallocene polyethylene packaging film suitable for polycrystalline silicon packaging bags according to claim 13, characterized in that: In the step (3), before the three-layer co-extrusion blown film is carried out, the required amount of mLLDPE and the lubricant are mixed.
Citation Information
Patent Citations
Polysilicon packaging film and preparation method for same
CN105017601A
Electronic-grade polycrystalline silicon packaging bag and production method thereof
CN113232393A
Clean PE bag for packaging polycrystalline silicon
CN219707743U
High-purity polycrystalline silicon packaging bag
CN220683315U
Airtight antirust packing film for precise product
CN101020517A