Polymer, polymer electrolyte, solid-state battery and electric equipment

By using polymer electrolyte formed by copolymerization of monomer A and crosslinking agent B in lithium-ion batteries, the problems of low ion conductivity and low lithium ion migration of PEO-based solid electrolyte are solved, and the cycling performance of the battery is improved and Energy density enhances safety performance.

CN118994472AActive Publication Date: 2024-11-22BYD CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410807247.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-11-22
Estimated Expiration
2044-06-20

AI Technical Summary

Technical Problem

The existing PEO-based solid electrolyte has low ion conductivity and low lithium ion migration number, resulting in poor circulation performance of lithium ion batteries.

Method used

A polymer formed by copolymerization of monomer A and crosslinking agent B. Monomer A contains ethoxy groups and ester groups, and the ester group reduces the crystallinity of ethoxy groups and improves the ionic conductivity of the electrolyte; crosslinking agent B improves the electrolyte The mechanical strength of the lithium salt combines to form a high-performance polymer electrolyte.

Benefits of technology

It significantly improves the ion conductivity, lithium ion migration number and mechanical strength of solid-state batteries, improves the cycling performance and energy density of batteries, and enhances safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The embodiment of the invention provides a polymer, a polymer electrolyte, a solid-state battery and electric equipment, the polymer provided by the embodiment of the invention is formed by copolymerizing a monomer A and a cross-linking agent B, the monomer A contains ethyoxyl and an ester group, and the introduction of the ester group can reduce the crystallinity of the ethyoxyl, so that more ethyoxyl can participate in the transmission of lithium ions, and the lithium ion transmission efficiency is improved. The ionic conductivity of the electrolyte is improved; meanwhile, the binding force of ester groups and lithium ions is weaker than that of oxygen atoms and lithium ions, and sites more beneficial to lithium ion transmission can be provided, so that higher ionic conductivity and lithium ion transference number are achieved; by adding the cross-linking agent, the mechanical strength of the electrolyte can be improved; therefore, when the polymer provided by the invention is used for preparing the solid electrolyte, the problem that the cycle performance of a battery is relatively poor due to low ionic conductivity and low lithium ion transference number of the existing PEO-based solid electrolyte can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery manufacturing, and in particular to a polymer, a polymer electrolyte, a solid-state battery and electrical equipment. Background Art

[0002] Currently, lithium-ion batteries are widely used due to their advantages such as high energy density and operating voltage, long cycle life and low self-discharge rate.

[0003] In the prior art, the electrolyte of lithium-ion batteries is generally an organic liquid electrolyte, which has a low flash point, is flammable and easy to leak, and thus poses a great safety hazard.

[0004] In response to the above problems, the existing solid polymer electrolyte based on polyethylene oxide (PEO) has overcome the safety problem and has the advantages of light weight, thinness, and easy processing. It can also be matched with lithium metal as the negative electrode to improve the battery's capacity density.

[0005] However, existing PEO-based solid electrolytes have problems such as low ion conductivity and low lithium ion migration number during use, resulting in poor cycle performance. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a polymer, a polymer electrolyte, a solid-state battery and an electrical device to solve the problem that the existing PEO-based solid-state electrolyte has low ion conductivity and low lithium ion migration number, resulting in poor battery cycle performance.

[0007] In order to solve the above problems, the present invention is achieved through the following technical solutions:

[0008] The present invention provides a polymer, wherein the polymer is copolymerized by a monomer A and a crosslinking agent B, and the monomer A contains an ethoxy group and an ester group.

[0009] Furthermore, in the polymer, the monomer A contains vinyl, and the crosslinking agent B contains divinyl.

[0010] Furthermore, in the polymer, the monomer A comprises a compound having formula (I):

[0011]

[0012] Wherein, R1 is selected from one of hydrogen, halogen, C1-C6 alkyl, C1-C6 alkoxy, and cyano;

[0013] R2 is selected from Any one of; a is an integer between 0 and 10; b, c, and d are each independently an integer between 1 and 20;

[0014] R3 is selected from one of hydrogen and C1-C6 alkyl;

[0015] m is an integer between 1 and 20; n is an integer between 1 and 50.

[0016] Furthermore, in the polymer, the crosslinking agent B comprises a compound having formula (II):

[0017]

[0018] Wherein, R4 is selected from one of hydrogen, halogen, C1-C6 alkyl, C1-C6 alkoxy, and cyano;

[0019] R5 and R7 are each independently one of -O-, -S-, and -NH-;

[0020] R6 is selected from Any one of; e, f, g, h are each independently an integer between 1 and 20.

[0021] Furthermore, in the polymer, the molar ratio of the monomer A to the crosslinking agent B is (70-95):(5-30).

[0022] The present invention also provides a polymer electrolyte, which includes a lithium salt and the polymer as described above.

[0023] Furthermore, in the polymer electrolyte, the molar ratio of the total number of moles of the ethoxy units in the monomer A and the crosslinking agent B to the lithium salt is (25-10):1.

[0024] Furthermore, in the polymer electrolyte, the lithium salt is selected from one or more of lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium perchlorate, lithium tetrafluoroborate, lithium difluorooxalatoborate, and lithium dioxalatoborate.

[0025] The present invention also proposes a solid-state battery, which includes a positive electrode plate, a negative electrode plate and a polymer electrolyte membrane, and the polymer electrolyte membrane includes the polymer electrolyte as described above.

[0026] The present invention also proposes an electrical device, which includes the above-mentioned solid-state battery, and the lithium-ion battery serves as a power supply for the electrical device.

[0027] Compared with the prior art, the embodiments of the present invention have the following advantages:

[0028] In an embodiment of the present invention, the provided polymer is copolymerized by monomer A and crosslinking agent B, wherein monomer A contains ethoxy groups and ester groups, wherein the introduction of ester groups can reduce the crystallinity of ethoxy groups, so that more ethoxy groups can participate in the transmission of lithium ions, thereby improving the ionic conductivity of the electrolyte; at the same time, the binding force between ester groups and lithium ions is weaker than that between oxygen atoms and lithium ions, and sites that are more conducive to lithium ion transmission can be provided, thereby having higher ionic conductivity and lithium ion migration number; and the addition of crosslinking agents can improve the mechanical strength of the electrolyte; therefore, when the polymer provided by the present invention is used to prepare a solid electrolyte, the problem of low ionic conductivity and low lithium ion migration number of existing PEO-based solid electrolytes, which leads to poor battery cycle performance, can be effectively improved.

[0029] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. DETAILED DESCRIPTION

[0030] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below in conjunction with specific implementation methods.

[0031] In existing lithium-ion batteries, the PEO-based solid electrolytes used have low ion conductivity, low lithium ion migration number, and poor mechanical strength, resulting in poor rate performance and cycle performance of the battery.

[0032] In order to solve the above problems, an embodiment of the present invention provides a polymer, wherein the polymer is copolymerized by a monomer A and a cross-linking agent B, and the monomer A contains an ethoxy group and an ester group.

[0033] Among them, the introduction of ester groups can reduce the crystallinity of ethoxy groups, allowing more ethoxy groups to participate in the transmission of lithium ions and improve the ionic conductivity of the electrolyte; at the same time, the binding force between ester groups and lithium ions is weaker than that between oxygen atoms and lithium ions, and can provide sites that are more conducive to lithium ion transmission, thus having higher ionic conductivity and lithium ion migration number, making the rate performance and cycle performance of solid-state batteries better; in addition, the introduction of ester groups can also improve the high-voltage stability of the electrolyte; and the addition of cross-linking agents can improve the mechanical strength of the electrolyte, so that it can match the high-surface-density positive electrode to prepare lithium metal solid-state batteries, so that the batteries have higher energy density and safety performance.

[0034] Therefore, when the polymer provided by the present invention is used to prepare a solid electrolyte, it is possible to effectively improve the problem of low ion conductivity and low lithium ion migration number of existing PEO-based solid electrolytes, which leads to poor battery cycle performance.

[0035] Optionally, in one embodiment, the monomer A contains vinyl, and the crosslinking agent B contains divinyl. The divinyl can be reasonably crosslinked and polymerized with the vinyl in the monomer A, and can effectively improve the mechanical strength of the electrolyte without affecting the ionic conductivity.

[0036] Alternatively, in one embodiment, monomer A comprises a compound having formula (I):

[0037]

[0038] Wherein, R1 is selected from one of hydrogen, halogen, C1-C6 alkyl, C1-C6 alkoxy, and cyano;

[0039] R2 is selected from Any one of; a is an integer between 0 and 10; b, c, and d are each independently an integer between 1 and 20;

[0040] R3 is selected from one of hydrogen and C1-C6 alkyl;

[0041] m is an integer between 1 and 20; n is an integer between 1 and 50.

[0042] Wherein, R2 is selected from When a is 0, the two ester groups at both ends of R2 are directly connected to form oxalic acid ester.

[0043] In the above structural formula (I), the ester group exists between the ethoxy groups, which can effectively reduce the crystallinity of the ethoxy groups, and the ester group is less affected by the terminal olefin group, which can ensure its effective combination with lithium ions.

[0044] Optionally, in one embodiment, the crosslinking agent B comprises a compound having formula (II):

[0045]

[0046] Wherein, R4 is selected from one of hydrogen, halogen, C1-C6 alkyl, C1-C6 alkoxy, and cyano;

[0047] R5 and R7 are each independently one of -O-, -S-, and -NH-;

[0048] R6 is selected from Any one of; e, f, g, h are each independently an integer between 1 and 20.

[0049] In the above structural formula (II), the distance between the two vinyl groups is moderate and the steric hindrance is small, which is not only suitable for the reasonable cross-linking polymerization of the ethoxy and ester groups in monomer A, but also can effectively take into account the ionic conductivity and mechanical strength of the polymer.

[0050] Optionally, in a more specific embodiment, the molar ratio of monomer A and crosslinker B in the polymer is (70-95): (5-30), which can effectively improve the mechanical strength of the polymer electrolyte and will not restrict the movement of polymer chain segments, thereby ensuring that it has good ionic conductivity and contact performance with the positive and negative electrodes.

[0051] The present invention also provides a polymer electrolyte, which includes a lithium salt and the polymer as described above.

[0052] The polymer electrolyte provided by the present invention includes the above-mentioned polymer, which is copolymerized by monomer A and crosslinking agent B. Monomer A contains ethoxyl group and ester group. The crystallinity of ethoxyl group is reduced by combining with ester group, while ester group can provide additional lithium ion transmission site, and crosslinking agent can improve the mechanical strength of electrolyte. The ethoxyl group, ester group and crosslinking agent work together to make the polymer electrolyte have higher ion conductivity, lithium ion migration number and mechanical strength.

[0053] Optionally, in one embodiment, in the polymer electrolyte, the molar ratio of the total number of moles of ethoxy units in monomer A and crosslinker B to the lithium salt is (25-10):1, so that the ethoxy groups can reasonably coordinate with lithium ions, which is not only beneficial to the binding and debinding of lithium ions, but also can effectively improve the ionic conductivity.

[0054] Optionally, in one embodiment, the lithium salt is selected from one or more of lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium perchlorate, lithium tetrafluoroborate, lithium difluorooxalatoborate, and lithium dioxalatoborate, and can be effectively matched with the above-mentioned polymer, so that the electrolyte has higher ionic conductivity and lithium ion migration number, so that the rate performance and cycle performance of the solid-state battery are better.

[0055] The invention provides a method for preparing a polymer electrolyte. The method comprises: uniformly mixing a monomer A, a crosslinking agent B and a lithium salt, adding an initiator to initiate polymerization, and obtaining the polymer electrolyte.

[0056] Among them, the above-mentioned initiator is any one of azobisisobutyronitrile, azobisisoheptylnitrile, dimethyl azobisisobutyrate, benzoyl peroxide, tert-butyl benzoyl peroxide, benzophenone, dibenzophenone, methyl o-benzoylbenzoate, benzoin methyl ether, and benzoin ethyl ether, which can effectively initiate the polymerization and crosslinking of monomer A and crosslinker B.

[0057] The present invention also proposes a solid-state battery, which includes a positive electrode plate, a negative electrode plate and a polymer electrolyte membrane, and the polymer electrolyte membrane includes the above-mentioned polymer electrolyte.

[0058] Among them, the polymer electrolyte not only plays a role in conducting ions between the positive electrode sheet and the negative electrode sheet, but also can effectively isolate the positive electrode sheet and the negative electrode sheet to prevent short circuit.

[0059] The above-mentioned positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer provided on the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes lithium cobaltate (LiCoO2), lithium nickelate (LiNiO2), lithium iron phosphate (LiFePO4), lithium cobalt phosphate (LiCoPO4), lithium manganese phosphate (LiMnPO4), lithium nickel phosphate (LiNiPO4), lithium manganate (LiMnO2), binary material LiNi x A (1-x) O2 (wherein A is selected from one of Co and Mn, 0 < x < 1), ternary material LiNimBnC (1-m-n) O2 (wherein B and C are independently selected from at least one of Co, Al, and Mn, and B and C are different, 0 < m < 1, 0 < n < 1).

[0060] Furthermore, the above-mentioned positive electrode sheet further includes a lithium salt, and the lithium salt is selected from one or more of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium perchlorate, lithium tetrafluoroborate, lithium difluoro(oxalato)borate, and lithium bis(oxalato)borate.

[0061] Furthermore, the lithium salt in the above-mentioned positive electrode sheet is the same as the lithium salt in the polymer electrolyte, ensuring the matching effect between the positive electrode sheet and the electrolyte and improving the conductivity.

[0062] Optionally, in one embodiment, the above-mentioned positive electrode sheet further includes a conductive agent, a binder, and a plasticizer. The conductive agent is selected from at least one of acetylene black, Super P, Super S, graphene, carbon fiber, carbon nanotube, and Ketjen black. The binder is selected from at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polytetrafluoroethylene, polyacrylonitrile, polypropylene carbonate, styrene-butadiene rubber, nitrile rubber, sodium carboxymethyl cellulose, poly(ethylene oxide), and ethylene oxide-propylene oxide copolymer. The plasticizer is selected from at least one of ethylene glycol dimethyl ether, ethylene glycol diethyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol diethyl ether, tetraethylene glycol diethyl ether, dipropylene glycol dimethyl ether, tripropylene glycol dimethyl ether, tetrapropylene glycol dimethyl ether, dipropylene glycol diethyl ether, tripropylene glycol diethyl ether, tetrapropylene glycol diethyl ether, 1,3-dioxolane, 1,4-dioxane, propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, succinonitrile, and adiponitrile.

[0063] Optionally, in one embodiment, the mass ratio of the positive electrode active material, conductive agent, binder, lithium salt and plasticizer in the above-mentioned positive electrode plate is (50-90): (1-10): (9-20): (0-10): (0-10), which can effectively take into account the energy density and ionic conductivity of the battery.

[0064] In some embodiments, the positive electrode sheet is prepared as follows: the components for preparing the positive electrode sheet, such as the positive electrode active material, the binder and any other components, are dispersed in a solvent such as N-methylpyrrolidone to form a positive electrode slurry; the positive electrode slurry is coated on both sides of a positive electrode collector such as aluminum foil; after baking, rolling, cutting and other processes, the positive electrode sheet can be obtained.

[0065] Among them, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer arranged on the negative electrode current collector. The above-mentioned negative electrode active material layer can adopt negative electrode active materials used for batteries, for example, selected from metal negative electrode materials or non-metallic negative electrode materials; the metal negative electrode material is preferably lithium metal or lithium metal alloy; the non-metallic negative electrode material is preferably any one of hard carbon, soft carbon, graphite, silicon oxide, silicon-carbon composite, and silicon alloy, or a combination of at least two of them.

[0066] Furthermore, when the above-mentioned negative electrode active material is selected from non-metallic negative electrode materials, the above-mentioned negative electrode plate also includes a lithium salt, and the above-mentioned lithium salt is selected from one or more of lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium perchlorate, lithium tetrafluoroborate, lithium difluorooxalatoborate, and lithium dioxalatoborate.

[0067] Furthermore, the lithium salt in the negative electrode plate is the same as the lithium salt in the polymer electrolyte, which ensures the matching effect between the negative electrode plate and the electrolyte and improves the conductivity.

[0068] Optionally, in one embodiment, when the negative electrode active material is selected from non-metallic negative electrode materials, the negative electrode plate further comprises a conductive agent, a binder and a plasticizer, the conductive agent is selected from at least one of acetylene black, Super P, Super S, graphene, carbon fiber, carbon nanotubes and Ketjen black, the binder is selected from at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polytetrafluoroethylene, polyacrylonitrile, polypropylene carbonate, styrene-butadiene rubber, nitrile rubber, sodium carboxymethyl cellulose, polyethylene oxide, ethylene oxide-propylene oxide copolymer, the plasticizer is selected from at least one of ethylene glycol dimethyl ether, ethylene glycol diethyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, diethylene ... At least one of glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol diethyl ether, tetraethylene glycol diethyl ether, dipropylene glycol dimethyl ether, tripropylene glycol dimethyl ether, tetrapropylene glycol dimethyl ether, dipropylene glycol diethyl ether, tripropylene glycol diethyl ether, tetrapropylene glycol diethyl ether, 1,3-dioxolane, 1,4-dioxane, propylene carbonate, ethylene carbonate, diethyl carbonate or dimethyl carbonate, succinonitrile, and adiponitrile.

[0069] Optionally, in one embodiment, the mass ratio of the negative electrode active material, conductive agent, binder, lithium salt and plasticizer in the above-mentioned negative electrode plate is (50-90): (1-10): (9-20): (0-10): (0-10), which can effectively take into account the energy density and ionic conductivity of the battery.

[0070] In some embodiments, the negative electrode sheet is prepared as follows: the components for preparing the negative electrode sheet, such as the negative electrode active material, binder and conductive agent, are dispersed in a solvent such as deionized water to form a negative electrode slurry; the negative electrode slurry is coated on both sides of a negative electrode collector such as copper foil; after baking, rolling, cutting and other processes, the negative electrode sheet can be obtained.

[0071] In practical applications, the negative electrode sheet, the polymer electrolyte membrane and the positive electrode sheet are stacked in order, wound to obtain a core, sealed and sorted to obtain the above-mentioned solid-state battery.

[0072] The present invention also proposes an electrical device, which includes the above-mentioned solid-state battery, and the solid-state battery serves as a power supply for the electrical device.

[0073] For the above-mentioned solid-state battery embodiment and electrical equipment embodiment, they include the above-mentioned polymer electrolyte and can achieve the same technical effects. In order to avoid repetition, they will not be described here. For relevant matters, please refer to the partial description of the polymer electrolyte embodiment.

[0074] In order to make the invention purpose, technical scheme and beneficial effect of the present invention clearer, the present invention is further described below in conjunction with embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0075] The present invention is described in detail below by way of examples.

[0076] Example 1

[0077] (1) Preparation of polymer electrolyte membrane:

[0078] The monomer A and the cross-linking agent B were mixed uniformly at a molar ratio of 90:10, and then lithium salt was added at a molar ratio of 15:1 of the total molar amount of ethoxy groups on the monomer A and the cross-linking agent B to the lithium salt, and an initiator was added at 0.5% of the total mass of the monomer A and the cross-linking agent B, and the mixture was heated to 60° C. and polymerized for 4 hours to obtain a polymer electrolyte membrane with a thickness of 40 μm;

[0079] Among them, the structural formula of monomer A is The structural formula of crosslinking agent B is The lithium salt is lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and the initiator is azobisisobutyronitrile (AIBN).

[0080] (2) Preparation of solid-state batteries

[0081] The positive electrode active material lithium iron phosphate, conductive agent Super P, binder polyethylene oxide with a molecular weight of 600,000, lithium salt lithium bis(trifluoromethylsulfonyl)imide and plasticizer succinonitrile were mixed in N,N-dimethylformamide at a mass ratio of 78:2:10:5:5, and then the slurry was applied on the aluminum current collector with a scraper. After that, it was dried at 60°C for 1h and then at 80°C for 3h to obtain the positive electrode sheet. The single-sided surface loading of lithium iron phosphate was 15mg / cm 2 ;

[0082] Cut the positive electrode into 4.5×6cm 2 , a lithium copper alloy strip with a thickness of 15 μm was used as the negative electrode and cut into 4.7×6.2 cm 2 , polymer electrolyte membrane cut into 4.8×6.3cm 2 , in a glove box filled with argon, the positive electrode sheet, polymer electrolyte membrane, and negative electrode sheet are assembled in order to make a solid-state battery.

[0083] Example 2

[0084] The only difference from Example 1 is that, during the preparation of the polymer electrolyte membrane, the molar ratio of monomer A to cross-linking agent B is adjusted to 95:5.

[0085] Example 3

[0086] The only difference from Example 1 is that, during the preparation of the polymer electrolyte membrane, the molar ratio of monomer A to cross-linking agent B is adjusted to 80:20.

[0087] Example 4

[0088] The only difference from Example 1 is that, during the preparation of the polymer electrolyte membrane, the molar ratio of monomer A to cross-linking agent B is adjusted to 70:30.

[0089] Example 5

[0090] The only difference from Example 1 is that, during the preparation of the polymer electrolyte membrane, the molar ratio of monomer A to cross-linking agent B is adjusted to 60:40.

[0091] Example 6

[0092] The only difference from Example 1 is that, during the preparation of the polymer electrolyte membrane, the structural formula of monomer A is adjusted to

[0093] Example 7

[0094] The only difference from Example 1 is that, during the preparation of the polymer electrolyte membrane, the structural formula of monomer A is adjusted to

[0095] Example 8

[0096] The only difference from Example 1 is that, during the preparation of the polymer electrolyte membrane, the structural formula of monomer A is adjusted to

[0097] Example 9

[0098] The only difference from Example 1 is that, during the preparation of the polymer electrolyte membrane, the structural formula of monomer A is adjusted to

[0099] Example 10

[0100] The difference between Example 10 and Example 1 is that, in the preparation process of the polymer electrolyte membrane, the structural formula of the monomer A is adjusted to

[0101] Embodiment 11

[0102] The only difference from Example 1 is that, during the preparation of the polymer electrolyte membrane, the structural formula of the crosslinking agent B is adjusted to

[0103] Example 12

[0104] The only difference from Example 1 is that, during the preparation of the polymer electrolyte membrane, the structural formula of the crosslinking agent B is adjusted to

[0105] Embodiment 13

[0106] The only difference from Example 1 is that, during the preparation of the polymer electrolyte membrane, the molar ratio of the total molar amount of ethoxy groups on the monomer A and the crosslinking agent B to the lithium salt is adjusted to 25:1.

[0107] Embodiment 14

[0108] The only difference from Example 1 is that, during the preparation of the polymer electrolyte membrane, the molar ratio of the total molar amount of ethoxy groups on the monomer A and the crosslinking agent B to the lithium salt is adjusted to 10:1.

[0109] Embodiment 15

[0110] The only difference from Example 1 is that the thickness of the polymer electrolyte membrane is adjusted to 20 μm.

[0111] Example 16

[0112] The only difference from Example 1 is that the thickness of the polymer electrolyte membrane is adjusted to 50 μm.

[0113] Embodiment 17

[0114] The only difference from Example 1 is that the lithium salt is adjusted to lithium tetrafluoroborate.

[0115] Comparative Example 1

[0116] The difference between Comparative Example 1 and Example 1 is that, during the preparation of the polymer electrolyte membrane, the molar ratio of the monomer A to the cross-linking agent B is adjusted to 100:0.

[0117] Comparative Example 2

[0118] The difference between Comparative Example 2 and Example 1 is that, in the process of preparing the polymer electrolyte membrane, the polymer electrolyte is adjusted to consist of 600,000 polyethylene oxide and lithium bis(trifluoromethylsulfonyl)imide.

[0119] Test example:

[0120] 1) The polymer electrolyte membranes prepared in the above embodiments and comparative examples were assembled with stainless steel sheets into a stainless steel symmetrical battery for ion conductivity testing. The testing method is: the symmetrical battery was placed in an oven at 60°C for 10 minutes and then the EIS of the symmetrical battery was tested. According to the formula The ionic conductivity of the polymer electrolyte was calculated; where σ is the ionic conductivity of the electrolyte, L is the thickness of the electrolyte, S is the area of ​​the stainless steel, and R is the impedance of the symmetrical battery; the test results are shown in Table 1.

[0121] The preparation steps of the stainless steel symmetrical battery are as follows:

[0122] Use a punching machine to cut stainless steel sheets with a diameter of 16 mm and a thickness of 200 μm, and polymer electrolyte membranes with a diameter of 19 mm;

[0123] The obtained stainless steel sheets and polymer electrolyte membranes are stacked in order so that the polymer electrolyte membrane is located between the stainless steel sheets, thereby completing the preparation of a stainless steel symmetrical battery.

[0124] 2) The polymer electrolyte membranes prepared in the above embodiments and comparative examples were assembled with lithium sheets into lithium symmetric batteries for lithium ion migration test. The test method is: the symmetric battery was placed in an oven at 60°C for 10 minutes, and then a polarization voltage was applied to the battery using an electrochemical workstation. The current and impedance of the symmetric battery before and after polarization were tested. According to the formula The lithium ion migration number of the electrolyte can be obtained by calculation; where t + is the lithium ion migration number, I0 and I ss are the current before polarization begins and the current after polarization stabilizes, R0 and R ss are the impedance before polarization starts and the impedance after polarization stabilizes, ΔV is the polarization voltage; the polarization voltage is usually 10mV, and the polarization time is usually 2h; the test results are shown in Table 1.

[0125] The preparation steps of the lithium symmetric battery are as follows:

[0126] Use a punching machine to cut lithium sheets with a diameter of 16 mm and a thickness of 200 μm, and polymer electrolyte membranes with a diameter of 19 mm;

[0127] The obtained lithium sheets and polymer electrolyte membranes are stacked in order so that the polymer electrolyte membranes are located between the lithium sheets, thereby completing the preparation of the lithium symmetric battery.

[0128] 2) The solid-state batteries prepared in each embodiment and comparative example were subjected to battery cycle performance tests, and the test data are shown in Table 1; wherein the test method is:

[0129] After placing the battery in a 60°C oven for 10 minutes, first charge it to 3.8V at a constant current rate of 0.05C, then let it stand for 5 minutes, then discharge it to 2.5V at a constant current rate of 0.05C, and repeat the above process three times. Then charge it to 3.8V at a constant current rate of 0.2C, and charge it to 0.01C at 3.8V, then let it stand for 5 minutes, and finally discharge it to 2.5V at a rate of 0.2C, and finally let it stand for 5 minutes. When the battery capacity is 80% of the initial capacity, the battery is considered to be failed, and the number of cycles at this time is recorded.

[0130] Table 1

[0131]

[0132]

[0133] According to the above test data, ethoxy groups and ester groups are introduced into the polymer electrolyte, and a cross-linking agent is added. The ethoxy groups, ester groups and cross-linking agents work together to make the polymer electrolyte have higher ionic conductivity, lithium ion migration number and mechanical strength, and can also improve the cycle performance of solid-state batteries.

[0134] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concept. Therefore, the claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present invention.

[0135] The above is a detailed introduction to a polymer, a polymer electrolyte, a solid-state battery and an electrical device provided by the present invention. Specific examples are used herein to illustrate the principle and implementation mode of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for a person skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation mode and the scope of application. In summary, the content of this specification should not be understood as a limitation on the present invention.

Claims

1. A polymer, characterized in that The polymer is formed by copolymerization of a monomer A and a crosslinking agent B, wherein the monomer A contains an ethoxy group and an ester group.

2. The polymer according to claim 1, characterized in that The monomer A contains a vinyl group, and the cross-linking agent B contains a divinyl group.

3. The polymer according to claim 1 or 2, characterized in that The monomer A includes a compound having formula (I): Wherein, R1 is selected from one of hydrogen, halogen, C1-C6 alkyl, C1-C6 alkoxy, and cyano; R2 is selected from Any one of; a is an integer between 0 and 10; b, c, and d are each independently an integer between 1 and 20; R3 is selected from one of hydrogen and C1-C6 alkyl; m is an integer between 1 and 20; n is an integer between 1 and 50.

4. The polymer according to claim 1 or 2, characterized in that The crosslinking agent B includes a compound having formula (II): Wherein, R4 is selected from one of hydrogen, halogen, C1-C6 alkyl, C1-C6 alkoxy, and cyano; R5 and R7 are each independently one of -O-, -S-, and -NH-; R6 is selected from Any one of; e, f, g, h are each independently an integer between 1 and 20.

5. The polymer according to claim 2, characterized in that In the polymer, the molar ratio of the monomer A to the crosslinking agent B is (70-95):(5-30).

6. A polymer electrolyte, characterized in that The invention comprises a lithium salt and a polymer as claimed in any one of claims 1 to 5.

7. The polymer electrolyte according to claim 6, characterized in that In the polymer electrolyte, the molar ratio of the total molar number of the ethoxy units in the monomer A and the crosslinking agent B to the lithium salt is (25-10):

1.

8. The polymer electrolyte according to claim 6, characterized in that The lithium salt is selected from one or more of lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium perchlorate, lithium tetrafluoroborate, lithium difluorooxalatoborate, and lithium dioxalatoborate.

9. A solid-state battery, comprising a positive electrode sheet and a negative electrode sheet, characterized in that: It also includes a polymer electrolyte membrane, wherein the polymer electrolyte membrane includes the polymer electrolyte according to any one of claims 6 to 8.

10. The lithium ion battery according to claim 9, characterized in that: The thickness of the polymer electrolyte membrane is 20-50 μm.

11. An electrical device, characterized in that: It includes the solid-state battery according to claim 9 or 10, and the solid-state battery serves as a power supply for the electrical equipment.

Citation Information

Patent Citations

  • Electrolyte polymer substrate, solid electrolyte, preparation method of solid electrolyte and lithium ion battery

    CN112442153A

  • Ketone group-containing solid polymer electrolyte and battery

    CN113224382A

  • Solid electrolyte, preparation method and lithium ion battery

    CN115332622A

  • Solid-state electrolyte and solid-state battery comprising same

    CN116247289A

  • Polymer electrolyte prepolymerization liquid, polymer electrolyte and electrochemical device

    CN116525935A