Isocyanate-modified hard thermoplastic polymer composition
By introducing linear polymer polyester diol and diisocyanate into thermoplastic polymers, combining supplementary monomers and branched monomers, the processing and stability problems of existing thermoplastic polymers in high temperature and humid environments have been solved, and high Properties of hard thermoplastic polymers.
Patent Information
- Application Number
- CN202411173247.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2016-04-25
- Filing Date
- 2017-02-15
- Publication Date
- 2024-11-22
AI Technical Summary
The existing thermoplastic polymers are difficult to process at high temperatures and are limited in nature. Traditional hard thermoplastic polyurethanes are costly and easily absorbent, limiting their use in high temperature and humid applications.
An isocyanate modified thermoplastic polymer has been developed, including linear polymer polyester glycol and diisocyanate monomers, with high glass transition temperature and high tensile modulus, suitable for processing at temperatures below 300°C and at Supplementary monomers and branched monomers are introduced into the polymer to improve performance.
Hard thermoplastic polymers processed at low temperatures have properties similar to traditional hard thermoplastic polymers and show better stability and useability in high temperature and humid environments.
Smart Images

Figure CN118994518A_ABST
Abstract
Description
[0001] This application is a divisional application, the application date of the parent application is February 15, 2017, the application number is 201780013021.9, and the name of the invention is "Isocyanate-modified rigid thermoplastic polymer composition". Technical Field
[0002] The present invention relates generally to thermoplastic polymers. In particular, the present invention relates to thermoplastic polymer compositions having desirable properties, and methods of making and using the same. Background Art
[0003] Thermoplastic polymers can be used in a wide variety of applications, including, for example, various electrical, automation, medical, consumer, industrial and packaging applications. The advantage of thermoplastic polymers over thermosetting plastics is that thermoplastic polymers can be easily melt processed into a variety of useful articles. Different types of thermoplastic polymers have different properties that make them desirable for certain end uses. Elastomeric thermoplastic polymers have glass transition temperature values below room temperature and low modulus values that make them suitable for applications that require flexibility and stretchability. In contrast, rigid thermoplastic polymers have glass transition temperature values above room temperature and high modulus values that make them suitable for applications that require stiffness and strength.
[0004] Thermoplastic polyesters are a class of thermoplastic polymers that are generally formed by the polycondensation of monomeric diacids and monomeric diols. Thermoplastic polyesters can be elastomeric or rigid, but the vast majority are rigid. Rigid thermoplastic polyesters exhibit desirable properties, such as dimensional stability, chemical resistance, heat resistance, low creep, low haze, good color stability, and / or toughness, depending at least in part on the specific composition and morphology of the material. However, thermoplastic polyesters must be processed at elevated temperatures that can cause molecular weight degradation, which adversely affects the properties of the final material. Furthermore, thermoplastic polyesters degrade significantly at temperatures above 300°C, and therefore the use of these materials in high temperature applications is very limited.
[0005] Thermoplastic polyurethanes (TPUs) are another class of thermoplastic polymers that are formed by the reaction of isocyanates and diols. The vast majority of TPUs have glass transition temperature values well below room temperature and have low modulus values, and are therefore mostly elastomeric or at most partially rigid. Therefore, conventional thermoplastic polyurethanes are not used in applications that require polymers that exhibit high stiffness and strength. Rigid thermoplastic polyurethanes (RTPUs) can be prepared by incorporating very high amounts of isocyanate residues into TPUs, but such polymers are expensive and not widely used. In addition, although these polymers have higher dry glass transition temperatures than other thermoplastic polyurethanes, RTPUs are highly hygroscopic, which ultimately suppresses the glass transition temperature, thereby limiting the usability of these materials in wet applications.
[0006] Therefore, there is a need for a rigid thermoplastic polyester composition that can be processed at temperatures well below 300° C. In particular, this can provide a rigid thermoplastic polyester composition that can be processed (e.g., molded) and that can be suitable for use in high temperature applications. Desirably, the polymer will be compatible with existing thermoplastic processes and equipment and can be used in many types of articles, and will exhibit properties similar to or better than articles formed from conventional rigid thermoplastic polymers. Summary of the invention
[0007] One aspect of the present invention relates to thermoplastic polymers. In an embodiment of the present invention, the thermoplastic polymer comprises residues of at least one linear polymerized polyester diol, wherein the linear polymerized polyester diol comprises residues of at least one monomeric diacid and at least one monomeric diol, and the linear polymerized polyester diol has a number average molecular weight of at least 400 Daltons. In an embodiment, the thermoplastic polymer further comprises residues of at least one diisocyanate monomer, and the residues of the diisocyanate monomer are present in the polymer in an amount of no greater than 40 weight percent based on the total weight of the polymer. In an embodiment, the polymer has a glass transition temperature of at least 140°C.
[0008] In certain embodiments, the linear polymeric polyester diol has a glass transition temperature of at least 35°C or at least 40°C. In one embodiment, the monomeric diol is selected from 2,2,4,4-tetramethyl-1,3-cyclobutanediol, isosorbide, 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, ethylene glycol, 2,2' ((sulfonylbis(4,1-phenylene))bis(oxy)diethanol, 2,6-decalinedimethanol, tricyclodecane dimethanol, 1,4-benzenedimethanol, 2,2'-(1,4-phenylenebis(oxy))diethanol, 2,2'-(2,4,8,10-tetraoxaspiro(5,5)undecane-3,9-diyl)bis(2-methylpropan-1-ol), neopentyl glycol, and combinations thereof. In one embodiment, the linear polymeric polyester diol comprises residues of at least two monomeric diols. In one embodiment, the linear polymeric polyester diol comprises residues of at least two monomeric diols selected from 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 1,4- Cyclohexanedimethanol and ethylene glycol; or selected from 2,2,4,4-tetramethyl-1,3-cyclobutanediol, and at least one of 1,4-cyclohexanedimethanol or ethylene glycol. In certain embodiments, the monomer diacid is selected from terephthalic acid, dimethyl terephthalic acid, 4,4-sulfonyl dibenzoic acid, resorcinol-o,o'diacetic acid, dimethyl succinate, dimethyl biphenyl 4,4'-dicarboxylate, 1,4 cyclohexanedicarboxylic acid, 4,4'-stilbene dicarboxylic acid, 4,4'-isopropylidene diphenoxyacetic acid, dimethyl isophthalate, dimethyl 2,6-naphthalene dicarboxylate, dimethyl decalin-2,6-dicarboxylate, succinic acid, furandicarboxylic acid dimethyl ester and combinations thereof; or selected from terephthalic acid, dimethyl terephthalic acid and combinations thereof.
[0009] In an embodiment of the present invention, the monomeric diol is selected from 2,2,4,4-tetramethyl-1,3-cyclobutanediol, isosorbide, 1,4-cyclohexanedimethanol, ethylene glycol, 2,6-decalin dimethanol, 1,4-benzenedimethanol and combinations thereof and / or the monomeric diacid is selected from terephthalic acid, dimethyl terephthalic acid, 4,4-sulfonyldibenzoic acid, dimethyl biphenyl 4,4'-dicarboxylate, 1,4-cyclohexanedicarboxylic acid, 4,4'-stilbene dicarboxylic acid, dimethyl isophthalate, dimethyl 2,6-naphthalene dicarboxylate, dimethyl decalin-2,6-dicarboxylate and combinations thereof.
[0010] In certain embodiments, the diisocyanate monomer comprises an aromatic diisocyanate monomer. In one embodiment, the diisocyanate monomer comprises 4,4'-diphenylmethane diisocyanate.
[0011] In certain embodiments, the polymer further comprises at least 0.5 wt % of the residue of at least one supplementary monomeric diol, based on the total weight of the polymer. In some embodiments, the polymer further comprises at least 0.5 wt % of the residue of at least one supplementary monomeric diol, based on the total weight of the polymer, wherein the supplementary monomeric diol is selected from 2,2,4,4-tetramethyl-1,3-cyclobutanediol, isosorbide, 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, ethylene glycol, 2,6-decalin, tricyclodecane dimethanol, 1,4 benzenedimethanol, neopentyl glycol, and combinations thereof.
[0012] In some embodiments, the polymer further comprises residues of at least one branching monomer and / or at least one polyfunctional isocyanate, wherein the total amount of the residues of the branching monomer and the polyfunctional isocyanate present in the polymer is no greater than 1 wt %, based on the total weight of the polymer.
[0013] In certain embodiments, the polymer has a number average molecular weight of at least 10,000 Daltons. In embodiments, the polymer has a tensile modulus of at least 1000 MPa. In embodiments, the lower processing temperature (T p ) and glass transition temperature (T g ) is not more than 135°C, or not more than 110°C.
[0014] In one embodiment, the linear polymeric polyester diol has a number average molecular weight of 500 to 2000 Daltons and a glass transition temperature of at least 35°C, the polymer comprises from 0.5 to 20 wt % of the residue of at least one supplemental monomeric diol, based on the total weight of the polymer, the polymer has a glass transition temperature of no greater than 200°C and the polymer has a tensile modulus of at least 1000 MPa.
[0015] In one embodiment, the polymer has a glass transition temperature of at least 145°C, the polymer has a tensile modulus of at least 1000 MPa, and the residues of the diisocyanate monomer are present in the polymer in an amount of no greater than 35 wt % based on the total weight of the residues of the polymer.
[0016] In one embodiment, the monomeric diacid comprises the residue of terephthalic acid and the monomeric diol comprises the residue of at least two monomeric diols selected from 2,2,4,4-tetramethyl-1,3-cyclobutanediol, isosorbide, 1,4-cyclohexanedimethanol, ethylene glycol, 2,6-decalin dimethanol, 1,4 benzenedimethanol, and combinations thereof, wherein the residue of at least one of the at least two monomeric diols is present in the polymer in an amount of 1 to 50 mole % and wherein the residue of another of the at least two monomeric diols is present in the polymer in an amount of 50 to 99 mole %, based on The linear polymeric polyester diol comprises 100 mol% of the diol component; the diisocyanate monomer comprises 4,4'-diphenylmethane diisocyanate; and the polymer further comprises up to 20 wt% of the residue of at least one supplementary monomer diol based on the total weight of the polymer, wherein the supplementary monomer diol is selected from 2,2,4,4-tetramethyl-1,3-cyclobutanediol, isosorbide, 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, ethylene glycol, 2,6-decalinedimethanol, tricyclodecane dimethanol, 1,4-benzenedimethanol, neopentyl glycol and combinations thereof.
[0017] In one aspect, the present invention is directed to a method for preparing a thermoplastic polymer comprising: combining at least one polymeric polyester diol, at least one monomeric diisocyanate, and optionally at least one supplemental monomeric diol, optionally in the presence of a catalyst, in a reaction zone, and reacting the combination in the reaction zone to form a thermoplastic polymer; wherein the thermoplastic polymer comprises: (a) residues of at least one linear polymeric polyester diol, wherein the linear polymeric polyester diol comprises residues of: (i) at least one monomeric diacid; and (ii) at least one monomeric diol, wherein the linear polymeric polyester diol has a number average molecular weight of at least 400 Daltons; and (b) residues of at least one diisocyanate monomer, wherein the residues of the diisocyanate monomer are present in the polymer in an amount not greater than 40 weight percent based on the total weight of the polymer; and wherein the polymer has a glass transition temperature of at least 140°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Various embodiments of the present invention are described in detail below with reference to the accompanying drawings, in which: Figure 1 is a graph depicting temperature scans of several inventive and comparative polymers as described in Example 7; and Figure 2 is a graph depicting temperature scans of several other inventive and comparative polymers as described in Example 7. DETAILED DESCRIPTION
[0019] Various embodiments of the present invention relate to isocyanate modified thermoplastic polymer compositions and methods of making and using the same. It has been found that adding small amounts of diisocyanate materials to certain thermoplastic polymer compositions can provide rigid polymers having glass transition temperatures and / or high modulus values that can be melt processed at temperatures significantly below 300° C. These rigid polymers (which are different from conventional thermoplastic polyesters, thermoplastic polyurethanes, and rigid thermoplastic polyurethanes) can be used in conventional applications to provide shaped articles, including but not limited to sheets, films, pipes, preforms, bottles, profiles, and other similar articles, which exhibit properties similar to or better than similar articles formed from conventional thermoplastic materials.
[0020] The term "thermoplastic" as used herein is intended to have its ordinary meaning as understood by those of ordinary skill in the art. Specifically, a thermoplastic polymer is a polymer that softens when exposed to heat and returns to its original state when cooled to room temperature. The term "thermosetting" as used herein is also intended to have its ordinary meaning as understood by those of ordinary skill in the art. More specifically, thermosetting polymers or prepolymers are those that can be irreversibly cured by applying heat, chemicals and / or irradiation energy. As described in further detail below, the polymers of the present invention can be thermoplastic and therefore exclude traditional thermosetting materials. Other details about the specific composition of the polymers of the present invention and the methods for preparing and using them will be discussed further below.
[0021] The thermoplastic polymer of the present invention comprises the residue of at least one polymeric diol and at least one isocyanate. As used herein, the term "residue" refers to any organic structure incorporated into a polymeric material by step-growth, polycondensation or ring-opening reactions involving corresponding monomers. It should also be understood that the residue associated with various polymeric materials, including polymeric diols, can be derived from the parent monomer compound itself or any suitable derivative thereof. For example, a polyester diol comprising the residue of a diacid can be derived from a dicarboxylic acid monomer or its associated acyl halide, ester, half ester, salt, half salt, anhydride, mixed anhydride or mixture thereof. Therefore, unless otherwise indicated, the generic name of the parent compound used herein, such as "diacid" is intended to include the parent compound itself as well as its derivatives.
[0022] The term "glycol" as used herein refers to a compound with two reactive hydroxyl functional groups. The glycol formed by a single molecular unit is called a "monomeric glycol", while the term "polymeric glycol" is used to represent a glycol with two or more molecular units. Polymeric glycols can be formed by, for example, reacting a hydroxyl functional monomer with one or more other types of monomers. According to various embodiments of the present invention, at least about 45, at least about 50, at least about 55, at least about 60, at least about 65, at least about 70, at least about 75 or at least about 80% by weight of the total residue of the thermoplastic polymer can be the residue of one or more polymeric glycols. Additionally or alternatively, not more than about 95, not more than about 92.5 or not more than about 90% by weight of the total residue of the thermoplastic polymer can include the residue of one or more polymeric glycols. Examples of suitable polymeric glycols can include, but are not limited to, polyester glycols, polyether glycols, polycaprolactone glycols, polycarbonate glycols and combinations thereof.
[0023] In some embodiments, the thermoplastic polymer may include residues of one or more polymeric glycols in an amount of 45 to 95 wt %, 45 to 92.5 wt %, about 45 to about 90 wt %, 50 to 95 wt %, 50 to 92.5 wt %, about 50 to about 90 wt %, about 55 to about 95 wt %, about 55 to about 92.5 wt %, about 55 to about 90 wt %, about 60 to about 95 wt %, about 60 to about 92.5 wt %, based on the total weight of the polymer. %, about 60 to about 90 weight %, about 65 to about 95 weight %, about 65 to about 92.5 weight %, about 65 to about 90 weight %, about 70 to about 95 weight %, about 70 to about 92.5 weight %, about 70 to about 90 weight %, about 75 to about 95 weight %, about 75 to about 92.5 weight %, about 75 to about 90 weight %, about 80 to about 95 weight %, about 80 to about 92.5 weight % or about 80 to about 90 weight %.
[0024] In some embodiments, the polymeric diol used to form the thermoplastic polymer of the present invention may include at least one linear polymeric polyester diol. As used herein, the term "linear diol" when used to refer to a polymeric diol refers to a polymeric diol having a theoretical hydroxyl functionality of less than 2.2. In some embodiments, a linear polyester polymeric diol suitable for use in the thermoplastic polymer described herein may have a theoretical hydroxyl functionality of no greater than 2.15, no greater than 2.10, no greater than 2.05, or no greater than 2.01.
[0025] Compared to conventional thermosetting or other cross-linkable polymeric materials, the isocyanate-modified thermoplastic polymeric materials described herein may contain less than about 5, less than about 3, less than about 2, less than about 1, less than about 0.5, or less than about 0.1 weight percent of residues of one or more non-linear polymeric polyester polyfunctional alcohols having a hydroxyl functionality of 2.2 or greater, based on the total weight of the polymer. In addition to the polymeric polyester diols, in some embodiments, the thermoplastic polymer may contain no more than about 10, no more than about 7, no more than about 5, no more than about 3, no more than about 2, no more than about 1, or no more than about 0.5 weight percent of one or more linear polymeric diols other than linear polymeric polyester diols, based on the total weight of the polymer.
[0026] In embodiments, the polymeric polyester diol used to form the isocyanate-modified thermoplastic polymer described herein comprises an acid component, a diol component, and optionally a polyfunctional alcohol component.
[0027] Polyester diol used in the present invention can be prepared from dicarboxylic acid and diol usually, and it reacts with substantially the same proportion and is incorporated into polyester diol as its corresponding residue.Therefore, polyester diol of the present invention can comprise acid residue (100 mol %) and diol (and / or polyfunctional hydroxy compound) residue (100 mol %) in substantially equal molar proportion, so that the total mole number of repeating units is equal to 100 mol %.Therefore, the mole percentage provided in the present invention can be based on the total mole number of acid residue (or the total mole number of acid component), the total mole number of diol residue (or the total mole number of diol component) or the total mole number of repeating units.For example, the polyester containing 30 mol % of isophthalic acid based on total acid residue means that the polyester contains 30 mol % of isophthalic acid residue based on 100 mol % of total acid residue.Therefore, there are 30 mol of isophthalic acid residues per 100 mol of acid residues. In another example, a polyester containing 30 mole % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol based on total diol residues means that the polyester contains 30 mole % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues based on 100 mole % of the total amount of diol residues. Thus, there are 30 moles of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues per 100 moles of diol residues.
[0028] The acid component of the polymerized polyester diol may contain the residues of one or more monomeric diacids. The term "diacid" as used herein refers to a compound containing two reactive carboxyl functional groups and the term "monomeric diacid" refers to a diacid having a single molecular unit. In some embodiments, at least about 95, at least about 97, at least about 99, or at least about 99.5 mol % of the total acid component of the polymerized polyester diol may contain the residues of one or more monomeric diacids. Optionally, in some embodiments, the acid component of the polymerized polyester diol may contain the residues of at least one monomeric multifunctional acid having more than two reactive carboxyl functional groups. However, if used, the residues of the monomeric multifunctional acid are generally present in an amount of less than about 5, less than about 3, less than about 1, or less than about 0.5 mol % based on the total moles of the acid component. In some embodiments, the acid component of the polymerized polyester diol does not contain the residues of the monomeric multifunctional acid.
[0029] In some embodiments, the acid component can include residues of two or more different monomeric diacids. When two or more monomeric diacid residues are present, the diacids can be of the same type (e.g., two different aromatic diacids) or of different types (e.g., an aromatic diacid and an aliphatic diacid), and the residues of each of the different diacids can be present in similar or different amounts based on the total moles of the acid component.
[0030] In embodiments where the acid component comprises at least a first monomeric diacid and a second monomeric diacid, the residue of at least one of the first and second monomeric diacids may be present in an amount of at least about 1, at least about 5, at least about 10, at least about 20, or at least about 25 mole % and / or no more than about 50, no more than about 40, no more than about 35 mole % based on the total moles of the acid component, while the other of the first and second monomeric diacids may be present in an amount of at least about 50, at least about 60, or at least about 65 mole % and / or no more than about 99, no more than about 95, no more than about 90, no more than about 80, or no more than about 75 mole % based on the total moles of the acid component. In other embodiments, the residue of each of the first and second monomeric diacids may be present in an amount of at least about 40 or at least about 45 mole % and / or no more than about 60, no more than about 55, or no more than about 50 mole % based on the total moles of the acid component. In other embodiments, the acid component may comprise residues of at least three or four or more different monomeric diacids.
[0031] In some embodiments, the residue of at least one of the first and second monomeric diacids may be present in an amount of about 1 to about 50, about 1 to about 40 mole %, about 1 to about 35 mole %, about 5 to about 50 mole %, about 5 to about 40 mole %, about 5 to about 35 mole %, about 10 to about 50 mole %, about 10 to about 40 mole %, about 10 to about 35 mole %, about 20 to about 50 mole %, about 20 to about 40 mole %, about 20 to about 35 mole %, about 25 to about 50 mole %, about 25 to about 40 mole %, or about 25 to about 35 mole %, based on the total moles of the acid component. The other of the first and second monomeric diacids can be present in an amount of about 50 to about 99 mol%, about 50 to about 95 mol%, about 50 to about 90 mol%, about 50 to about 80 mol%, about 50 to about 75 mol%, about 60 to about 99 mol%, about 60 to about 95 mol%, about 60 to about 90 mol%, about 60 to about 80 mol%, about 60 to about 75 mol%, about 65 to about 99 mol%, about 65 to about 95 mol%, about 65 to about 90 mol%, about 60 to about 80 mol%, about 60 to about 75 mol%, about 65 to about 99 mol%, about 65 to about 95 mol%, about 65 to about 90 mol%, about 65 to about 80 mol% or about 65 to about 75 mol%, based on the total moles of the acid component.
[0032] In some embodiments, the residue of each of the first and second monomeric diacids is present in the acid component in an amount of about 40 to about 60 mole %, about 40 to about 55 mole %, about 40 to about 50 mole %, about 45 to about 60 mole %, about 45 to about 55 mole %, or about 45 to about 50 mole %, based on the total moles of the acid component.
[0033] Any suitable type of monomeric diacid can be used to form the polymeric polyester diol described herein. Aromatic diacids, aliphatic diacids, acyclic diacids, alicyclic diacids and combinations thereof can be used. Examples of suitable monomeric diacids can include, but are not limited to, terephthalic acid, dimethyl terephthalic acid, 4,4-sulfonyl dibenzoic acid, resorcinol-o,o'diacetic acid, dimethyl succinate, biphenyl 4,4'-dimethyl dicarboxylate, 1,4 cyclohexane dicarboxylic acid, 4,4'-stilbene dicarboxylic acid, 4,4'-isopropylidene diphenoxyacetic acid, isophthalic acid, dimethyl isophthalate, 2,6-dimethyl naphthalene dicarboxylate, decalin-2,6-dicarboxylic acid dimethyl ester, succinic acid, adipic acid, furandicarboxylic acid, dimethyl furandicarboxylate and combinations thereof. In some embodiments, the polymeric polyester diol may include at least one residue of a monomeric diacid selected from the group consisting of terephthalic acid, dimethyl terephthalic acid, 4,4-sulfonyl dibenzoic acid, dimethyl biphenyl 4,4'-dicarboxylate, 1,4 cyclohexane dicarboxylic acid, 4,4'-stilbene dicarboxylic acid, dimethyl isophthalate, dimethyl 2,6-naphthalene dicarboxylate, dimethyl decalin-2,6-dicarboxylate, adipic acid, furandicarboxylic acid, dimethyl furandicarboxylate, and combinations thereof. As noted above, the term "diacid" includes the associated acyl halides, esters, half-esters, salts, half-salts, anhydrides, or mixed anhydrides of the above-listed components.
[0034] Polymerized polyester diols also include a diol component containing the residues of one or more monomeric diols. As described above, the term "diol" refers to a compound with two reactive hydroxyl functional groups, and the term "monomer diol" refers to a diol formed by a single molecular unit. In some embodiments, at least about 95, at least about 97, at least about 99, or at least about 99.5 mol % of the diol component may include the residues of one or more monomeric diols. Optionally, in some embodiments, the diol component of the polymerized polyester diol may include the residues of at least one monomeric multifunctional alcohol having more than two reactive hydroxyl functional groups. However, if used, the residues of the monomeric multifunctional alcohols are typically present in an amount of less than about 5, less than about 3, less than about 1, or less than about 0.5 mol % based on the total moles of the diol component.
[0035] In some embodiments, the diol component of the polymeric polyester diol can include residues of two or more different monomeric diols. When residues of two or more monomeric diols are present, the monomeric diols can be of the same type (e.g., two different aromatic diols) or of different types (e.g., an aromatic diol and an aliphatic diol), and the residues of each of the different monomeric diols can be present in similar or different amounts based on the total moles of the diol component.
[0036] When the diol component comprises residues of at least a first monomeric diol and a second monomeric diol, the residues of at least one of the first and second monomeric diols may be present in an amount of at least about 1, at least about 5, at least about 10, at least about 20, at least about 25 mol % or at least about 30 mol % and / or not more than about 50, not more than about 40, not more than about 35 mol % based on the total moles of the diol component, and the residues of the other of the first and second monomeric diols may be present in an amount of at least about 50, at least about 60, at least about 70 mol % and / or not more than about 99, not more than about 95, not more than about 90, not more than about 80 or not more than about 75 mol % based on the total moles of the diol component. In other embodiments, the residues of each of the first and second monomeric diols may be present in an amount of at least about 40 or at least about 45 mol % and / or not more than about 60, not more than about 55 or not more than about 50 mol % based on the total moles of the diol component. In other embodiments, the diol component may comprise residues of at least three or four or more different monomeric diols.
[0037] In some embodiments, the residue of at least one of the first and second monomeric diols may be present in an amount of about 1 to about 50, about 1 to about 40 mole percent, about 1 to about 35 mole percent, about 5 to about 50 mole percent, about 5 to about 40 mole percent, about 5 to about 35 mole percent, about 10 to about 50 mole percent, about 10 to about 40 mole percent, about 10 to about 35 mole percent, about 20 to about 50 mole percent, about 20 to about 40 mole percent, about 20 to about 35 mole percent, about 25 to about 50 mole percent, about 25 to about 40 mole percent, or about 25 to about 35 mole percent, based on the total moles of the diol component. The other of the first and second monomeric diols can be present in an amount of about 50 to about 99 mole %, about 50 to about 95 mole %, about 50 to about 90 mole %, about 50 to about 80 mole %, about 50 to about 75 mole %, about 60 to about 99 mole %, about 60 to about 95 mole %, about 60 to about 90 mole %, about 60 to about 80 mole %, about 60 to about 75 mole %, about 65 to about 99 mole %, about 65 to about 95 mole %, about 65 to about 90 mole %, about 65 to about 80 mole %, or about 65 to about 75 mole %, based on the total moles of the diol component.
[0038] In some embodiments, the residue of each of the first and second monomeric diols is present in the diol component in an amount of about 40 to about 60 mole %, about 40 to about 55 mole %, about 40 to about 50 mole %, about 45 to about 60 mole %, about 45 to about 55 mole %, or about 45 to about 50 mole %, based on the total moles of the diol component.
[0039] Any suitable type of monomeric diol can be used to form the polymerized polyester diol described herein. Aromatic diols, aliphatic diols, acyclic diols, alicyclic diols and combinations thereof can be used. Examples of suitable monomeric diols may include, but are not limited to, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, isosorbide, 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, ethylene glycol, 2,2'((sulfonylbis(4,1-phenylene))bis(oxy)diethanol, 2,6-decalin dimethanol, tricyclodecane dimethanol, 1,4 benzenedimethanol, 2,2'-(1,4-phenylenebis(oxy))diethanol, 2,2'-(2,4,8,10-tetraoxaspiro(5,5)undecane-3,9-diyl)bis(2-methylpropane-1-ol), neopentyl glycol and combinations thereof. In some embodiments, the polymerized polyester diol may include at least one residue selected from the following diols: 2,2,4,4-tetramethyl-1,3-cyclobutanediol, isosorbide, 1,4-cyclohexanedimethanol, ethylene glycol, 2,6-decalin dimethanol, 1,4 benzenedimethanol, and combinations thereof. In one embodiment, the monomeric diols used to form the polymeric polyester diols described herein include 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 1,4-cyclohexanedimethanol.
[0040] In an embodiment, the polymeric polyester diol comprises 2,2,4,4-tetramethyl-1,3-cyclobutanediol in an amount of 50 to 80 mole % and 1,4-cyclohexanedimethanol in an amount of 20 to 50 mole %; or 2,2,4,4-tetramethyl-1,3-cyclobutanediol in an amount of 60 to 80 mole % and 1,4-cyclohexanedimethanol in an amount of 20 to 40 mole %; or 2,2,4,4-tetramethyl-1,3-cyclobutanediol in an amount of 65 to 75 mole % and 1,4-cyclohexanedimethanol in an amount of 25 to 35 mole %; or 2,2,4,4-tetramethyl-1,3-cyclobutanediol in an amount of about 70 mole % and 1,4-cyclohexanedimethanol in an amount of about 1 mole %; all based on the total moles of the diol components. In some embodiments, 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 1,4-cyclohexanedimethanol and less than 5, or less than 4, or less than 3, or less than 2, or less than 1 mole % of any other monomeric diols based on the total moles of the diol component. In one embodiment, no other monomeric diols are intentionally added to the polymerized polyester diol. In one embodiment, when the diol component is based on 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 1,4-cyclohexanedimethanol, the diacid component comprises at least 95 mole % or 100 mole % of terephthalic acid or its derivatives based on the total moles of the diacid component.
[0041] The polymeric polyester diol used to form the thermoplastic polymer of the present invention can have a molecular weight of at least 400 Daltons. The terms "molecular weight" and "number average molecular weight" used herein refer to the number average molecular weight measured by gel permeation chromatography (GPC) in an Agilent 1100 series GPC-SEC system with a refractive index detector calibrated to a polystyrene standard using HFIP / methylene chloride as a solvent according to ASTM method D-5296. In some embodiments, the number average molecular weight of the polymeric polyester diol can be at least about 450, at least about 500 Daltons, or at least about 600 Daltons and / or not more than about 5000, not more than about 4000, not more than about 3000, not more than about 2500, not more than about 2000, not more than about 1800 Daltons, or not more than about 1200 Daltons.
[0042] The polymeric polyester diols may have a molecular weight of about 400 to about 5000 Daltons, about 400 to about 4000 Daltons, about 400 to about 3000 Daltons, about 400 to about 2500 Daltons, about 400 to about 2000 Daltons, about 400 to about 1800 Daltons, about 400 to about 1200 Daltons, about 450 to about 5000 Daltons, about 450 to about 4000 Daltons, about 450 to about 3000 Daltons, about 450 to about 2500 Daltons, about 450 to about 2000 Daltons, about 450 to about 1800 Daltons, about 450 to about 1200 Daltons. In some embodiments, the present invention relates to a molecular weight of about 500 to about 5000 daltons, about 500 to about 4000 daltons, about 500 to about 3000 daltons, about 500 to about 2500 daltons, about 500 to about 2000 daltons, about 500 to about 1800 daltons, about 500 to about 1200 daltons, about 600 to about 5000 daltons, about 600 to about 4000 daltons, about 600 to about 3000 daltons, about 600 to about 2500 daltons, about 600 to about 2000 daltons, about 600 to about 1800 daltons or about 600 to about 1200 daltons.
[0043] In some embodiments, polymeric polyester diols having molecular weights within one or more of the above ranges may also have a glass transition temperature greater than about -5°C as measured using a Q2000 differential scanning calorimeter (DSC) available from TA Instruments according to ASTM method D-3418 at a scan rate of 20°C / min. The polymeric polyester diol can have a glass transition temperature of at least about 0, at least about 5, at least about 10, at least about 15, at least about 20, at least about 25, at least about 30, at least about 35, at least about 40, at least about 45, at least about 50, at least about 55° C. and / or no greater than about 150, no greater than about 145, no greater than about 140, no greater than about 135, no greater than about 130, no greater than about 125, no greater than about 120, no greater than about 115, no greater than about 110, no greater than about 105, no greater than about 100, no greater than about 95, no greater than about 90, no greater than about 85, no greater than about 80, no greater than about 75, no greater than about 70, no greater than about 65, no greater than about 60, or no greater than about 55, no greater than about 50, no greater than about 45, no greater than about 40, no greater than about 35, no greater than about 30, or no greater than about 25° C.
[0044] The glass transition temperature of the polymeric polyester diol can be from about -5 to about 150°C, from about -5 to about 145°C, from about -5 to about 140°C, from about -5 to about 135°C, from about -5 to about 130°C, from about -5 to about 125°C, from about -5 to about 120°C, from about -5 to about 115°C, from about -5 to about 110°C, from about -5 to about 105°C, from about -5 to about 100°C, from about -5 to about 95°C, from about -5 to about 90°C, from about -5 to about 85°C, from about -5 to about 80°C, from about -5 to about 75°C, from about -5 to about 70°C, from about -5 to about 65°C, from about -5 to about 60°C, from about -5 to about 55°C, more preferably from about -5 to about 95°C, from about -5 to about 90°C, from about -5 to about 85°C, from about -5 to about 80°C, about -5 to about 50°C, about -5 to about 45°C, about -5 to about 40°C, about -5 to about 35°C, about -5 to about 30°C, about -5 to about 25°C, about 0 to about 150°C, about 0 to about 145°C, about 0 to about 140°C, about 0 to about 135°C, about 0 to about 130°C, about 0 to about 125°C, about 0 to about 120°C, about 0 to about 115°C, about 0 to about 110°C, about 0 to about 105°C, about 0 to about 100°C, about 0 to about 95°C, about 0 to about 90°C, about 0 to about 85°C, about 0 to about 80°C, about 0 to about 75°C, about 0 to about 70°C, about 0 to about 65°C, about 0 to about 60°C, about 0 to about 55°C, about 0 to about 50°C, about 0 to about 45°C, about 0 to about 40°C, about 0 to about 35°C, about 0 to about 30°C, about 0 to about 25°C, about 5 to about 150°C, about 5 to about 145°C, about 5 to about 140°C, about 5 to about 135°C, about 5 to about 130°C, about 5 to about 125°C, about 5 to about 120°C, about 5 to about 115°C, about 5 to about 110°C, about 5 to about 105°C, about 5 to about 100°C, about 5 to about 95°C, about 5 to about 90°C, about 5 to about 85°C, about 5 to about 80°C, about 5 to about 75°C, about 5 to about 70°C, about 5 to about 65°C, about 5 to about 60°C, about 5 to about 55°C, about 5 to about 50°C, about 5 to about 45°C, about 5 to about 40°C, about 5 to about 35°C, about 5 to about 30°C, about 5 to about 25°C, about 10 to about 150°C, about 10 to about 145°C, about 10 to about 140°C, about 10 to about 135°C, about 10 to about 130°C, about 10 to about 125°C, about 10 to about 120°C, about 10 to about 115°C, about 10 to about 110°C, about 10 to about 105°C, about 10 to about 100°C, about 10 to about 95°C,about 10 to about 90°C, about 10 to about 85°C, about 10 to about 80°C, about 10 to about 75°C, about 10 to about 70°C, about 10 to about 65°C, about 10 to about 60°C, about 10 to about 55°C, about 10 to about 50°C, about 10 to about 45°C, about 10 to about 40°C, about 10 to about 35°C, about 10 to about 30°C, about 10 to about 25°C, about 15 to about 150°C, about 15 to about 145°C, about 15 to about 140°C, about 15 to about 135°C, about 15 to about 130°C, about 15 to about 125°C, about 15 to about 120°C, about 15 to about 115°C, about 15 to about 110°C, about 15 to about 105°C, about 15 to about 100°C, about 15 to about 95°C, about 15 to about 90°C, about 15 to about 85°C, about 15 to about 80°C, about 15 to about 75°C, about 15 to about 70°C, about 15 to about 65°C, about 15 to about 60°C, about 15 to about 55°C, about 15 to about 50°C, about 15 to about 45°C, about 15 to about 40°C, about 15 to about 35°C, about 15 to about 30°C, about 15 to about 25°C, about 20 to about 150°C, about 20 to about 145°C, about 20 to about 140°C, about 20 to about 135°C, more about 20 to about 130°C, about 20 to about 125°C, about 20 to about 120°C, about 20 to about 115°C, about 20 to about 110°C, about 20 to about 105°C, about 20 to about 100°C, about 20 to about 95°C, about 20 to about 90°C, about 20 to about 85°C, about 20 to about 80°C, about 20 to about 75°C, about 20 to about 70°C, about 20 to about 65°C, about 20 to about 60°C, about 20 to about 55°C, about 20 to about 50°C, about 20 to about 45°C, about 20 to about 40°C, about 20 to about 35°C, about 20 to about 30°C, about 20 to about 25°C, about 25 to about 150°C, about 25 to about 145°C, about 25 to about 140°C, about 25 to about 135°C, about 25 to about 130°C, about 25 to about 125°C, about 25 to about 120°C, about 25 to about 115°C, about 25 to about 110°C, about 25 to about 105°C, about 25 to about 100°C, about 25 to about 95°C, about 25 to about 90°C, about 25 to about 85°C, about 25 to about 80°C, about 25 to about 75°C, about 25 to about 70°C, about 25 to about 65°C, about 25 to about 60°C, about 25 to about 55°C, about 25 to about 50°C, about 25 to about 45°C,about 25 to about 40°C, about 25 to about 35°C, about 25 to about 30°C, about 30 to about 150°C, about 30 to about 145°C, about 30 to about 140°C, about 30 to about 135°C, about 30 to about 130°C, about 30 to about 125°C, about 30 to about 120°C, about 30 to about 115°C, about 30 to about 110°C, about 30 to about 105°C, about 30 to about 100°C, about 30 to about 95°C, about 30 to about 90°C, about 30 to about 85°C, about 30 to about 80°C, about 30 to about 75°C, about 30 to about 70°C, about 30 to about 65°C, about 30 to about 65°C, about 30 to about 0°C, about 30 to about 55°C, about 30 to about 50°C, about 30 to about 45°C, about 30 to about 40°C, about 30 to about 35°C, about 35 to about 150°C, about 35 to about 145°C, about 35 to about 140°C, about 35 to about 135°C, about 35 to about 130°C, about 35 to about 125°C, about 35 to about 120°C, about 35 to about 115°C, about 35 to about 110°C, about 35 to about 105°C, about 35 to about 100°C, about 35 to about 95°C, about 35 to about 90°C, about 35 to about 85°C, about 35 to about 80°C, about 35 to about 75°C, about 35 to about about 70°C, about 35 to about 65°C, about 35 to about 60°C, about 35 to about 55°C, about 35 to about 50°C, about 35 to about 45°C, about 35 to about 40°C, about 40 to about 150°C, about 40 to about 145°C, about 40 to about 140°C, about 40 to about 135°C, about 40 to about 130°C, about 40 to about 125°C, about 40 to about 120°C, about 40 to about 115°C, about 40 to about 110°C, about 40 to about 105°C, about 40 to about 100°C, about 40 to about 95°C, about 40 to about 90°C, about 40 to about 85°C, about 40 to about 80°C, about 40 to about 75°C, about 40 to about 70°C, about 40 to about 65°C, about 40 to about 60°C, about 40 to about 55°C, about 40 to about 50°C, about 40 to about 45°C, about 45 to about 150°C, about 45 to about 145°C, about 45 to about 140°C, about 45 to about 135°C, about 45 to about 130°C, about 45 to about 125°C, about 45 to about 120°C, about 45 to about 115°C, about 45 to about 110°C, about 45 to about 105°C, about 45 to about 100°C, about 45 to about 95°C, about 45 to about 90°C, about 45 to about 85°C, about 45 to about 80°C,about 45 to about 75°C, about 45 to about 70°C, about 45 to about 65°C, about 45 to about 60°C, about 45 to about 55°C, about 45 to about 50°C, about 50 to about 150°C, about 50 to about 145°C, about 50 to about 140°C, about 50 to about 135°C, about 50 to about 130°C, about 50 to about 125°C, about 50 to about 120°C, about 50 to about 115°C, about 50 to about 110°C, about 50 to about 105°C, about 50 to about 100°C, about 50 to about 95°C, about 50 to about 90°C, about 50 to about 85°C, about 50 to about 80°C, about 50 to about 75°C, about 50 to about about 70°C, about 50 to about 65°C, about 50 to about 60°C, about 50 to about 55°C, about 55 to about 150°C, about 55 to about 145°C, about 55 to about 140°C, about 55 to about 135°C, about 55 to about 130°C, about 55 to about 125°C, about 55 to about 120°C, about 55 to about 115°C, about 55 to about 110°C, about 55 to about 105°C, about 55 to about 100°C, about 55 to about 95°C, about 55 to about 90°C, about 55 to about 85°C, about 55 to about 80°C, about 55 to about 75°C, about 55 to about 70°C, about 55 to about 65°C, or about 55 to about 60°C.
[0045] In some embodiments, the thermoplastic polymer described herein may include residues of two or more different polymerized polyester diols. For example, in some embodiments, the thermoplastic polymer may include at least the first polymerized polyester diol and the second polymerized polyester diol. It is preferred that the first and second polymerized polyester diols are not transesterified with each other so that the thermoplastic polymer includes at least 0.5% by weight of the residues of the first and second polymerized polyester diols. In some embodiments, the weight ratio of the first and second polyester diols may be 90:10 to 10:90, 80:20 to 20:80, 70:30 to 30:70 or 60:40 to 40:60. In some embodiments, the residues of the first and second polymerized polyester diols may be present in the thermoplastic polymer in an amount of at least about 1, at least about 5, at least about 10, at least about 15, at least about 20, at least about 25, at least about 35, at least about 40 or at least about 45% by weight based on the gross weight of the thermoplastic polymer and / or not more than about 50, not more than about 40, not more than about 35% by weight based on the gross weight of the thermoplastic polymer. The residues of each of the first and second polymerized polyester diols may be present in the thermoplastic polymer in similar amounts or the residues of one of the polymerized polyester diols may be present in a greater amount than the residues of the other.
[0046] When the thermoplastic polymer comprises residues of at least a first and a second polymerized polyester diol, in some embodiments, the residues of each of the first and second polymerized polyester diols can be present in the thermoplastic polymer in an amount of about 1 to about 50, about 1 to about 40 weight percent, about 1 to about 35 weight percent, about 5 to about 50 weight percent, greater than 5 to about 40 weight percent, greater than 5 to about 35 weight percent, greater than 10 to about 50 weight percent, about 10 to about 40 weight percent, about 10 to about 35 weight percent, about 15 to about 50 weight percent, about 15 to about 40 weight percent, about 15 to about 35 weight percent, about 20 to about 50 weight percent, about 20 to about 40 weight percent, about 20 to about 35 weight percent, about 25 to about 50 weight percent, about 25 to about 40 weight percent, about 25 to about 35 weight percent, or about 30 to 35 weight percent.
[0047] The polymerized polyester diol used to form the thermoplastic polymer material described herein can be formed according to any suitable method. For example, in some embodiments, the diacid and diol starting materials can be combined and heated under conditions sufficient to form the desired polymerized polyester diol. Byproducts such as water (if acid is used as a starting material) or alcohol (if ester is used as a starting material) can be collected and removed from the reaction zone to promote the synthesis of the polymerized polyester diol. The reaction temperature can be from about 150 to about 250°C, and the reaction pressure can be atmospheric pressure or below atmospheric pressure. The reaction can be carried out for a time sufficient to reach the glass transition temperature and molecular weight within one or more of the above ranges of the polymerized polyester diol. The initial molar ratio of the diacid starting material to the diol starting material can be about 1:1, the diol may be slightly excessive and if necessary, the reaction can be carried out in the presence of a catalyst, such as a tin-based catalyst and an optional organic solvent. In some embodiments, the amount of the catalyst may be present in an amount of 0.1 to 1% by weight based on the total weight of the reaction mixture. Any suitable method for recovering the resulting polymerized polyester diol from the reaction mixture can be used.
[0048] As mentioned above, the thermoplastic polymer of the present invention can also include the residue of at least one isocyanate. The term "isocyanate" used herein refers to a compound comprising at least one reactive isocyanate group. Compared with other polymerization systems using one or more isocyanate components as crosslinking agents, the thermoplastic polymer described herein includes the residue of at least one isocyanate in its polymer backbone. According to an embodiment of the present invention, the total amount of isocyanate residues present in the thermoplastic polymer can be no more than about 40, no more than about 35, no more than about 30, no more than about 25 or no more than about 20 weight % based on the total weight of the polymer. In addition, in an embodiment, the total amount of isocyanate residues present in the thermoplastic polymer can be at least about 5, at least about 7.5, at least about 10 or at least about 12 based on the total weight of the polymer.
[0049] In some embodiments, the total amount of isocyanate residues in the thermoplastic polymer can be from about 5 to about 40 weight percent, from about 5 to about 35 weight percent, from about 5 to about 30 weight percent, from about 5 to about 25 weight percent, from about 5 to about 20 weight percent, from about 7.5 to about 40 weight percent, from about 7.5 to about 35 weight percent, from about 7.5 to about 30 weight percent, from about 7.5 to about 25 weight percent, from about 7.5 to about 20 weight percent, from about 10 to about 40 weight percent, from about 10 to about 35 weight percent, from about 10 to about 30 weight percent, from about 10 to about 25 weight percent, from about 10 to about 20 weight percent, from about 12 to about 40 weight percent, from about 12 to about 35 weight percent, from about 12 to about 30 weight percent, from about 12 to about 25 weight percent, or from about 12 to about 20 weight percent, based on the total weight of the polymer. In some embodiments, the total amount of isocyanate residues can be from about 20 to about 40 weight percent, from about 20 to about 35 weight percent, from about 20 to about 30 weight percent, from about 25 to about 40 weight percent, from about 25 to about 35 weight percent, from about 25 to about 30 weight percent, from about 27 to about 40 weight percent, from about 27 to about 35, or from about 27 to about 30 weight percent based on the total weight of the polymer.
[0050] Suitable isocyanates can include diisocyanates, polyisocyanates, or combinations thereof. As used herein, the term "diisocyanate" refers to a compound containing two reactive isocyanate groups, while the terms "polyisocyanate" and "polyfunctional isocyanate" refer to isocyanates having three or more reactive isocyanate groups. When present, the total amount of polyisocyanate residues can be less than about 5, less than about 3, less than about 1, or less than about 0.5 weight percent based on the total weight of the isocyanate residues.
[0051] Any suitable monomeric diisocyanate may be used to form the thermoplastic polymeric materials described herein. The monomeric diisocyanate may include aromatic diisocyanates, aliphatic diisocyanates, and combinations thereof.
[0052] For example, in some embodiments, the thermoplastic polymer can contain at least about 50, at least about 55, at least about 60, at least about 65, at least about 70, at least about 75, at least about 80, at least about 85, at least about 90, at least about 95, or at least about 97 weight percent of residues of one or more aromatic diisocyanate monomers, based on the total weight of the isocyanate residues. In some cases, the thermoplastic polymers described herein may include residues of at least one aliphatic isocyanate monomer, and when present, the monomeric aliphatic isocyanate residues may be present in an amount of at least about 5, at least about 10, at least about 15, at least about 20 weight percent and / or not greater than about 70, not greater than about 60, not greater than about 50 weight percent, based on the total amount of isocyanate residues or the total amount of monomeric aliphatic isocyanate residues may be from about 5 to about 70 weight percent, from about 5 to about 60 weight percent, from about 5 to about 50 weight percent, from about 10 to about 70, from about 10 to about 60 weight percent, from about 10 to about 50 weight percent, from about 15 to about 70 weight percent, from about 15 to about 60 weight percent, from about 15 to about 50 weight percent, from about 20 to about 70 weight percent, from about 20 to about 60 weight percent or from about 20 to about 50 weight percent, based on the total amount of isocyanate residues. In some embodiments, the ratio of the total amount of aromatic isocyanate residues to the total amount of aliphatic isocyanate residues present in the thermoplastic polymer may be greater than 1.5:1, greater than 2:1, greater than 2.5:1, or greater than 3:1 on a molar basis.
[0053] Examples of suitable isocyanates may include, but are not limited to, hexamethylene diisocyanate, isophorone diisocyanate, methylene dicyclohexyl diisocyanate, ethylene diisocyanate, 1,4-tetramethylene diisocyanate, 1,6-hexamethylene diisocyanate, 1,12-dodecane diisocyanate, cyclobutane-1,3-diisocyanate, cyclohexane-1,3-diisocyanate, cyclohexane-1,4-diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, ditolyl diisocyanate, m-tetramethylbenzene diisocyanate, Meta-tetramethylxylylenediisocyanate, hydrogenated diisocyanato ditoluene, 1,5-naphthalene diisocyanate, p-phenylene diisocyanate, 3,3'-dimethyldiphenyl-4,4'-diisocyanate, 1,6-hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, norbornane diisocyanate, 4,4'-dibenzyl diisocyanate and combinations thereof. In some embodiments, the isocyanate may be selected from 2,2'-diphenylmethane diisocyanate and 4,4'-diphenylmethane diisocyanate, while in other embodiments, the isocyanate may be 4,4'-diphenylmethane diisocyanate.
[0054] In addition to the residues of at least one polymerized polyester diol and at least one isocyanate, the thermoplastic polymers described herein may contain residues of one or more additional components in various amounts. Such additional components may include, but are not limited to, at least one supplementary monomeric diol, at least one branching monomer, or a combination thereof. The term "supplementary monomeric diol" as used herein refers to a diol that is different from (or in addition to) the diol present in the polymerized polyester diol used to form the thermoplastic polymer of the present invention. For clarity, in embodiments, the supplementary monomeric diol may be of the same type (i.e., the same chemical substance or compound) as the monomeric diol used to prepare the polymerized polyester diol. In other embodiments, the supplementary monomeric diol may be of a different type (i.e., a different chemical substance or compound) than any monomeric diol used to prepare the polymerized polyester diol. Supplementary means that the monomeric diol is present in the thermoplastic polymer in addition to the polymerized polyester diol. In some embodiments, the thermoplastic polymers described herein may include at least about 0.5, at least about 1, at least about 2, at least about 3, at least about 5, at least about 8, or at least about 10 weight percent and / or no more than about 20, no more than about 18, no more than about 15, or no more than about 12 weight percent of at least one supplemental monomeric diol, based on the total weight of the thermoplastic polymer. In other embodiments, substantially no or no supplemental monomeric diol may be used, such that the total amount of residues of the supplemental diol present in the thermoplastic polymer may be less than 0.5 or less than about 0.1, based on the total weight of the thermoplastic polymer.
[0055] In some embodiments, the thermoplastic polymers described herein may include the residue of at least one supplemental diol in an amount of about 0.5 to about 20 weight percent, about 0.5 to about 18 weight percent, about 0.5 to about 15 weight percent, about 0.5 to about 12 weight percent, about 1 to about 20 weight percent, about 1 to about 18 weight percent, about 1 to about 15 weight percent, about 1 to about 12 weight percent, about 2 to about 20 weight percent, about 2 to about 18 weight percent, about 2 to about 15 weight percent, about 2 to about 12 weight percent, based on the total weight of the polymerized polyester diol. wt %, about 3 to about 20 wt %, about 3 to about 18 wt %, about 3 to about 15 wt %, about 3 to about 12 wt %, about 5 to about 20 wt %, about 5 to about 18 wt %, about 5 to about 15 wt %, about 5 to about 12 wt %, about 8 to about 20 wt %, about 8 to about 18 wt %, about 8 to about 15 wt %, about 8 to about 12 wt %, about 10 to about 20 wt %, about 10 to about 18 wt %, about 10 to about 15 wt % or about 10 to about 12 wt %.
[0056] When used, the supplemental diol may include any suitable monomeric diol. Suitable monomeric diols may be the same or different from the one or more diols used to form the polymeric polyester diol as described above. Examples of monomeric diols suitable for use as supplemental diols in thermoplastic polymers may include, but are not limited to, 2,2'-bis[4-(2-hydroxyethoxy)phenyl]propane, 1,4-butanediol, tricyclodecane dimethanol, 2,2'-(1,4-phenylenebis(oxy))diethanol, 1,4-benzenedimethanol, 2,2-dimethyl-1,3-propanediol, 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 4,8-bis(hydroxymethyl)tricyclo[5.2.1 .02,6] decane, bis-4-(2-hydroxyethoxy)phenyl sulfone), spirodiol, 2,2'-(1,4-phenylenebis(oxy))diethanol, 2,2'-(2,4,8,10-tetraoxaspiro(5,5)undecane-3,9-diyl)bis(2-methylpropan-1-ol), 2,6-decalin, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 1,4-cyclohexanediol, isosorbide, hydroquinone, neopentyl glycol, and combinations thereof. In some embodiments, the supplemental monomer diol may be selected from 1,4-cyclohexanedimethanol, 1,4-cyclohexanediol, 2,6-decalin, and combinations thereof. In one embodiment, the supplemental monomer diol is 1,4-cyclohexanedimethanol.
[0057] According to some embodiments, thermoplastic polymers described herein may include the residue of at least one branched monomer.Term used herein " branched monomer " refers to the monomer component comprising three or more reactive functional groups, and the functional group is selected from carboxyl substituent, hydroxyl substituent and combination thereof.The example of suitable branched monomer may include but is not limited to trimellitic acid, trimellitic anhydride, pyromellitic dianhydride, trimethylolpropane, glycerine, pentaerythritol, citric acid, tartaric acid, 3-hydroxyglutaric acid etc.In some embodiments, branched monomer may be selected from trimethylolpropane, glycerine, pentaerythritol and combination thereof.Branched monomer may be added to reaction mixture or blended with thermoplastic polymer in the form of concentrate as described in, for example, U.S. Patent Nos. 5,654,347 and 5,696,176.
[0058] If present, the total amount of polymerized polyester polyfunctional alcohol having a hydroxyl functionality of 2.2 or greater, branching monomers, and polyfunctional isocyanates may be present in the thermoplastic polymer in an amount of less than 2 weight percent based on the total weight of the polymer. In some embodiments, the thermoplastic polymer of the present invention may contain no more than about 1.5, no more than about 1, no more than about 0.70, no more than about 0.50, or no more than about 0.25 weight percent of branching monomers, polyfunctional isocyanates, and polymerized polyester polyfunctional alcohol having a hydroxyl functionality of 2.2 or greater, based on the total weight of the polymer.
[0059] As described above, the thermoplastic polymers of the present invention may comprise at least one polymeric polyester diol and at least one monomeric isocyanate, optionally with residues of one or more supplementary diols, branching monomers, and / or multifunctional isocyanates as described above. According to some embodiments of the present invention, the thermoplastic polymer may exclude or substantially exclude other components in addition to those described above, such that, for example, less than about 20, less than about 15, less than about 10, less than about 5, less than about 3, less than about 1, or less than about 0.5 weight percent of the total residues of the thermoplastic polymers of the present invention may comprise residues of components other than the polymeric polyester diols, monomeric isocyanates, and, if present, supplementary diols, branching monomers, and multifunctional isocyanates described herein. In some embodiments, the thermoplastic polymers as described herein may consist essentially of or consist of the polymeric polyester diols, monomeric isocyanates, and, if present, supplementary diols, branching monomers, and multifunctional isocyanates.
[0060] Unlike conventional thermosetting polymer resins, the thermoplastic polymers described herein may not be cross-linked. Thus, the thermoplastic polymers of the present invention may be substantially free of or free of residues of cross-linking agents. For example, the thermoplastic polymers described herein may contain less than about 10, less than about 8, less than about 5, less than about 3, less than about 1, or less than about 0.5 weight percent of one or more cross-linking agents based on the total weight of the polymer.
[0061] In certain embodiments, the thermoplastic polymers as described herein can have an isocyanate to polyol ratio, measured as a molar ratio of isocyanate to hydroxyl functional groups (NCO:OH), of at least about 1:1, at least about 1.01:1, at least about 1.025:1, at least about 1.05:1 and / or no greater than about 1.25:1, no greater than about 1.2:1, no greater than about 1.15:1, or no greater than about 1.1:1 or from about 1:1 to about 1.25:1, from about 1:1 to about 1.2:1, from about 1:1 to about 1.15:1, or from about 1:1 to about 1.1:1 , about 1.01:1 to about 1.25:1, about 1.01:1 to about 1.2:1, about 1.01:1 to about 1.15:1, about 1.01:1 to about 1.1:1, about 1.025:1 to about 1.25:1, about 1.025:1 to about 1.2:1, about 1.025:1 to about 1.15:1, about 1.025:1 to about 1.1:1, about 1.05:1 to about 1.25:1, about 1.05:1 to about 1.2:1, about 1.05:1 to about 1.15:1, about 1.05:1 to about 1.1:1.
[0062] According to embodiments of the present invention, the thermoplastic polymers described herein may have a glass transition temperature of at least about 70° C., measured using a Q2000 differential scanning calorimeter (DSC) available from TA Instruments according to ASTM method D-3418 at a scan rate of 20° C. / min. This is in contrast to many conventional thermoplastic polyurethane compositions, which typically have a glass transition temperature at or below room temperature. In some embodiments, the thermoplastic polymers of the present invention can have a glass transition temperature of at least about 25, at least about 50, at least about 75, at least about 80, at least about 85, at least about 90, at least about 95, at least about 100, at least about 105, at least about 110, at least about 115, at least about 120, at least about 125, at least about 130, at least about 135, at least about 140, at least about 145, at least about 150, at least about 155, or at least about 160° C. and / or no greater than about 200, no greater than about 195, no greater than about 190, no greater than about 185, no greater than about 180, no greater than about 170, no greater than about 165, no greater than about 160, no greater than about 155, no greater than about 150, or no greater than about 145° C.
[0063] The thermoplastic polymer may have a temperature of about 25 to about 200°C, about 25 to about 195°C, about 25 to about 190°C, about 25 to about 185°C, about 25 to about 180°C, about 25 to about 175°C, about 25 to about 170°C, about 25 to about 165°C, about 25 to about 160°C, about 25 to about 155°C, about 25 to about 150°C, about 25 to about 145°C, about 50 to about 200°C, about 50 to about 195°C, about 50 to about 190°C, about 50 to about 185°C, about 50 to about 180°C, about 50 to about 175°C, about 50 to about 170°C, about 50 to about 165°C ℃, about 50 to about 160 ℃, about 50 to about 155 ℃, about 50 to about 150 ℃, about 50 to about 145 ℃, about 70 to about 200 ℃, about 70 to about 195 ℃, about 70 to about 190 ℃, about 70 to about 185 ℃, about 70 to about 180 ℃, about 70 to about 175 ℃, about 70 to about 170 ℃, about 70 to about 165 ℃, about 70 to about 160 ℃, about 70 to about 155 ℃, about 70 to about 150 ℃, about 70 to about 145 ℃, about 75 to about 200 ℃, about 75 to about 195 ℃, about 75 to about 190 ℃, about 75 to about 185 ℃, about 75 to about 180°C, about 75 to about 175°C, about 75 to about 175°C, about 75 to about 165°C, about 75 to about 160°C, about 75 to about 155°C, about 75 to about 150°C, about 75 to about 145°C, about 80 to about 200°C, about 80 to about 195°C, about 80 to about 190°C, about 80 to about 185°C, about 80 to about 180°C, about 80 to about 175°C, about 80 to about 180°C, about 80 to about 165°C, about 80 to about 160°C, about 80 to about 155°C, about 80 to about 150°C, about 80 to about 145°C, about 85 to about 200°C, about 80 to about 195°C, about 80 to about 190°C, about 80 to about 185°C 5 to about 195°C, about 85 to about 190°C, about 85 to about 185°C, about 85 to about 180°C, about 85 to about 175°C, about 85 to about 185°C, about 85 to about 165°C, about 85 to about 160°C, about 85 to about 155°C, about 85 to about 150°C, about 85 to about 145°C, about 90 to about 200°C, about 90 to about 195°C, about 90 to about 190°C, about 90 to about 185°C, about 90 to about 180°C, about 90 to about 175°C, about 90 to about 190°C, about 90 to about 165°C, about 90 to about 160°C, about 90 to about 155°C,about 90 to about 150°C, about 90 to about 145°C, about 95 to about 200°C, about 95 to about 195°C, about 95 to about 190°C, about 95 to about 185°C, about 95 to about 180°C, about 95 to about 175°C, about 95 to about 195°C, about 95 to about 165°C, about 95 to about 160°C, about 95 to about 155°C, about 95 to about 150°C, about 95 to about 145°C, about 100 to about 200°C, about 100 to about 195°C, about 100 to about 190°C, about 100 to about 185°C, about 100 to about 180°C, about 100 to about 175°C, about 100 to about 1100°C, about 100 to about 165°C, about 100 to about 160°C, about 100 to about 155°C, about 100 to about 150°C, about 100 to about 145°C, about 105 to about 200°C, about 105 to about 195°C, about 105 to about 190°C, about 105 to about 185°C, about 105 to about 180°C, about 105 to about 175°C, about 105 to about 1105°C, about 105 to about 165°C, about 105 to about 160°C, about 105 to about 155°C, about 105 to about 150°C, about 105 to about 145°C, about 110 to about 200°C, more about 110 to about 195°C, about 110 to about 190°C, about 110 to about 185°C, about 110 to about 180°C, about 110 to about 175°C, about 110 to about 1110°C, about 110 to about 165°C, about 110 to about 160°C, about 110 to about 155°C, about 110 to about 150°C, about 110 to about 145°C, about 115 to about 200°C, about 115 to about 195°C, about 115 to about 190°C, about 115 to about 185°C, about 115 to about 180°C, about 115 to about 175°C, about 115 to about 1115°C, about 115 to about 165°C, about 115 to about 160°C, about 115 to about 155°C, about 115 to about 150°C, about 115 to about 145°C, about 120 to about 200°C, about 120 to about 195°C, about 120 to about 190°C, about 120 to about 185°C, about 120 to about 180°C, about 120 to about 175°C, about 120 to about 1120°C, about 120 to about 165°C, about 120 to about 160°C, about 120 to about 155°C, about 120 to about 150°C, about 120 to about 145°C, about 125 to about 200°C, about 125 to about 195°C, about 125 to about 190°C,about 125 to about 185°C, about 125 to about 180°C, about 125 to about 175°C, about 125 to about 1125°C, about 125 to about 165°C, about 125 to about 160°C, about 125 to about 155°C, about 125 to about 150°C, about 125 to about 145°C, about 130 to about 200°C, about 130 to about 195°C, about 130 to about 190°C, about 130 to about 185°C, about 130 to about 180°C, about 130 to about 175°C, about 130 to about 1130°C, about 130 to about 165°C, about 130 to about 160°C, about 130 to about 155°C , about 130 to about 150°C, about 130 to about 145°C, about 135 to about 200°C, about 135 to about 195°C, about 135 to about 190°C, about 135 to about 185°C, about 135 to about 180°C, about 135 to about 175°C, about 135 to about 1135°C, about 135 to about 165°C, about 135 to about 160°C, about 135 to about 155°C, about 135 to about 150°C, about 135 to about 145°C, about 140 to about 200°C, about 140 to about 195°C, about 140 to about 190°C, about 140 to about 185°C, about 140 to about 180°C, about 140 to about 175°C, about 140 to about 1140°C, about 140 to about 165°C, about 140 to about 160°C, about 140 to about 155°C, about 140 to about 150°C, about 140 to about 145°C, about 145 to about 200°C, about 145 to about 195°C, about 145 to about 190°C, about 145 to about 185°C, about 145 to about 180°C, about 145 to about 175°C, about 145 to about 1145°C, about 145 to about 165°C, about 145 to about 160°C, about 145 to about 155°C, about 145 to about 150°C, about 150 to about 200°C, about 150 to about 195°C, about 150 to about 190°C, about 150 to about 185°C, about 150 to about 180°C, about 150 to about 175°C, about 150 to about 1150°C, about 150 to about 165°C, about 150 to about 160°C, about 150 to about 155°C, about 155 to about 200°C, about 155 to about 195°C, about 155 to about 190°C, about 155 to about 185°C, about 155 to about 180°C, about 155 to about 175°C, about 155 to about 1155°C, about 155 to about 165°C, about 155 to about 160°C, about 160 to about 200°C,A glass transition temperature of about 160 to about 195°C, about 160 to about 190°C, about 160 to about 185°C, about 160 to about 180°C, about 160 to about 175°C, about 160 to about 1160°C, or about 160 to about 165°C. ,
[0064] In addition to a glass transition temperature within one or more of the above ranges, the thermoplastic polymer may also have a tensile modulus higher than most conventional thermoplastic polyurethanes and other similar materials. For example, in some embodiments, the thermoplastic polymer of the present invention may have a tensile modulus greater than 1000 MPa, measured according to ASTM D-638 at a nominal strain rate of 0.1 / min. In embodiments, the tensile modulus of the inventive thermoplastic polymers described herein may be at least about 1250, at least about 1500, or at least about 2000 MPa and / or no greater than about 5000, no greater than about 4000, or no greater than about 3000 MPa, or it may be from about 1000 to about 5000 MPa, from about 1000 to about 4000 MPa, from about 1000 to about 3000 MPa, from about 1250 to about 5000 MPa, from about 1250 to about 4000 MPa, from about 1250 to about 3000 MPa, from about 1500 to about 5000 MPa, from about 1500 to about 4000 MPa, from about 1500 to about 3000 MPa, from about 2000 to about 5000 MPa, from about 2000 to about 4000 MPa, or from about 2000 to about 3000 MPa.
[0065] In embodiments of the present invention, the thermoplastic polymer may also have a "lower processing temperature (Tp)" that is closer to the glass transition temperature than conventional thermoplastic polyesters. The term "lower processing temperature" as used herein refers to a temperature below which the melt viscosity of the polymer exceeds 10,000 poise (P). The lower processing temperature is determined by measuring the viscosity at a shear rate of 25 rad / sec as a function of temperature using an oscillating dynamic mechanical rheometer according to ASTM D-4440. For most conventional polyesters, the change in viscosity as a function of temperature requires that the conventional polyester must be processed at least 140°C above Tg (i.e., the Tp-Tg of the conventional polyester is greater than or equal to greater than 140°C). This places a strict upper limit on the Tg of conventional polyesters because Tp cannot be higher than the temperature at which significant thermal and oxidative degradation occurs. In contrast, the difference between the lower processing temperature and the glass transition temperature (Tp-Tg) of the thermoplastic polymers of the present invention are all less than about 135°C, which allows the Tg of these polymers to be much higher than the Tg of conventional polyesters.
[0066] In certain embodiments, the difference between the lower processing temperature and the glass transition temperature (Tp-Tg) of the thermoplastic polymer of the present invention may be at least about 80, at least about 85, at least about 90, at least about 95, at least about 100, or at least about 105° C. Additionally or alternatively, in certain embodiments, the difference between the lower processing temperature and the glass transition temperature (Tp-Tg) of the thermoplastic polymer of the present invention may be no greater than about 135, no greater than about 130, no greater than about 125, no greater than about 120, no greater than about 115, no greater than about 110, no greater than about 105, no greater than about 100, no greater than about 95, or no greater than about 90° C.
[0067] In embodiments of the present invention, the difference between the lower processing temperature limit and the glass transition temperature (Tp-Tg) of the thermoplastic polymers described herein may be from about 80 to about 135°C, from about 80 to about 130°C, from about 80 to about 125°C, from about 80 to about 120°C, from about 80 to about 115°C, from about 80 to about 110°C, from about 80 to about 105°C, from about 80 to about 105°C, from about 80 to about 100°C, from about 80 to about 95°C, from about 80 to about 90°C, about 85 to about 135°C, about 85 to about 130°C, about 85 to about 125°C, about 85 to about 120°C, about 85 to about 115°C, about 85 to about 110°C, about 85 to about 105°C, about 85 to about 105°C, about 85 to about 100°C, about 85 to about 95°C, about 85 to about 90°C, about 90 to about 135°C, about 90 to about 130°C, about 90 to about 125°C, about 90 to about 120°C, about 90 to about 115°C, about 90 to about 110°C, about 90 to about 105°C, about 90 to about 105°C, about 90 to about 100°C, about 90 to about 95°C, about 95 to about 135°C, about 95 to about 130°C, about 95 to about 125°C, about 95 to about 120°C, about 95 to about 115°C, about 95 to about 110°C, about 95 to about 105°C, about 95 to about 105°C, about 95 to about 100°C, about 100 to about 135°C, about 100 to about 130°C, about 100 to about 125°C, about 100 to about 120°C, about 100 to about 115°C, about 100 to about 110°C, about 100 to about 105°C, about 100 to about 105°C, about 105 to about 135°C, about 105 to about 130°C, about 105 to about 125°C, about 105 to about 120°C, about 105 to about 115°C or about 105 to about 110°C.
[0068] The molecular weight of the thermoplastic polymer can vary and can be selected based at least in part on the desired end use or application of the reaction system. For example, in some embodiments, the thermoplastic polymers described herein can have a number average molecular weight of at least about 3,000, at least about 5,000, at least about 10,000, at least about 15,000, at least about 20,000, or at least about 25,000 Daltons and / or no greater than about 100,000, no greater than about 90,000, no greater than about 80,000, no greater than about 70,000, no greater than about 60,000, no greater than about 50,000, no greater than about 40,000, no greater than about 35,000, no greater than about 30,000, or no greater than about 25,000 Daltons as measured by gel permeation chromatography (GPC) according to ASTM method D-5296 using HFIP / dichloromethane as the solvent on an Agilent 1100 series GPC-SEC system with a refractive index detector calibrated to polystyrene standards.
[0069] In some embodiments, the molecular weight of the thermoplastic polymer may be from about 3,000 to about 100,000 Daltons, from about 3,000 to about 90,000 Daltons, from about 3,000 to about 80,000 Daltons, from about 3,000 to about 70,000 Daltons, from about 3,000 to about 60,000 Daltons, from about 3,000 to about 50,000 Daltons, from about 3,000 to about 40,000 Daltons, from about 3,000 to about 35,000 Daltons, from about 3,000 to about 30,000 Daltons, from about 3,000 to about 25,000 Daltons, from about 5,000 to about 100,000 Daltons, from about 5,000 to about 60,000 Daltons. 00 to about 90,000 daltons, about 5,000 to about 80,000 daltons, about 5,000 to about 70,000 daltons, about 5,000 to about 60,000 daltons, about 5,000 to about 50,000 daltons, about 5,000 to about 40,000 daltons, about 5,000 to about 35,000 daltons, about 5,000 to about 30,000 daltons, about 5,000 to about 25,000 daltons, about 10,000 to about 100,000 daltons, about 10,000 to about 90,000 daltons, about 10,000 to about 80,000 daltons, about 10,000 to about 70,000 Daltons, about 10,000 to about 60,000 Daltons, about 10,000 to about 50,000 Daltons, about 10,000 to about 40,000 Daltons, about 10,000 to about 35,000 Daltons, about 10,000 to about 30,000 Daltons, about 10,000 to about 25,000 Daltons, about 15,000 to about 100,000 Daltons, about 15,000 to about 90,000 Daltons, about 15,000 to about 80,000 Daltons, about 15,000 to about 70,000 Daltons, about 15,000 to about 60,000 Daltons, about 15,000 to about 50,000 Daltons, about 15,000 to about 40,000 Daltons, about 15,000 to about 35,000 Daltons, about 15,000 to about 30,000 Daltons, about 15,000 to about 25,000 Daltons, about 20,000 to about 100,000 Daltons, about 20,000 to about 90,000 Daltons, about 20,000 to about 80,000 Daltons, about 20,000 to about 70,000 Daltons, about 20,000 to about 60,000 Daltons, about 20,000 to about 50,000 Daltons, about 20,000 to about 40,000 Daltons, about 20,, about 25,000 to about 35,000 Daltons, about 20,000 to about 30,000 Daltons, about 20,000 to about 25,000 Daltons, about 25,000 to about 100,000 Daltons, about 25,000 to about 90,000 Daltons, about 25,000 to about 80,000 Daltons, about 25,000 to about 70,000 Daltons, about 25,000 to about 60,000 Daltons, about 25,000 to about 50,000 Daltons, about 25,000 to about 40,000 Daltons, about 25,000 to about 35,000 Daltons or about 25,000 to about 30,000 Daltons.
[0070] Thermoplastic polymers of the present invention can be formed according to any suitable method.For example, in some embodiments, it is optional to combine polymerized polyester diols and monomeric isocyanates in the presence of a catalyst as described above and one or more other additives in a reaction zone.Then polymerized polyester diols, isocyanates and other components (if present) can react to form a thermoplastic polymer having a composition, glass transition temperature, modulus and molecular weight within one or more scopes provided herein.When using two or more polymerized polyester diols to form a thermoplastic polymer, it is possible to combine polymerized polyester diols before or during reaction with isocyanate monomers.The polymerized polyester diols and isocyanate starting materials of thermoplastic polymers as herein described can react continuously in, for example, a single screw or twin screw extruder.Optionally, the reaction can be carried out in a batch or semi-batch reaction vessel.
[0071] In some embodiments, the temperature of the reaction can be at least about 200, at least about 220, at least about 230, at least about 240, at least about 250°C and / or no greater than about 340, no greater than about 330, no greater than about 320, no greater than about 310, or no greater than about 300°C, or the temperature can be from about 200 to about 340°C, from about 200 to about 330°C, from about 200 to about 320°C, from about 200 to about 310°C, from about 200 to about 300°C, from about 220 to about 340°C, from about 220 to about 330°C, from about 220 to about 320°C, 300°C, about 220 to about 310°C, about 200 to about 300°C, about 230 to about 340°C, about 230 to about 330°C, about 230 to about 320°C, about 230 to about 310°C, about 230 to about 300°C, about 240 to about 340°C, about 240 to about 330°C, about 240 to about 320°C, about 240 to about 310°C, about 240 to about 300°C, about 250 to about 340°C, about 250 to about 330°C, about 250 to about 320°C, about 250 to about 310°C or about 250 to about 300°C.
[0072] As described above, the glass transition temperature of the thermoplastic materials of the present invention can be higher than conventional thermoplastic polyurethanes and polyesters and thus the difference between the reaction temperature and the glass transition temperature of the resulting thermoplastic polymer can be less for the thermoplastic resins of the present invention than for other conventional polymers. For example, in some embodiments, the difference between the glass transition temperature of the thermoplastic polymers of the present invention and the temperature at which the polymer is formed is no greater than about 175, no greater than about 160, no greater than about 150, no greater than about 135, no greater than about 120, no greater than about 100, no greater than about 80, no greater than about 70, no greater than about 60, or no greater than about 50° C. Similarly, in some embodiments, comparable differences between the average melting temperature and the glass transition temperature of the thermoplastic polymers can also be observed during melt processing of the thermoplastic resins of the present invention.
[0073] Once formed, the thermoplastic polymer can be any suitable solid shape or form and can have, for example, a total solids content of at least about 90, at least about 95, at least about 97, at least about 99, or at least about 99.5% by weight of the thermoplastic polymer, as measured according to ASTM D-2369. Examples of suitable forms can include, but are not limited to, polymer particles or pellets or as extruded films or sheets. In embodiments of the present invention, the thermoplastic polymer compositions described herein can contain little or no liquid components and can contain, for example, less than about 5, less than about 3, less than about 1, or less than about 0.5% by weight of solvent or other liquid phase components based on the total weight of the polymer composition. Therefore, in some embodiments, the thermoplastic polymers described herein may not be suitable for applications requiring solvent-based or water-based coatings.
[0074] In embodiments of the present invention, thermoplastic polymers as described herein are suitable for making many shaped articles, including but not limited to sheets, films, pipes, preforms, bottles, profiles and other similar articles. Such articles can be generated by any suitable method using thermoplastic resins according to various embodiments of the present invention. Examples of such methods include but are not limited to extrusion, calendering, thermoforming, blow molding, extrusion blow molding, injection molding, reactive injection molding, compression molding, casting, drafting, tentering or blowing molding according to the type of shaped article.
[0075] The following examples are given to illustrate the present invention and enable those skilled in the art to implement and use the present invention. However, it should be understood that the present invention is not limited to the specific conditions or details described in these examples. The patentable scope of the present invention is limited by the claims and may include other embodiments that occur to those skilled in the art. Example
[0076] Example 1 Several isocyanate-modified thermoplastic polymers were formed according to the following general procedure. First, at least one monomeric diacid and at least one monomeric diol (type and amount of which are summarized in Table 2 below) were loaded into a 500 mL single-necked round-bottom flask equipped with a metal stirrer. The amount in Table 2 is mol%, based on 100 mol% of the acid component and 100 mol% of the diol component. The flask is also equipped with an agitator adapter with a sidearm condenser, which is configured so that the sidearm extends into a measuring cylinder connected to a vacuum trap. The vacuum trap is filled with a mixture of isopropanol and dry ice and the measuring cylinder is placed in a dry ice bucket. The flask is vacuum purged to a pressure of 5 Torr twice, then covered with nitrogen.
[0077] A separate metal bath is preset to a temperature of 220°C and the flask is introduced into the metal bath. When the round-bottom flask is inserted into the metal bath, the temperature setting point is reduced to 190°C and the agitator is set at 50 rpm. When the flask contents are completely dissolved, the agitator speed is increased to 250 to 265 rpm. If no condensation occurs, the temperature setting point of the metal bath is also increased in 10°C increments until a maximum bath temperature of 230 to 245°C is reached, depending on the polymerized polyester diol formed. When the maximum bath temperature is reached, the flask contents are stirred for one hour. The pressure in the flask is then reduced to 100 torr and maintained for another hour. Thereafter, the vacuum is released and the polyol is evacuated to an aluminum pan. The resulting cooled polymeric diol is then broken into small pieces and its glass transition temperature and number average molecular weight are determined by DSC and GPC, respectively, as described herein.
[0078] Table 1 provides a summary of the monomeric diacids and monomeric diols used to form the polymeric polyester diols listed in Table 2. Table 2 also provides the glass transition temperature and number average molecular weight of each of the polymeric polyester diols listed in Table 2.
[0079] Several polymeric polyester diols listed in Table 2 above were then used to form isocyanate-modified thermoplastic polymers according to the following procedure.
[0080] A certain amount (depending on the specific composition of the polymer formed) of one of the polymerized polyester diols shown in Table 2 is added to a 500 mL round-bottom flask equipped with heating and stirring functions. For thermoplastic polymers that also contain supplementary diols, an appropriate amount of supplementary diols is also added to the flask. The contents of the flask are then heated to a temperature of 230°C and maintained until all the contents are completely melted, and then the contents are stirred to promote thorough mixing. Solid pieces of 4,4'-diphenylmethane diisocyanate (MDI) are then added to the reaction mixture along with any catalyst (if used) and the contents are vigorously stirred until the contents are too viscous to stir. At this point, the flask is cooled to room temperature, at which point the contents of the flask are removed by breaking the flask and cutting off the polymer from the agitator. The relative amounts of each component in weight % are shown in Table 3.
[0081] The glass transition temperature and number average molecular weight of each polymer sample in this and all subsequent examples were measured according to the procedure described herein. Table 3 below summarizes the composition of several isocyanate-modified thermoplastic polymers prepared according to this procedure and the glass transition temperature and number average molecular weight measured for each polymer.
[0082] Example 2 Additional isocyanate-modified thermoplastic polymers were prepared according to the following procedure.
[0083] First, several polymerized polyester diols were prepared using a 3 L 3-neck flask equipped with a steel stir bar, a 24 / 40 nitrogen inlet, a 45 / 50 stir bar adapter, a 24 / 40 polymer thermocouple neck, two thermocouples, a reflux condenser, a polymer condenser arm with a 10 / 30 fitting (the thermometer fits into the 10 / 30 fitting), and a condensate collection cylinder with a 24 / 40 fitting. The condenser was connected to a cooling water system and the 3 L flask was placed in a solid heating mantle instead of a metal bath.
[0084] To prepare each polymerized polyester diol, all monomers of a particular composition were introduced into a 3L flask along with FASTCAT 4100 (a tin-based catalyst). Sufficient catalyst was added to make the reaction mixture contain approximately 600 ppm tin based on the total weight of the reaction mixture. When two monomer diols were used, the diols were added at a ratio of approximately 1.33:1. The computer controlled the reaction temperature. Initially, a heating mantle was used to control the temperature of the reaction melt to melt the reactants in the center portion of the bottom of the flask by placing a mantle thermocouple between the flask and the mantle. The mantle temperature was then set at 200°C and the stirring speed was set at 70 rpm.
[0085] After the material formed a slurry, an initial melt thermocouple was immersed in the melt and connected to the experimental apparatus, after which the reaction temperature was controlled by the melt thermocouple. When necessary, a circulating bath with heating oil and heating tape (each set to a temperature of approximately 135°C) was used to melt any sublimated 2,2,4,4-tetramethyl-1,3-cyclobutanediol and keep it within the flask. Heating oil was circulated through the reflux condenser and heating tape was placed around the exposed glass near the top of the flask.
[0086] After the material was completely melted, the temperature of the melt was steadily increased from 190°C to about 230°C over about 3 hours. After reaching a temperature of 230°C, the melt was maintained at that temperature for about 3 ½ hours, then cooled and poured into a metal pan for recovery. The resulting polymeric diol was then broken into small pieces and its glass transition temperature and number average molecular weight were determined by DSC and GPC, respectively.
[0087] Table 4 below summarizes the glass transition temperature and number average molecular weight of each polymerized polyester diol formed as described above. The names of the types of monomeric acids and monomeric diols shown in Table 4 are consistent with those in Table 1 above. The amount of each component is shown in Table 4 in mole %, based on the acid component being 100 mole % and the diol component being 100 mole %.
[0088] Several additional isocyanate-modified thermoplastic polymers were then formed from the polymerized polyester diols shown above in Table 4 in a manner similar to that described above in Example 1. The glass transition temperature and number average molecular weight of each resulting thermoplastic polymer were measured and the results are summarized in Table 5 below along with the composition of each polymer.
[0089] Example 3 Several additional isocyanate-modified thermoplastic polymers were prepared according to the following procedure.
[0090] Polyester diol was prepared using 4L Parr 4551 pressure vessel, reflux condenser and water-cooled condenser. In order to form the polyester diol, 625.4 grams of terephthalic acid (TPA), 208.27 grams of isophthalic acid (IPA) or dimethyl 2,6-naphthalene dicarboxylate, 565.77 grams of ethylene glycol (EG) and 231.3 grams of 1,4-cyclohexanedimethanol (CHDM) were loaded into a metal beaker together with 19.12 grams of titanium catalyst in ethylene glycol. Ethylene glycol was loaded in excess of about 100%. Titanium metal concentration was about 50 ppm, based on the gross weight of the reaction mixture. The reaction mixture was stirred and formed into a slurry on a hot plate set to a temperature of 85 ° C. Thereafter, the resulting mixture was loaded into a Parr container by vacuum and the temperature of the reactor was set to 170 ° C, then the mixture was heated using an automatic heating curve. Stirring speed was initially set at 150 rpm.
[0091] After the oligomeric polyester diol has been formed, the molar ratio of diol to acid is measured by NMR and excess ethylene glycol is removed to reach the calculated target molecular weight. The oligomer is added to a 3L 3-neck flask and heated to a temperature of 230°C, at which point the pressure in the flask is reduced to 50 Torr. Excess ethylene glycol removed and recovered via passage through a water-cooled condenser is measured in a graduated cylinder and when the target amount of recovered ethylene glycol is reached, the resulting polymer melt is poured from the flask into a metal pan and cooled. The resulting polymeric diol is then broken into small pieces and its glass transition temperature and number average molecular weight are measured by DSC and GPC, respectively.
[0092] Table 6 below summarizes the glass transition temperature and number average molecular weight of each polymerized polyester diol formed as described above. The names of the types of monomeric acids and monomeric diols shown in Table 6 are consistent with those in Table 1 above. The amount of each component is shown in Table 6 in mole %, based on the acid component being 100 mole % and the diol component being 100 mole %.
[0093] Several additional isocyanate-modified thermoplastic polymers were then formed in a similar manner as described above in Example 1. The glass transition temperature and number average molecular weight of each resulting thermoplastic polymer were measured and the results are summarized in Table 7 below, along with the composition of each polymer.
[0094] Example 4 Several isocyanate-modified thermoplastic polymers were prepared in a pilot scale facility according to the following procedure.
[0095] First, the reactor system is purged with nitrogen and 544 pounds of a mixture of 90 weight % 2,2,4,4-tetramethyl-1,3-cyclobutanediol in methanol are added to the reactor while continuing nitrogen purging at 10 standard cubic feet per hour. The reactor temperature is raised to 120°C and the agitator is started at a speed of 25rpm. Once the internal temperature of the reactor reaches 60°C, the agitator is stopped. When a temperature of 120°C is reached, the reactor contents are then cooled to 100°C and excess methanol is removed from the reactor trap. The remaining raw materials, which include 196 pounds of dimethyl terephthalate, 58 pounds of 1,4-cyclohexanedimethanol, 127 grams of FASTCAT4100 catalyst and 28 grams of manganese acetate catalyst, are loaded into the reactor and the temperature is raised to 230°C. When the reaction temperature reaches 160°C, the agitator is opened again at 25 rpm.
[0096] Once the reaction mixture reaches a temperature of 230°C, the contents are maintained at a temperature of 230°C and an agitator speed of 25 rpm for 4 hours. After 4 hours, the reaction vessel pressure is reduced to 100 mm Hg, at which point the reactor contents are maintained at that temperature and pressure for an additional 2 hours. After 2 hours, the resulting polymerized polyester diol (PPD-63) is cooled to 180°C and emptied into a suitable container for cooling. The polymerized polyester diol comprises an acid component having 100 mole % of terephthalic acid residues (based on 100 mole % of the acid component) and a diol component having 30 weight % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues and 70 weight % of 1,4-cyclohexanedimethanol residues (based on 100 mole % of the diol component). The polymerized polyester diol has a glass transition temperature of 47.5°C and a number average molecular weight of 742 Daltons.
[0097] The polymerized polyester diol was divided into several samples and each sample was added to a 500 mL flask along with 4,4'-diphenylmethane diisocyanate (MDI) and 1,4-cyclohexanedimethanol (CHDM), 1,4-benzenedimethanol (BDM), 2,6-decalin dimethanol (DDM), 1,4-cyclohexanediol (CDO) (when used) as supplementary monomer diols to form several isocyanate-modified thermoplastic polymers in a similar manner as described in Example 1. The resulting thermoplastic polymers were recovered and the glass transition temperature and number average molecular weight of each sample were measured as described above. The results of these measurements are summarized in Table 8 below along with the composition of each polymer.
[0098] Example 5 Several isocyanate modified thermoplastic polymers were prepared in a pilot scale facility according to the following procedure. First, several additional polymeric polyester diols were prepared according to the procedure described in Example 4. Table 9 below summarizes the glass transition temperature and number average molecular weight of each polymeric polyester diol. The names of the types of monomeric acids and monomeric diols shown in Table 9 are consistent with those in Table 1 above and the amounts of monomers are in mole % based on 100 mole % of the acid component and 100 mole % of the diol component.
[0099] Each polymeric polyester diol listed in Table 9 was then combined with solid flake 4,4'-diphenylmethane diisocyanate (MDI) and, where used, 1,4-cyclohexanedimethanol (CHDM) in a 40 mm twin screw extruder having an L / D of 52, combined with a Gala underwater cutting system. The resulting thermoplastic polymer was produced at an average rate of 30 kg / hour to 100 kg / hour and the pellets were used for film pressing, molded parts, and evaluation of various physical properties, including glass transition temperature and number average molecular weight. Table 10 below summarizes the composition of each isocyanate-modified thermoplastic polymer formed according to this method along with analytical results.
[0100] Example 6 Samples of selected polymeric materials formed in Examples 1 to 5 above were ground and pressed into 0.9 mm thick films on a Carver press for 3 minutes at the temperatures summarized in Table 11 below. Modulus values were then measured according to ASTM D-638 at a crosshead speed of 1.4 mm / min (a nominal strain rate of 0.1 / min) on ASTM D-638 Type V dogbone specimens cut from the pressed films. As shown in Table 11 below, each of the inventive polymers had a modulus value greater than 1000 MPa, confirming that these are considered hard materials.
[0101] Example 7 The lower processing temperature limits (Tp) of several polymers from Examples 1 to 5 above were determined by grinding the sample at a shear rate of 25 rad / sec in an RDA melt rheometer while increasing the temperature from 200°C to 260°C at a scan rate of 5°C / min. The results are summarized in Table 12 below. In addition, the lower processing temperature limits (Tp) values of several comparative thermoplastic polyesters (PC-A to PC-D) were also determined according to this method. PC-A is TRITAN® copolyester TX1001, PC-B is TRITAN® copolyester TX1500HF, PC-C is EASTAR® copolyester 6763, and PC-D is EASTAR® copolyester 5011 (all available from Eastman Chemical Company). The results of the comparative thermoplastic polyesters are also summarized in Table 12.
[0102] A graphical representation of the full temperature scans of selected inventive and comparative materials according to the above procedure is provided at Figure 1 and 2 In. Figure 1 and 2 As shown, the viscosity of thermoplastic polymers formed according to embodiments of the present invention varies more significantly with temperature than conventional thermoplastic polyesters.
[0103] definition The term "comprising" as used herein is an open transition term that is used to transform the object described before the term to one or more elements described after the term, wherein the one or more elements listed after the transition term are not necessarily the only elements that constitute the object.
[0104] As used herein, the term "including" has the same open-ended meaning as "comprising."
[0105] As used herein, the term "having" has the same open-ended meaning as "comprising."
[0106] As used herein, the term "comprising" has the same open-ended meaning as "including."
[0107] As used herein, the terms "a," "an," "the," and "said" refer to one or more.
[0108] As used herein, the term "and / or" when used in conjunction with a list of two or more items means that any one of the listed items may be used alone or any combination of two or more of the listed items may be used. For example, if a composition is described as comprising components A, B, and / or C, the composition may comprise A alone, B alone, C alone, a combination of A and B, a combination of A and C, a combination of B and C, or a combination of A, B, and C.
[0109] The preferred forms of the present invention described above are for illustration only and should not be used to interpret the scope of the present invention in a limiting sense. Obvious modifications to the above exemplary embodiments can be easily made by those skilled in the art without departing from the spirit of the present invention.
[0110] The inventors hereby declare that it is their intention to rely on equivalents to determine and assess the fair and equitable scope of the present invention as any device that does not materially depart from the literal scope of the present invention as set forth in the following claims.
Claims
1. A thermoplastic polymer comprising: (a) the residue of at least one linear polymeric polyester diol, wherein the linear polymeric polyester diol comprises the residue of: (i) at least one monomeric diacid selected from terephthalic acid or dimethyl 2,6-naphthalene dicarboxylate; and (ii) at least two monomeric diols including 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 1,4-cyclohexanedimethanol, wherein the linear polymeric polyester diol has a number average molecular weight of at least 400 Daltons; and (b) residues of at least one diisocyanate monomer, wherein the residues of the diisocyanate monomers are present in the polymer in an amount of no greater than 40 wt % based on the total weight of the polymer, wherein the polymer has a glass transition temperature of at least 140°C, and wherein the polymer has a lower processing temperature limit (Tp) and the difference between the lower processing temperature limit (Tp) and the glass transition temperature (Tg) of the polymer is 80-110°C.
2. The polymer according to claim 1, wherein the linear polymeric polyester diol has a number average molecular weight of 400 to 5000 Daltons.
3. The polymer according to claim 1, wherein the linear polymeric polyester diol has a glass transition temperature of at least 35°C.
4. The polymer according to claim 1, wherein the linear polymeric polyester diol comprises residues of the following monomeric diols: 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 1,4-cyclohexanedimethanol and less than 5 mole % of any other monomeric diols based on the total moles of diol components.
5. The polymer according to claim 1, wherein the linear polymeric polyester diol comprises the residue of terephthalic acid.
6. The polymer according to claim 1, wherein the diisocyanate monomer comprises an aromatic diisocyanate monomer.
7. The polymer according to claim 6, wherein the diisocyanate monomer comprises 4,4'-diphenylmethane diisocyanate.
8. The polymer according to claim 1, wherein the polymer further comprises at least 0.5 wt. %, based on the total weight of the polymer, of residues of at least one supplemental monomeric diol.
9. The polymer according to claim 8, wherein the polymer further comprises at least 0.5 wt. % of the residue of at least one supplemental monomeric diol, based on the total weight of the polymer, wherein the supplemental monomeric diol is selected from the group consisting of isosorbide, 1,3-cyclohexanedimethanol, ethylene glycol, 2,6-decalin, tricyclodecane dimethanol, 1,4-benzenedimethanol, neopentyl glycol, and combinations thereof.
10. The polymer according to claim 1, further comprising residues of at least one branching monomer and / or at least one polyfunctional isocyanate, wherein the total amount of said residues of said branching monomer and said polyfunctional isocyanate present in said polymer is no greater than 1 wt %, based on the total weight of said polymer.
11. The polymer according to claim 1, wherein the linear polymeric polyester diol has a number average molecular weight of 600 to 1200 Daltons and the polymer has a number average molecular weight of at least 10,000 Daltons.
12. The polymer according to claim 1, wherein the polymer has a tensile modulus of at least 1000 MPa.
13. The polymer according to claim 1, wherein the linear polymeric polyester diol has a number average molecular weight of 500 to 2000 Daltons and a glass transition temperature of at least 35°C, wherein the polymer comprises from 0.5 to 20 weight percent, based on the total weight of the polymer, of residues of at least one supplemental monomeric diol, wherein the polymer has a glass transition temperature of no greater than 200°C, and wherein the polymer has a tensile modulus of at least 1000 MPa.
14. The polymer according to claim 1, wherein the polymer has a glass transition temperature of at least 145°C, wherein the polymer has a tensile modulus of at least 1000 MPa, and wherein the residue of the diisocyanate monomer is present in the polymer in an amount of no greater than 35 weight percent based on the total weight of the residues of the polymer.
15. The polymer according to claim 1, wherein the polymer has a lower processing temperature limit (Tp) and the difference between the lower processing temperature limit (Tp) and the glass transition temperature (Tg) of the polymer is 80-100°C.
16. Shaped articles formed from the polymer according to claim 1.
17. A method for preparing a thermoplastic polymer, comprising: combining at least one polymeric polyester diol, at least one monomeric diisocyanate, and optionally at least one supplemental monomeric diol, optionally in the presence of a catalyst, in a reaction zone; and reacting the combination in a reaction zone to form a thermoplastic polymer; wherein the thermoplastic polymer comprises: (a) the residue of at least one linear polymeric polyester diol, wherein the linear polymeric polyester diol comprises the residue of: (i) at least one monomeric diacid selected from terephthalic acid or dimethyl 2,6-naphthalene dicarboxylate; and (ii) at least two monomeric diols including 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 1,4-cyclohexanedimethanol; wherein the linear polymeric polyester diol has a number average molecular weight of at least 400 Daltons; and (b) residues of at least one diisocyanate monomer, wherein the residues of the diisocyanate monomers are present in the polymer in an amount of no greater than 40 weight percent, based on the total weight of the polymer, and wherein the polymer has a glass transition temperature of at least 140°C, and wherein the polymer has a lower processing temperature limit (Tp) and the difference between the lower processing temperature limit (Tp) and the glass transition temperature (Tg) of the polymer is 80-110°C.