Polyamic acid for low-temperature curing power semiconductor packaging and preparation method thereof
By introducing flexible groups and polyether bonds into polyimidic acid, reducing the glass transition temperature and improving the bonding strength, the adhesion, matching and curing time energy of polyimidic acid in the prior art is solved. Inadequate consumption has achieved low temperature curing and high reliability power semiconductor packaging.
Patent Information
- Application Number
- CN202411119365.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-15
AI Technical Summary
The existing polyimides for power semiconductor packaging have shortcomings in adhesion, matching, reliability and curing time and energy consumption, especially incomplete thermal imidation, resulting in poor device yield and long-term operation reliability.
Copolymerization in polar aprotic solvents using diether dianhydride with polyethylene glycol chains, aromatic diamines containing flexible spacer groups and bis(3-aminopropyl)-terminated polydimethylsiloxanes. , introduce flexible groups and polyether bonds, reduce glass transition temperature, improve bonding strength and adhesion, control molecular weight and molar ratio, and achieve low temperature curing.
The low-temperature curing of polyimidic acid (≤220℃, ≤4h) is achieved, and the degree of imidation is reached by 100%, which improves the matching and bonding strength with the device, enhances heat resistance and electrical insulation. Improves the long-term operation reliability and stability of power semiconductor devices.
Smart Images

Figure CN118994577A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of liquid polyimide coating adhesive, and in particular relates to a polyamic acid for low-temperature curing power semiconductor packaging and a preparation method thereof. Background Art
[0002] After thermal imidization, the polyamic acid for power semiconductor packaging not only has the excellent physical and chemical properties inherent in polyimide, but also has high bonding strength with materials such as silicon, aluminum, copper, nickel, ceramics or aluminum nitride. It can be coated on the surface of power semiconductors as a protective layer to improve the insulation level of the device. However, the polyamic acid for power semiconductor packaging currently produced in China has certain deficiencies in terms of adhesion to the substrate, matching with the device manufacturing process, reliability guarantee for long-term operation of the device, and time and energy consumption required for curing.
[0003] Chinese patent document CN103865471A provides a method for preparing a polyimide adhesive, wherein 2,2-bis[4-(4-aminophenoxy)phenyl]propane, diaminodiphenyl ether and 2,3,3',4'-diphenyl ether tetraacid dianhydride are used to react to generate polyamic acid, and then polyimide powder is obtained through chemical imidization and powder making processes. The curing temperature of the polyimide powder is only 170-200°C, and it is not easy to generate bubbles or form voids in the adhesive layer, but its bonding strength with substrates such as copper, aluminum, platinum and stainless steel is relatively general. It can be used and promoted initially in some power semiconductor packaging fields where bonding performance is not high, but it is difficult to achieve application when bonding strength requirements are more stringent.
[0004] Chinese patent document CN102093559A discloses a polyimide electronic packaging material and a synthesis method thereof, which firstly dissolves 2,3,3',4'-biphenyltetracarboxylic acid dianhydride and 2,2'-bis(trifluoromethyl)-4,4-diaminodiphenyl sulfide in an aprotic polar solvent in equal molar ratios to react and synthesize polyamic acid; then, the prepared polyamic acid is placed in a high-temperature oven for imidization according to the following procedure: 80°C / 3h, 150°C / 1h, 180°C / 1h, 250°C / 1h, 300°C / 1h, 350°C / 15min, and naturally cools to obtain a power semiconductor packaging polyimide material. This material has high light transmittance, low water absorption, excellent mechanical properties and high temperature resistance, but its glass transition temperature is generally higher than 300°C. In the power semiconductor packaging process, there may be problems with incomplete thermal imidization, which is poorly matched with the device manufacturing process, thus affecting the yield and long-term operation reliability of power semiconductor devices. In addition, the entire imidization heating time is ≥7h, which is time-consuming and energy-intensive. Summary of the invention
[0005] In order to overcome the problems in the prior art, the present invention provides a low-temperature curing polyamic acid for power semiconductor packaging and a preparation method thereof. The prepared polyamic acid has a maximum curing temperature of ≤220°C, a curing time of ≤4h, an imidization degree of 100%, and is highly compatible with the manufacturing process of power semiconductor devices. After curing, it has outstanding heat resistance, electrical insulation and substrate adhesion, can achieve good packaging of power semiconductor devices, protect the interconnection inside the device, and prevent the device from mechanical and chemical damage, thereby improving the long-term operation reliability and stability of the power semiconductor device.
[0006] In order to solve the above technical problems, the technical solutions proposed by the present invention are as follows:
[0007] A low-temperature curing polyamic acid for power semiconductor packaging is prepared by copolymerizing a diether dianhydride with a polyethylene glycol chain in the middle, an aromatic diamine containing a flexible spacer group and a bis(3-aminopropyl)-terminated polydimethylsiloxane in a polar aprotic solvent, wherein the average molecular weight of the (3-aminopropyl)-terminated polydimethylsiloxane is ≤3000 g / mol; and the molar ratio of the total molar amount of the bis(3-aminopropyl)-terminated polydimethylsiloxane and the aromatic diamine containing a flexible spacer group to the diether dianhydride with a polyethylene glycol chain in the middle is 1.00:(0.95-1.1).
[0008] In the present invention, a flexible group is introduced into the polyimide molecular chain to make the flexibility of the polyimide molecular chain lower, and the main chain of the polyimide molecular chain and the end-capped flexible side chain act together to further reduce the glass transition temperature of the polyimide while maintaining high insulation. In addition, phenoxy, siloxane, etc. make the material have a very strong hydrogen bond interaction, and the polyimide shows a higher cohesive energy and interface adhesion energy to increase the free volume of the polyimide condensed structure. Simultaneously, the average molecular weight of the (3-aminopropyl) end-capped polydimethylsiloxane is controlled to be less than or equal to 3000 g / mol, which is conducive to the reaction. The molecular weight is too large, the molecular chain is too long, the reaction activity is not enough, the polyamic acid resin performance is not good, and the molecular chain is prone to entanglement, and the adhesion decreases.
[0009] Furthermore, the molar ratio of the total molar amount of the bis(3-aminopropyl)-terminated polydimethylsiloxane and the aromatic diamine containing a flexible spacer group to the molar amount of the diether dianhydride with a polyethylene glycol chain in the middle is preferably 1.00:(0.99-1.0).
[0010] As an optional embodiment, in the polyamic acid provided by the present invention, the molar ratio of the bis(3-aminopropyl)-terminated polydimethylsiloxane to the aromatic diamine containing a flexible spacer group is 1.00:(15.00-20.00).
[0011] In the present invention, controlling the molar ratio of the bis(3-aminopropyl)-terminated polydimethylsiloxane to the aromatic diamine containing a flexible spacer group can further improve the low-temperature curing and adhesion of the product. If the ratio of the bis(3-aminopropyl)-terminated polydimethylsiloxane is too low, the effect is not obvious, and if the ratio is too high, the reaction activity is too high.
[0012] As an optional embodiment, in the polyamic acid provided by the present invention, the flexible spacer group in the aromatic diamine is selected from one of the alkyl groups having 1 to 12 carbon atoms.
[0013] In the present invention, the use of alkyl groups as flexible groups can hinder the orderly stacking and arrangement of conjugated units, improve the flexibility of the molecular chain, and reduce the curing temperature.
[0014] As an optional embodiment, in the polyamic acid provided by the present invention, the diether dianhydride with a polyethylene glycol chain in the middle is selected from one or more of bis(phthalic anhydride) linked by -OCH2CH2O-, bis(phthalic anhydride) linked by -(OCH2CH2O)2-, bis(phthalic anhydride) linked by -(OCH2CH2O)3-, bis(phthalic anhydride) linked by -(OCH2CH2O)4-, bis(phthalic anhydride) linked by -(OCH2CH2O)5-, and bis(phthalic anhydride) linked by -(OCH2CH2O)6-.
[0015] In the present invention, the introduction of polyethylene glycol in the dianhydride can promote the formation of hydrogen bonds with the substrate during the application process, improve the adhesion of the material, and at the same time play a role in reducing the glass transition temperature.
[0016] As an optional embodiment, in the polyamic acid provided by the present invention, the aromatic diamine containing a flexible spacer group is selected from bis(4-aminophenoxy)methane, 1,2-bis(4-aminophenoxy)ethane, 1,2-bis(3-aminophenoxy)ethane, 1,2-bis(4-aminophenoxy)propane, 1,2-bis(4-aminophenoxy)pentane, 1,2-bis(4-aminophenoxy)octane, 1,3-bis(4-aminophenoxy)propane, 1,3-bis(3-aminophenoxy)propane, 2,2-bis(4-aminophenoxymethylene)propane, 2,2-bis(4-aminophenoxymethylene)pentanepropane, 2,2-diethyl-1,3-bis(4-aminophenoxy)propane, 1,4-bis( One or more of 1,4-bis(m-aminophenoxy)butane, 1,5-bis(p-aminophenoxy)pentane, 1,5-bis(m-aminophenoxy)pentane, 1,6-bis(p-aminophenoxy)hexane, 1,6-bis(m-aminophenoxy)hexane, 1,8-bis(p-aminophenoxy)octane, 1,8-bis(m-aminophenoxy)octane, 1,9-bis(p-aminophenoxy)nonane, 1,9-bis(m-aminophenoxy)nonane, 1,10-bis(p-aminophenoxy)decane, 1,10-bis(m-aminophenoxy)decane, 1,12-bis(p-aminophenoxy)dodecane and 1,12-bis(m-aminophenoxy)dodecane.
[0017] As an optional embodiment, in the polyamic acid provided by the present invention, the bis(3-aminopropyl)-terminated polydimethylsiloxane is selected from one or more of an average molecular weight of 248 g / mol, an average molecular weight of 1000 g / mol, an average molecular weight of 2500 g / mol, and an average molecular weight of 3000 g / mol.
[0018] The siloxane group in the bis(3-aminopropyl)-terminated polydimethylsiloxane of the present invention can enhance the adhesion between the material and the substrate, and the bisamino group can play a reactive role, thereby achieving the introduction into the main chain of the polyimide and improving the stability of the material.
[0019] As an optional embodiment, in the polyamic acid provided by the present invention, the maximum curing temperature of the polyamic acid is ≤220° C., the curing time is ≤4 h, and the imidization degree reaches 100%.
[0020] Based on the same technical concept, the present invention also provides a method for preparing the above-mentioned low-temperature curing polyamic acid for power semiconductor packaging, comprising the following steps:
[0021] S1. In a high-purity inert gas atmosphere, an aromatic diamine containing a flexible spacer group and a bis(3-aminopropyl)-terminated polydimethylsiloxane are dissolved in a polar aprotic solvent.
[0022] S2. The reaction temperature is 0-5° C., and diether dianhydride with a polyethylene glycol chain in the middle is added to the system of step S1 in batches for copolymerization. The reaction time is 6-8 hours to obtain low-temperature curing polyamic acid for power semiconductor packaging.
[0023] As an optional embodiment, in the preparation method provided by the present invention, the polar aprotic solvent is selected from one or more of dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide.
[0024] As an optional embodiment, in the preparation method provided by the present invention, the addition amount of the polar aprotic solvent accounts for 70.0-90.0% of the mass of the polyamic acid for low-temperature curing power semiconductor packaging.
[0025] Furthermore, it is preferably 80.0 to 85.0%.
[0026] As an optional embodiment, in the preparation method provided by the present invention, the total addition amount of the aromatic diamine monomer containing a flexible spacer group and the diether dianhydride monomer with a polyethylene glycol chain in the middle accounts for 10.0 to 30.0% of the mass of the polyamic acid for low-temperature curing power semiconductor packaging.
[0027] Furthermore, it is preferably 15.0 to 20.0%.
[0028] As an optional embodiment, in the preparation method provided by the present invention, the inert gas is selected from one or more of helium, neon, argon, krypton, xenon, radon, nitrogen and carbon dioxide.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] (1) The low-temperature curing polyamic acid for power semiconductor packaging of the present invention is prepared by copolymerizing a diether dianhydride with a polyethylene glycol chain in the middle, an aromatic diamine containing a flexible spacer group and a bis(3-aminopropyl)-terminated polydimethylsiloxane (average molecular weight ≤3000 g / mol) in a polar aprotic solvent. Multiple ether bonds and flexible fatty chain structures are introduced into the main chain structure of the molecule, thereby giving the polyimide molecular chain higher flexibility, increasing the free volume of the polyimide condensed structure, greatly reducing its glass transition temperature, making its maximum curing temperature ≤220°C, the curing time ≤4h, and the imidization degree reaching 100%, which is highly compatible with the manufacturing process of power semiconductor devices.
[0031] (2) The molecular main chain of the polyamic acid for low-temperature curing power semiconductor packaging of the present invention contains a large amount of phenoxy and siloxane structures, which enables it to have high bonding strength with base materials such as silicon, aluminum, copper, nickel, ceramics or aluminum nitride at the molecular level. The bonding strength with the aluminum nitride substrate is ≥15.0MPa, which is more than 10 times that of ordinary polyimide products. The cross-hatch test result reaches level 0, which has ultra-high bonding strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0033] Figure 1 The thermal imidization process of the polyamic acid for low temperature curing power semiconductor packaging prepared in Examples 1-8;
[0034] Figure 2 Thermal imidization procedure of PMDA / ODA polyamic acid prepared in Comparative Example 1;
[0035] Figure 3 These are infrared curves of the low-temperature curing polyamic acid for power semiconductor packaging prepared in Example 1 and the polyamic acid prepared in Comparative Example 1 after thermal imidization. DETAILED DESCRIPTION
[0036] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0037] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0038] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0039] Example 1
[0040] A method for preparing a low-temperature curing polyamic acid for power semiconductor packaging comprises the following steps: (1) in a 1000 ml three-necked flask under a high-purity argon gas atmosphere, adding (34.54 g, 0.15 mol) of bis(4-aminophenoxy)methane and (2.48 g, 0.01 mol) of bis(3-aminopropyl)-terminated polydimethylsiloxane (molecular weight 248 g / mol), and using (443.87 g) of N-methylpyrrolidone (solid (2) adding (41.31 g, 0.16 mol) of di(phthalic anhydride) linked by -OCH2CH2O- to the system after step (1) in 7 batches (60%, 30%, 8%, 1%, 0.5%, 0.3%, 0.1%) at a reaction temperature of 0-5°C to carry out copolymerization reaction, with an addition interval of 0.8h and a total reaction time of 8h to obtain a low-temperature curing polyamic acid for power semiconductor packaging.
[0041] Example 2
[0042] A method for preparing a low-temperature curing polyamic acid for power semiconductor packaging comprises the following steps: (1) in a high-purity argon gas atmosphere, in a 1000 ml three-necked flask, adding (36.64 g, 0.15 mol) of 1,2-bis(4-aminophenoxy)ethane and (2.48 g, 0.01 mol) of bis(3-aminopropyl)-terminated polydimethylsiloxane (molecular weight 248 g / mol), and using (455.77 g) of N-methylpyrrolidone (solid content is 15%) to completely dissolve it; (2) the reaction temperature is 0-5°C, and 41.31 g, 0.16 mol) of di(phthalic anhydride) linked by -OCH2CH2O- is added to the system after step (1) in 7 batches (60%, 30%, 8%, 1%, 0.5%, 0.3%, 0.1%) for copolymerization reaction. The addition interval time is 0.8h and the overall reaction time is 8h to obtain low-temperature curing polyamic acid for power semiconductor packaging.
[0043] Example 3
[0044] A method for preparing a low-temperature curing polyamic acid for power semiconductor packaging, comprising the following steps: (1) in a high-purity argon gas atmosphere, in a 1000 ml three-necked flask, adding (49.27 g, 0.15 mol) 1,8-bis(p-aminophenoxy)octane and (2.48 g, 0.01 mol) bis(3-aminopropyl)-terminated polydimethylsiloxane (molecular weight 248 g / mol), and using (527.34 g) N-methylpyrrolidone (solid content is 15%) to completely dissolve it; (2) the reaction temperature is 0-5°C, and 41.31 g, 0.16 mol) of di(phthalic anhydride) linked by -OCH2CH2O- is added to the system after step (1) in 7 batches (60%, 30%, 8%, 1%, 0.5%, 0.3%, 0.1%) for copolymerization reaction. The addition interval time is 0.8h and the overall reaction time is 8h to obtain low-temperature curing polyamic acid for power semiconductor packaging.
[0045] Example 4
[0046] A method for preparing a low-temperature curing polyamic acid for power semiconductor packaging comprises the following steps: (1) in a high-purity argon gas atmosphere, in a 1000 ml three-necked flask, adding (57.68 g, 0.15 mol) of 1,12-bis(m-aminophenoxy)dodecane and (2.48 g, 0.01 mol) of bis(3-aminopropyl)-terminated polydimethylsiloxane (molecular weight 248 g / mol), and using (575.00 g) of N-methylpyrrolidine Ketone (solid content of 15%) is added to completely dissolve it; (2) the reaction temperature is 0-5°C, and 41.31 g, 0.16 mol) of di(phthalic anhydride) linked by -OCH2CH2O- is added to the system after step (1) in 7 batches (60%, 30%, 8%, 1%, 0.5%, 0.3%, 0.1%) for copolymerization reaction. The addition interval time is 0.8 h, and the overall reaction time is 8 h to obtain low-temperature curing polyamic acid for power semiconductor packaging.
[0047] Example 5
[0048] A method for preparing a polyamic acid for low temperature curing power semiconductor packaging comprises the following steps: (1) in a high purity argon gas atmosphere, in a 1000 ml three-necked flask, adding (57.68 g, 0.15 mol) of 1,12-bis(m-aminophenoxy)dodecane and (2.48 g, 0.01 mol) of bis(3-aminopropyl)-terminated polydimethylsiloxane (molecular weight 248 g / mol), and using (526.49 g) of N-methylpyrrolidone ( Solid content is 18%) to make it completely dissolved; (2) the reaction temperature is 0-5°C, and 7 batches (60%, 30%, 8%, 1%, 0.5%, 0.3%, 0.1%) of bis(phthalic anhydride) linked by -(OCH2CH2O)3- are added to the system after step (1) to carry out copolymerization reaction. The addition interval time is 0.8h and the overall reaction time is 8h to obtain low-temperature curing polyamic acid for power semiconductor packaging.
[0049] Example 6
[0050] A method for preparing a polyamic acid for low temperature curing power semiconductor packaging comprises the following steps: (1) in a 2000 ml three-necked flask under a high purity argon gas atmosphere, adding (69.22 g, 0.18 mol) of 1,12-bis(m-aminophenoxy)dodecane and (2.48 g, 0.01 mol) of bis(3-aminopropyl)-terminated polydimethylsiloxane (molecular weight 248 g / mol), and using (650.40 g) of N-methylpyrrolidone ( (2) adding (90.90 g, 0.19 mol) of di(phthalic anhydride) linked by -(OCH2CH2O)6- to the system after step (1) in 7 batches (60%, 30%, 8%, 1%, 0.5%, 0.3%, 0.1%) at a reaction temperature of 0-5°C for copolymerization, with a feed interval of 0.8 h and a total reaction time of 8 h to obtain a low-temperature curing polyamic acid for power semiconductor packaging.
[0051] Example 7
[0052] A method for preparing a low-temperature curing polyamic acid for power semiconductor packaging, comprising the following steps: (1) in a high-purity argon gas atmosphere, in a 2000 ml three-necked flask, adding (73.07 g, 0.19 mol) of 1,12-bis(m-aminophenoxy)dodecane and (10 g, 0.01 mol) of bis(3-aminopropyl)-terminated polydimethylsiloxane (average molecular weight of 1000 g / mol), and using (715.04 g) of N-methylpyrrolidone (solid content is 20%) to completely dissolve it; (2) the reaction temperature is 0-5°C, and 7 batches (60%, 30%, 8%, 1%, 0.5%, 0.3%, 0.1%) of di(phthalic anhydride) linked by -(OCH2CH2O)6- are added to the system after step (1) to carry out copolymerization reaction. The addition interval time is 0.8h and the overall reaction time is 8h to obtain low-temperature curing polyamic acid for power semiconductor packaging.
[0053] Example 8
[0054] A method for preparing a polyamic acid for low temperature curing power semiconductor packaging comprises the following steps: (1) in a high purity argon gas atmosphere, adding (76.91 g, 0.20 mol) of 1,12-bis(m-aminophenoxy)dodecane and (30 g, 0.01 mol) of bis(3-aminopropyl)-terminated polydimethylsiloxane (average molecular weight 3000 g / mol) into a 2000 ml three-necked flask, and using (829.52 g) of N-methylpyrrolidone ( (2) adding (100.47 g, 0.21 mol) of di(phthalic anhydride) linked by -(OCH2CH2O)6- to the system after step (1) in 7 batches (60%, 30%, 8%, 1%, 0.5%, 0.3%, 0.1%) at a reaction temperature of 0-5°C for copolymerization, with a feed interval of 0.8h and a total reaction time of 8h to obtain a low-temperature curing polyamic acid for power semiconductor packaging.
[0055] Comparative Example 1
[0056] A preparation method of PMDA / ODA polyamic acid resin comprises the following steps:
[0057] (1) Under nitrogen atmosphere, 0.10 mol (20.02 g) of ODA (4,4'-diaminodiphenyl ether) was dissolved in (237.04 g) of N-methylpyrrolidone.
[0058] (2) The reaction temperature was 5° C., and 0.10 mol (21.81 g) of PMDA (pyromellitic dianhydride) was added to the system after step (1) for 8 h to obtain PMDA / ODA polyamic acid.
[0059] Comparative Example 2
[0060] Compared with Example 1, only 0.15 mol of bis(4-aminophenoxy)methane containing a spacer group was replaced by 0.15 mol of p-phenylenediamine.
[0061] Comparative Example 3
[0062] Compared with Example 1, only 0.16 mol of bis(phthalic anhydride) linked by -(OCH2CH2O)3- was replaced by 0.16 mol of pyromellitic dianhydride.
[0063] The viscosity of the polyamic acid for low temperature curing power semiconductor packaging prepared in the above Examples 1-8 and the polyamic acid prepared in Comparative Examples 1-3 was tested, and the test method was tested in accordance with the GB / T 2794-1995 standard, and the results are shown in Table 1. As can be seen from Table 1, the viscosity of the polyamic acid for low temperature curing power semiconductor packaging prepared by the present invention is appropriate, and it has good fluidity. When dispensing and coating on substrate materials such as silicon, aluminum, copper, nickel, ceramics or aluminum nitride, it is not easy to generate bubbles and has good leveling properties.
[0064] Table 1: Polyamic acid viscosity test results
[0065]
[0066] The thermal imidization procedure of the polyamic acid for low temperature curing power semiconductor packaging prepared in the above Examples 1-8 is as follows: Figure 1 As shown, the thermal imidization procedure of PMDA / ODA polyamic acid prepared in Comparative Example 1 is as follows Figure 2 As shown, Figure 3 The infrared curves of the polyamic acid prepared in Comparative Example 1 after thermal imidization are shown in Figure 1. Figure 3 It can be seen that under the conditions of a maximum curing temperature of 220°C and a curing time of 3.5h, the imidization degree of the low-temperature curing polyamic acid for power semiconductor packaging reaches 100%, while the -NHCO- bond still exists in the infrared curve of ordinary polyamic acid, and complete imidization is not achieved.
[0067] The curing parameters of the low-temperature curing polyamic acid for power semiconductor packaging prepared in Examples 1-8 and the polyamic acid prepared in Comparative Examples 1-3 and the relevant performance data of the polyimide materials obtained after curing are shown in Table 2.
[0068] Glass transition temperature (T g ) Tested in accordance with HB 7655-1999 standard.
[0069] The insulation strength is tested according to GB / T 1408.1-2016 standard.
[0070] The bonding strength is tested according to GB / T 5210-2006 standard.
[0071] The cross-cut test is tested in accordance with GB / T9286-2021 standard.
[0072] Table 2: Curing parameters of polyamic acid and related performance data of polyimide materials obtained after curing
[0073]
[0074] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.
Claims
1. A low temperature curing polyamic acid for power semiconductor packaging, characterized in that: The invention is prepared by copolymerizing a diether dianhydride with a polyethylene glycol chain in the middle, an aromatic diamine containing a flexible spacer group and a bis(3-aminopropyl)-terminated polydimethylsiloxane in a polar aprotic solvent. The average molecular weight of the (3-aminopropyl)-terminated polydimethylsiloxane is ≤3000 g / mol. The molar ratio of the total molar amount of the bis(3-aminopropyl)-terminated polydimethylsiloxane and the aromatic diamine containing a flexible spacer group to the diether dianhydride with a polyethylene glycol chain in the middle is 1.00:(0.95-1.00).
2. The low temperature curing polyamic acid for power semiconductor packaging according to claim 1, characterized in that: The molar ratio of the bis(3-aminopropyl)-terminated polydimethylsiloxane to the aromatic diamine containing a flexible spacer group is 1.00:(15.00-20.00).
3. The low temperature curing polyamic acid for power semiconductor packaging according to claim 1, characterized in that: The flexible spacer group in the aromatic diamine is selected from an alkyl group having 1 to 12 carbon atoms.
4. The low temperature curing polyamic acid for power semiconductor packaging according to claim 1, characterized in that: The diether dianhydride with a polyethylene glycol chain in the middle is selected from one or more of bis(phthalic anhydride) linked by -OCH2CH2O-, bis(phthalic anhydride) linked by -(OCH2CH2O)2-, bis(phthalic anhydride) linked by -(OCH2CH2O)3-, bis(phthalic anhydride) linked by -(OCH2CH2O)4-, bis(phthalic anhydride) linked by -(OCH2CH2O)5-, and bis(phthalic anhydride) linked by -(OCH2CH2O)6-.
5. The low temperature curing polyamic acid for power semiconductor packaging according to claim 1, characterized in that: The aromatic diamine containing a flexible spacer group is selected from bis(4-aminophenoxy)methane, 1,2-bis(4-aminophenoxy)ethane, 1,2-bis(3-aminophenoxy)ethane, 1,2-bis(4-aminophenoxy)propane, 1,2-bis(4-aminophenoxy)pentane, 1,2-bis(4-aminophenoxy)octane, 1,3-bis(4-aminophenoxy)propane, 1,3-bis(3-aminophenoxy)propane, 2,2-bis(4-aminophenoxymethylene)propane, 2,2-bis(4-aminophenoxymethylene)pentanepropane, 2,2-diethyl-1,3-bis(4-aminophenoxy)propane, 1,4-bis(p-aminophenoxy)but ...4-aminophenoxy) One or more of 4-bis(m-aminophenoxy)butane, 1,5-bis(p-aminophenoxy)pentane, 1,5-bis(m-aminophenoxy)pentane, 1,6-bis(p-aminophenoxy)hexane, 1,6-bis(m-aminophenoxy)hexane, 1,8-bis(p-aminophenoxy)octane, 1,8-bis(m-aminophenoxy)octane, 1,9-bis(p-aminophenoxy)nonane, 1,9-bis(m-aminophenoxy)nonane, 1,10-bis(p-aminophenoxy)decane, 1,10-bis(m-aminophenoxy)decane, 1,12-bis(p-aminophenoxy)dodecane and 1,12-bis(m-aminophenoxy)dodecane.
6. The low temperature curing polyamic acid for power semiconductor packaging according to claim 1, characterized in that: The bis(3-aminopropyl) terminated polydimethylsiloxane is selected from one or more of the group consisting of an average molecular weight of 248 g / mol, an average molecular weight of 1000 g / mol, an average molecular weight of 2500 g / mol, and an average molecular weight of 3000 g / mol.
7. The low temperature curing polyamic acid for power semiconductor packaging according to claim 1, characterized in that: The maximum curing temperature of the polyamic acid is ≤220° C., the curing time is ≤4 hours, and the imidization degree reaches 100%.
8. The method for preparing the low temperature curing polyamic acid for power semiconductor packaging according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1. In a high-purity inert gas atmosphere, an aromatic diamine containing a flexible spacer group and a bis(3-aminopropyl)-terminated polydimethylsiloxane are dissolved in a polar aprotic solvent; S2. The reaction temperature is 0-5° C., and diether dianhydride with a polyethylene glycol chain in the middle is added to the system of step S1 in batches for copolymerization. The reaction time is 6-8 hours to obtain low-temperature curing polyamic acid for power semiconductor packaging.
9. The method for preparing the low temperature curing polyamic acid for power semiconductor packaging according to claim 7, characterized in that: The polar aprotic solvent is selected from one or more of dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide, and the added amount of the polar aprotic solvent accounts for 70.0-90.0% of the mass of the polyamic acid for low-temperature curing power semiconductor packaging; the total added amount of the aromatic diamine monomer containing a flexible spacer group and the diether dianhydride monomer with a polyethylene glycol chain in the middle accounts for 10.0-30.0% of the mass of the polyamic acid for low-temperature curing power semiconductor packaging.
10. The method for preparing the low temperature curing polyamic acid for power semiconductor packaging according to claim 7, characterized in that: The inert gas is selected from one or more of helium, neon, argon, krypton, xenon, radon, nitrogen and carbon dioxide.
Citation Information
Patent Citations
Flexible chain segment polyether-containing polyimide film material and method for preparing homogeneous film
CN101733027A
Polyimide adhesive for packaging power semiconductor and preparation method of polyimide adhesive
CN116731663A
Polyamide-imide resin adhesive, preparation method thereof and temporary adhesive film for packaging semiconductor element
CN117659932A
Copolymeric coating compositions
EP0015720A1
Low-temperature rapid-curing polyamic acid resin composition
JP2000265056A