Modified polylactic acid, preparation method thereof, plastic base material and plastic product thereof
By introducing epoxy chain extenders and antioxidants into polylactic acid and modifying them using extrusion process, the problem of reduced processing performance caused by modification of polylactic acid's mechanical properties is solved, and the modification is achieved that takes into account both mechanical properties and processing performance. Polylactic acid, with high thermal stability and complete degradability.
Patent Information
- Application Number
- CN202411058249.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-08-03
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-22
AI Technical Summary
Polylactic acid usually leads to a reduction in processing performance during the mechanical properties modification process, which cannot meet the requirements of both excellent mechanical properties and processing performance.
By introducing epoxy chain extenders and antioxidants into polylactic acid, the extrusion process is used to modify, the tensile strength is controlled at 45MPa-100MPa, the melt flow rate is 2g/10min-10g/10min, and the weight average molecular weight is 2g/10min. 100,000-200,000, the polydispersion coefficient is between 1.7-2.2, the elongation rate of break shall not be less than 2%, and the weight loss rate shall not be higher than 0.8% when thermal aging at 200℃-230℃, so as to achieve both mechanical properties and processing Performance modified polylactic acid.
It realizes the low weight loss rate, high thermal stability and high elongation of break in high temperature environments, and has excellent mechanical properties and processing properties, reducing production costs, improving production efficiency, and maintaining complete degradability. .
Smart Images

Figure CN118994598A_ABST
Abstract
Description
[0001] Cross-references
[0002] This application refers to Chinese Patent Application No. 202310972585.2 filed on August 3, 2023, entitled “A modified polylactic acid, its preparation method and its plastic product”, which is incorporated into this application in its entirety by reference. Technical Field
[0003] The invention belongs to the technical field of resin modification, and specifically relates to a modified polylactic acid and a preparation method thereof. Background Art
[0004] Polylactic acid (PLA) is a new type of biodegradable material made from starch raw materials extracted from renewable plant resources (such as corn). It has good biocompatibility and degradability, high strength and good transparency, and therefore has great application potential in the fields of packaging and medicine.
[0005] However, polylactic acid has poor mechanical properties, which greatly limits its application.
[0006] In order to expand the application scope of polylactic acid, it is often modified to improve its mechanical properties. However, the modification of the mechanical properties of polylactic acid often greatly reduces the processing performance of polylactic acid and cannot meet the processing requirements. Summary of the invention
[0007] The present application is made in view of the above-mentioned problems, and its object is to provide a modified polylactic acid having both excellent mechanical properties and processing properties.
[0008] In order to achieve the above object, the first aspect of the present application provides a modified polylactic acid, the tensile strength of the modified polylactic acid is not less than 45MPa, and the melt flow rate of the modified polylactic acid at 180°C-200°C and a load of 2kg-3kg is not less than 2g / 10min. In any embodiment, the tensile strength of the modified polylactic acid is 45MPa-100MPa, and can be optionally 50MPa-60MPa.
[0009] In any embodiment, the melt flow rate of the modified polylactic acid is 2g / 10min-10g / 10min, and can be 2g / 10min-6g / 10min. In any embodiment, the weight average molecular weight of the modified polylactic acid is 100,000-200,000, and can be 100,000-150,000; and / or the polydispersity coefficient of the modified polylactic acid is 1.7-2.2.
[0010] In any embodiment, the weight loss rate of the modified polylactic acid after heat aging in an air environment at 200° C.-230° C. for 4 hours is not higher than 0.8%, and can be optionally 0.1%-0.5%.
[0011] In any embodiment, the elongation at break of the modified polylactic acid is not less than 2%, and can be 2.5%-4%. In any embodiment, the modified polylactic acid comprises a structure shown in Formula I
[0012]
[0013] Wherein, A1 and A2 each independently include carboxyl, hydroxyl, At least one of; R includes R1, R2, R3, R4, R5, and R6 each independently include an organic group, x:y:z is (1-5):(3-7):(5-10), and the structural units are randomly copolymerized.
[0014] In any embodiment, the contact angle of the modified polylactic acid is not less than 63°, and can be selected from 63° to 80°.
[0015] In any embodiment, the modified polylactic acid comprises polylactic acid and a chain extender, wherein the chain extender is an epoxy chain extender, and the infrared spectrum of the chain extender is located at 860 cm -1 -870cm -1 The characteristic peak of epoxy group at 3000cm -1 -3300cm -1 The ratio of the carbon-hydrogen bond stretching vibration peak at is not less than 2.1.
[0016] In any embodiment, based on the total mass of the modified polylactic acid, the mass percentage of the chain extender is 0.1%-2.0%, and optionally 0.4%-1.0%. In any embodiment, the modified polylactic acid consists of polylactic acid and a chain extender.
[0017] In any embodiment, the modified polylactic acid further comprises an antioxidant.
[0018] In any embodiment, the antioxidant includes a primary antioxidant and an auxiliary antioxidant. Optionally, the primary antioxidant includes at least one of a hindered phenol antioxidant and an aromatic amine antioxidant. The hindered phenol antioxidant includes at least one of 2,6-tert-butyl-4-methylphenol, bis(3,5-tert-butyl-4-hydroxyphenyl) sulfide, and pentaerythritol tetrakis[β-(3,5-tert-butyl-4-hydroxyphenyl) propionate. Optionally, the auxiliary antioxidant includes at least one of thiodipropionic acid diester and tris[2.4-di-tert-butylphenyl] phosphite.
[0019] In any embodiment, based on the total mass of the modified polylactic acid, the mass percentage of the antioxidant is 0.1%-1%, and can be optionally 0.1%-0.5%. The second aspect of the present application also provides a method for preparing a modified polylactic acid, the preparation method comprising: blending polylactic acid and a chain extender, and preparing the modified polylactic acid of the first aspect of the present application by an extrusion process.
[0020] In any embodiment, the extrusion process comprises reacting at a temperature not less than 200° C. for not less than 2 minutes.
[0021] In any embodiment, the extrusion process comprises a screw speed of 150 rpm to 170 rpm.
[0022] The third aspect of the present application further provides a plastic substrate, which is prepared by processing the modified polylactic acid of the first aspect of the present application or the modified polylactic acid prepared by the preparation method of the second aspect.
[0023] In any embodiment, the plastic substrate is a nonwoven fabric.
[0024] A fourth aspect of the present application further provides a plastic product, wherein the plastic product is prepared from the plastic substrate of any embodiment.
[0025] In any embodiment, the plastic article is a desiccant package. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is the infrared spectrum of the chain extender used in the examples and comparative examples of the present application. DETAILED DESCRIPTION
[0027] The following detailed description specifically discloses the modified polylactic acid, its preparation method and its plastic product of the present application. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0028] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0029] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0030] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0031] If there is no special description, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps performed sequentially.
[0032] (a) and (b), or may include steps (b) and (a) performed sequentially. For example, the reference that the method may further include step (c) indicates that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0033] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0034] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0035] The first aspect of the present application provides a modified polylactic acid, wherein the tensile strength of the modified polylactic acid is not less than 45 MPa, and the melt flow rate of the modified polylactic acid is not less than 2 g / 10 min at 180° C.-200° C. and a load of 2 kg-3 kg.
[0036] Modified polylactic acid refers to a product obtained by modifying polylactic acid. It can be understood that the modification method of modified polylactic acid can include both physical modification and chemical modification.
[0037] The tensile strength of the modified polylactic acid can be measured by any known method. As an example, the test is performed with reference to the national standard GB 13022-91 "Test method for tensile properties of plastics and films".
[0038] In some embodiments, the tensile strength of the modified polylactic acid can be 43MPa, 44MPa, 45MPa,
[0039] 48 MPa, 50 MPa, 51 MPa, 52 MPa, 53 MPa, 54 MPa, 55 MPa, 56 MPa, 57 MPa, 58 MPa, 59 MPa, 60 MPa, 70 MPa, 80 MPa, 90 MPa, 100 MPa or any value therebetween.
[0040] Melt flow rate, also referred to as melt index, is the number of grams of melt that flows out of a standard capillary tube in a certain time, generally within 10 minutes, in a standardized melt indexer at a certain temperature and pressure. The unit is g / 10min. Melt flow rate is an important indicator for evaluating the processing performance of plastics. Modified polylactic acid has a low melt flow rate, which meets the requirements of the processing technology, can reduce the processing cost of its products, and improve quality stability.
[0041] Resins with a melt flow rate lower than 2g / 10min at 180℃-200℃ and a load of 2kg-3kg are usually difficult to process and need to be processed at extremely high reaction temperatures or reaction pressures. This greatly increases processing costs and reduces quality stability.
[0042] The melt flow rate of the modified polylactic acid can be measured by any known method. As an example, the test is performed with reference to the national standard ISO1133-1:2022 "Plastics. Determination of melt mass flow rate (MFR) and melt volume flow rate (MVR) of thermoplastics. Part 1: Standard method".
[0043] The modified polylactic acid provided in the present application has both excellent mechanical properties and processing properties, and can simultaneously meet the use requirements and processing requirements of the product.
[0044] In some embodiments, the tensile strength of the modified polylactic acid is 45 MPa-100 MPa, and can be optionally 50 MPa-60 MPa.
[0045] In some embodiments, the melt flow rate of the modified polylactic acid is 2 g / 10 min-10 g / 10 min, and can be optionally 2 g / 10 min-6 g / 10 min.
[0046] In some embodiments, the melt flow rate of the modified polylactic acid is 2 g / 10 min, 3 g / 10 min, 4 g / 10 min, 5 g / 10 min, 6 g / 10 min, 7 g / 10 min, 8 g / 10 min, 9 g / 10 min, 10 g / 10 min, or any value therebetween.
[0047] In some embodiments, the weight average molecular weight of the modified polylactic acid is 100,000-200,000, and can be optionally 100,000-150,000.
[0048] In some embodiments, the weight average molecular weight of the modified polylactic acid is 100,000, 110,000, 120,000, 130,000, 140,000, 150,000, 160,000, 170,000, 180,000, 190,000, 200,000 or any value therebetween.
[0049] The weight average molecular weight is a statistical average molecular weight by mass, which is a molecular weight averaged over a unit weight. The weight average molecular weight can be measured by any known method, and can be obtained, for example, by gel permeation chromatography.
[0050] The weight average molecular weight of the modified polylactic acid can effectively extend the chain of polylactic acid within a suitable range without having too much negative impact on its processing performance, so that it can have both excellent mechanical properties and processing properties.
[0051] In some embodiments, the polydispersity coefficient of the modified polylactic acid is 1.7-2.2.
[0052] In some embodiments, the polydispersity coefficient of the modified polylactic acid is 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, or any value therebetween.
[0053] The polydispersity coefficient, also known as the molecular weight distribution coefficient, is defined as the ratio of the weight average molecular weight to the number average molecular weight. The polydispersity coefficient is used to measure the width of the molecular weight distribution.
[0054] In some embodiments, the weight loss rate of the modified polylactic acid after heat aging in an air environment at 200° C.-230° C. for 4 hours is not higher than 0.8%, and can be optionally 0.1%-0.5%.
[0055] The weight loss rate of the modified polylactic acid after heat aging in an air environment at 200°C-230°C for 4 hours can be obtained by testing using a known method. As an example, it can be obtained by testing using the following method: testing the mass M1 of the modified polylactic acid sample, measuring the mass M2 of the modified polylactic acid sample by heat aging the modified polylactic acid sample in an air environment at 200°C-230°C for 4 hours in a thermogravimetric analyzer, and taking (M1-M2) / M1 as the weight loss rate of the modified polylactic acid after heat aging in an air environment at 200°C-230°C for 4 hours.
[0056] In some embodiments, the weight loss rate of the modified polylactic acid after heat aging in an air environment at 200°C-230°C for 4 hours can be selected to be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8% or any numerical range therebetween.
[0057] The modified polylactic acid provided in the embodiments of the present application has low weight loss rate and high thermal stability under high temperature environment.
[0058] In some embodiments, the elongation at break of the modified polylactic acid is not less than 2%, and may be 2.5%-4%.
[0059] In some embodiments, the elongation at break of the modified polylactic acid can be selected to be 2%, 2.2%, 2.5%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% or any value therebetween.
[0060] The modified polylactic acid provided in the embodiment of the present application has high mechanical strength and thermodynamic properties while still maintaining a high elongation at break and having excellent toughness. The modified polylactic acid provided in the present application has a low polydispersity coefficient, indicating that it is uniformly modified and has a high reaction rate, so it can have excellent mechanical properties and processing properties at the same time. In some embodiments, the elongation at break of the modified polylactic acid is 3%-4%.
[0061] The elongation at break of the modified polylactic acid can be selected to be 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% or any value therebetween.
[0062] The modified polylactic acid has a high elongation at break and its toughness is further improved.
[0063] In some embodiments, the modified polylactic acid comprises a structure shown in Formula I
[0064]
[0065] Wherein, A1 and A2 each independently include carboxyl, hydroxyl, At least one of; R includes The chain segments, R1, R2, R3, R4, R5, and R6 each independently include an organic group, x:y:z is (1-5):(3-7):(5-10), and the structural units are randomly copolymerized.
[0066] In some embodiments, the organic group includes at least one of a hydrocarbon group, an ester group, a carboxyl group, an alkoxy group, an aryl group, an amino group, and an amide group.
[0067] In some embodiments, x:y:z is (1-2):(3-4):(5-6).
[0068] In some embodiments, the contact angle of the modified polylactic acid is not less than 63°, and can be selected from 63° to 80°.
[0069] In some embodiments, the contact angle of the modified polylactic acid can be selected to be 63°, 65°, 67°, 69°, 71°, 73°, 75°, 77°, 78°, 80° or any value therebetween.
[0070] There are active groups such as carboxyl and hydroxyl in polylactic acid. The modifier often modifies polylactic acid by reacting with the active groups in polylactic acid. The modified polylactic acid has a high contact angle, indicating that the content of active groups such as carboxyl and hydroxyl in the modified polylactic acid is relatively low, indicating that the modified polylactic acid provided in the present application has a high yield and a large degree of modification.
[0071] In some embodiments, the modified polylactic acid comprises polylactic acid and a chain extender, wherein the chain extender is an epoxy chain extender, and the infrared spectrum of the chain extender is at 860 cm -1 -870cm -1 The characteristic peak of epoxy group at 3000cm -1 -3300cm -1 The ratio of the carbon-hydrogen bond stretching vibration peak at is not less than 2.1.
[0072] The chain extender is used to extend the polylactic acid chain. The chain extender introduces other segments and active functional groups into the polylactic acid molecular chain to increase the molecular weight of polylactic acid, change its structure, and optimize the mechanical properties of polylactic acid. Epoxy chain extender refers to a chain extender that includes epoxy groups. The epoxy groups react with the active functional groups (such as carboxyl and hydroxyl) of polylactic acid to modify polylactic acid.
[0073] In some embodiments, the chain extender includes styrene-co-glycidyl methacrylate.
[0074] In some embodiments, the chain extender structure is as shown in Formula II,
[0075]
[0076] R1, R2, R3, R4, R5, and R6 each independently include an organic group, and x:y:z is (1-5):(3-7):(5-
[0077] 10), random copolymerization of structural units.
[0078] In some embodiments, x:y:z is (1-2):(3-4):(5-6).
[0079] In the infrared spectrum of the chain extender, at 860cm -1 -870cm -1 The characteristic peak of epoxy group at 3000cm -1 -3300cm -1 The ratio of the carbon-hydrogen bond stretching vibration peak at is not less than 2.1, indicating that the chain extender has a high epoxidation degree. The chain extender with high epoxidation degree has many active sites and can greatly improve the mechanical properties of polylactic acid at a low addition amount without bringing too much negative impact on the processing performance of polylactic acid.
[0080] In some embodiments, based on the total mass of the modified polylactic acid, the mass percentage of the chain extender is 0.1%-2.0%, and optionally 0.4%-1.0%.
[0081] In some embodiments, based on the total mass of the modified polylactic acid, the mass percentage of the chain extender is 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0% or any value therebetween.
[0082] The chain extender used in the modified polylactic acid provided in the present application has high reactivity and can effectively improve the mechanical properties of polylactic acid at a low addition amount without bringing too much negative impact on the processing properties of polylactic acid.
[0083] In some embodiments, the modified polylactic acid consists of polylactic acid and a chain extender.
[0084] In the prior art, the improvement of mechanical properties of modified polylactic acid is often achieved at the expense of greatly sacrificing processing properties. Therefore, plasticizers are often added during the modification process to assist in the modification process. However, the addition of plasticizers will reduce production efficiency, increase production costs, and deteriorate degradability. The modified polylactic acid provided in the embodiments of the present disclosure only includes polylactic acid and a chain extender, which achieves a balance between mechanical properties and processing properties of the modified polylactic acid, effectively reducing production costs and improving production efficiency.
[0085] In some embodiments, the modified polylactic acid comprises polylactic acid, a chain extender, and an antioxidant.
[0086] Antioxidants are compounds that can inhibit or delay the thermal oxidation of polymers and other organic compounds in the air. In layman's terms, they are substances that can prevent polymer materials from deteriorating due to oxidation.
[0087] The thermal oxidation process of polylactic acid refers to the process in which the chemical bonds of polylactic acid break and active free radicals and hydroperoxides are generated under the action of heat, light or oxygen. Hydroperoxides undergo decomposition reactions and can also generate hydrocarbon oxygen free radicals and hydroxyl free radicals. These free radicals can trigger a series of free radical chain reactions, resulting in fundamental changes in the structure and properties of organic compounds. Antioxidants can eliminate newly generated free radicals in a timely manner, or promote the decomposition of hydroperoxides to prevent the chain reaction from proceeding.
[0088] Antioxidants are one of the common means to improve the thermal stability of polylactic acid, but a large amount of antioxidants are often required to effectively improve the thermal stability of polylactic acid, and the large amount of antioxidants added will have a negative impact on the mechanical properties and processing properties of polylactic acid. The examples of the present application unexpectedly found that by using an antioxidant and a chain extender together, the thermal stability of polylactic acid can be effectively improved when a small amount of antioxidant is added, while improving the thermal stability of polylactic acid while taking into account the mechanical properties and processing efficiency of polylactic acid.
[0089] In some embodiments, the antioxidant includes a primary antioxidant and a secondary antioxidant.
[0090] Primary antioxidants refer to antioxidants that can eliminate free radicals. As examples, primary antioxidants include but are not limited to aromatic amine compounds and hindered phenol compounds and their derivatives.
[0091] Auxiliary antioxidant refers to an antioxidant capable of decomposing hydroperoxides. In some embodiments, the auxiliary antioxidant includes phosphorus- and sulfur-containing organic compounds. As an example, the auxiliary antioxidant includes but is not limited to thiodipropionic acid diesters and phosphite compounds.
[0092] The primary antioxidant and the auxiliary antioxidant can further significantly improve the thermal stability of the modified polylactic acid through the synergistic effect of the two.
[0093] In some embodiments, the primary antioxidant includes at least one of a hindered phenol antioxidant and an aromatic amine antioxidant, the hindered phenol antioxidant includes at least one of 2,6-tert-butyl-4-methylphenol, bis(3,5-tert-butyl-4-hydroxyphenyl) sulfide, and pentaerythritol tetrakis[β-(3,5-tert-butyl-4-hydroxyphenyl) propionate, and the auxiliary antioxidant includes at least one of thiodipropionic acid diester and tris[2.4-di-tert-butylphenyl] phosphite.
[0094] In some embodiments, the primary antioxidant includes pentaerythritol tetrakis[β-(3,5-tributyl-4-hydroxyphenyl)propionate] (1010), and the secondary antioxidant includes tris[2,4-di-tert-butylphenyl]phosphite (168). In some embodiments, the modified polylactic acid is completely degradable.
[0095] In the prior art, in order to improve the mechanical properties of modified polylactic acid, it is often necessary to blend polylactic acid with other engineering plastics with poor degradability. Although this can improve the mechanical properties of modified polylactic acid, the modified polylactic acid cannot be completely degraded and cannot meet environmental protection requirements, which limits the application of modified polylactic acid. The modified polylactic acid provided in the non-disclosed embodiment has improved mechanical properties while still maintaining complete degradability.
[0096] The second aspect of the present application provides a method for preparing modified polylactic acid, which comprises: blending polylactic acid and a chain extender, and adopting an extrusion process to prepare the modified polylactic acid of the first aspect of the present application.
[0097] In some embodiments, the preparation method comprises: drying the polylactic acid before the extrusion process at a drying temperature of 60°C-80°C.
[0098] In some embodiments, the extrusion process includes reacting at no less than 200° C. for no less than 2 minutes.
[0099] In some embodiments, the extrusion process includes reacting at 200° C. for 2 minutes.
[0100] In some embodiments, the extrusion process includes reacting at 210° C. for 3 minutes.
[0101] Reacting at not less than 200°C for not less than 2 minutes is conducive to the epoxy groups of the chain extender to fully undergo a ring-opening reaction, so as to achieve effective modification of polylactic acid. In some embodiments, the extrusion process includes a screw speed of 150 rpm to 170 rpm.
[0102] In some embodiments, the extrusion screw speed is 150 rpm, 155 rpm, 160 rpm, 165 rpm, 170 rpm, or any value therebetween.
[0103] Controlling the screw speed can control the reaction time in a temperature range of not less than 200° C., thereby ensuring that the ring-opening reaction of the epoxy group proceeds fully.
[0104] In some embodiments, the extrusion temperature is 160°C-180°C in zone 1, 170°C-190°C in zone 2, 170°C-190°C in zone 3, 200-210°C in zone 4, 190°C-200°C in zone 5, 170°C-190°C in zone 6, the die temperature is 170°C-190°C, and the screw speed is 150r / min~170r / min, so that the time for the material to pass through the four zones is at least two minutes.
[0105] In some embodiments, the modified polylactic acid further comprises an antioxidant.
[0106] It is generally believed in the prior art that high processing temperatures easily lead to thermal degradation of polylactic acid, which is not conducive to improving the thermal stability of polylactic acid. Although the mechanism is not clear, the examples of the present application unexpectedly found that the extrusion process includes a reaction at not less than 200°C for not less than 2 minutes, which is conducive to further improving the thermal stability and thermodynamic properties of the modified polylactic acid. It is speculated that this may be related to the primary antioxidant, the auxiliary antioxidant and the chain extender playing a full synergistic role at this temperature. The third aspect of the present application provides a plastic substrate, which includes a modified polylactic acid of any embodiment or a modified polylactic acid prepared by a preparation method of any embodiment.
[0107] In some embodiments, the plastic substrate is a nonwoven fabric.
[0108] Non-woven fabric, also known as non-woven fabric, is made of directional or random fibers. It is breathable, thin, flexible, non-combustible, non-toxic, non-irritating, and inexpensive.
[0109] The non-woven fabric formed from the modified polylactic acid provided in the present application has the characteristics of high mechanical strength, good processing performance, and complete degradation.
[0110] A fourth aspect of the present application provides a plastic product, wherein the plastic product is prepared from the plastic substrate of any embodiment of the present application.
[0111] In some embodiments, the plastic product is a desiccant package.
[0112] It can be understood that the desiccant packaging product includes any form of desiccant packaging product, such as a desiccant bag.
[0113] Desiccant refers to a reagent with a drying effect. In some embodiments, the desiccant includes silica gel, alumina gel, molecular sieve, activated carbon, bone charcoal, charcoal, mineral desiccant, phosphorus pentoxide, anhydrous copper sulfate, lime, soda lime, anhydrous calcium chloride, anhydrous magnesium sulfate.
[0114] In some embodiments, the desiccant comprises a clay-based desiccant. In some embodiments, the clay-based desiccant comprises bentonite. The desiccant has a fast adsorption speed, a strong adsorption capacity, and can be fully biodegraded.
[0115] The modified polylactic acid provided in the present application has sufficient mechanical strength and processing performance, and can be directly used to prepare desiccant packaging products, without the need to be mixed with non-biodegradable engineering plastics such as polyethylene and polypropylene to improve the mechanical properties of the desiccant packaging products, nor with additives that are difficult to biodegrade to improve processing performance. Therefore, the prepared desiccant packaging products have both good mechanical properties and biodegradability.
[0116] Example
[0117] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0118] 1. Preparation method:
[0119] Example 1
[0120] Polylactic acid L130, styrene-methacrylate glycidyl copolymer chain extender (BASF ADR-4468), and antioxidant 1010 (RIANOX 1010 from Rianlon, with a chemical composition of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) were added into a twin-screw extruder at a mass ratio of 99.1:0.6:0.3, and melt-blended, extruded and granulated by the twin-screw extruder to obtain modified polylactic acid.
[0121] The temperature of the twin-screw extruder is 175°C in zone 1, 185°C in zone 2, 185°C in zone 3, 200°C in zone 4, 195°C in zone 5, 180°C in zone 6, the die temperature is 185°C, the material temperature is 185°C, and the screw speed is 160r / min, so that the time for the material to pass through the four zones is two minutes.
[0122] The chain extender is styrene-glycidyl methacrylate copolymer, and the structural formula of the chain extender is shown in Formula II.
[0123]
[0124] R1, R2, R3, R4, R5, and R6 each independently include an organic group, x:y:z is (1-5):(3-7):(5-10), and the structural units are randomly copolymerized.
[0125] The chain extender is a polycyclic epoxy chain extender. The infrared spectrum of the chain extender is as follows: Figure 1 As shown, the infrared spectrum of the chain extender is located at 860cm -1 -870cm -1 The characteristic peak of epoxy group at 3000cm -1 -3300cm -1 The ratio of the carbon-hydrogen bond stretching vibration peak at is 3.3.
[0126] Example 2
[0127] Polylactic acid L130, styrene-methacrylate glycidyl copolymer chain extender (the same as in Example 1), and antioxidant 168 (RIANOX 168 from Rianlon, with a chemical composition of tris[2.4-di-tert-butylphenyl]phosphite) were added into a twin-screw extruder in a mass ratio of 99.1:0.6:0.3 and a mass ratio of 99.4:0.6, and melt-blended, extruded and granulated by a twin-screw extruder to obtain modified polylactic acid.
[0128] The temperature of the twin-screw extruder is 175°C in zone 1, 185°C in zone 2, 185°C in zone 3, 200°C in zone 4, 195°C in zone 5, 180°C in zone 6, the die temperature is 185°C, the material temperature is 185°C, and the screw speed is 160r / min, so that the time for the material to pass through the four zones is two minutes.
[0129] Example 3
[0130] Polylactic acid L130, styrene-methacrylate glycidyl copolymer chain extender (the same as in Example 1), antioxidant 1010 (the same as in Example 1), and antioxidant 168 (the same as in Example 2) were melt-blended and extruded into granules in a mass ratio of 99.1:0.6:0.2:0.1 through a twin-screw extruder to obtain modified polylactic acid.
[0131] The temperature of the twin-screw extruder is 175°C in zone 1, 185°C in zone 2, 185°C in zone 3, 200°C in zone 4, 195°C in zone 5, 180°C in zone 6, the die temperature is 185°C, the material temperature is 185°C, and the screw speed is 160r / min, so that the time for the material to pass through the four zones is two minutes.
[0132] Example 4
[0133] Polylactic acid L130, styrene-methacrylate glycidyl copolymer chain extender (the same as in Example 1), antioxidant 1010 (the same as in Example 1), and antioxidant 168 (the same as in Example 2) were melt-blended and extruded into granules in a mass ratio of 99.1:0.6:0.1:0.2 through a twin-screw extruder to obtain modified polylactic acid.
[0134] The temperature of the twin-screw extruder is 175°C in zone 1, 185°C in zone 2, 185°C in zone 3, 200°C in zone 4, 195°C in zone 5, 180°C in zone 6, the die temperature is 185°C, the material temperature is 185°C, and the screw speed is 160r / min, so that the time for the material to pass through the four zones is two minutes.
[0135] Example 5
[0136] Take polylactic acid L130, styrene-methacrylate glycidyl copolymer chain extender (the same as in Example 1), antioxidant 1010 (the same as in Example 1), and antioxidant 168 (the same as in Example 2) at a mass ratio of 99.1:0.6:0.1:0.2 and add them into a twin-screw extruder, and melt-blend and extrude granulate through the twin-screw extruder to obtain modified polylactic acid.
[0137] The temperature of the twin-screw extruder is 175°C in zone 1, 185°C in zone 2, 185°C in zone 3, 200°C in zone 4, 195°C in zone 5, and 180°C in zone 6. The head temperature is 185°C, the material temperature is 185°C, and the screw speed is 180r / min, so that the time for the material to pass through the four zones is 1 minute.
[0138] Example 6
[0139] Take polylactic acid L130, styrene-methacrylate glycidyl copolymer chain extender (the same as in Example 1), antioxidant 1010 (the same as in Example 1), and antioxidant 168 (the same as in Example 2) at a mass ratio of 99.1:0.6:0.1:0.2 and add them into a twin-screw extruder, and melt-blend and extrude granulate through the twin-screw extruder to obtain modified polylactic acid.
[0140] The temperature of the twin-screw extruder is 175°C in zone 1, 185°C in zone 2, 185°C in zone 3, 195°C in zone 4, 195°C in zone 5, and 180°C in zone 6. The head temperature is 185°C, the material temperature is 185°C, and the screw speed is 160r / min, so that the time for the material to pass through the four zones is 2 minutes.
[0141] Example 7
[0142] Polylactic acid L130, styrene-methacrylate glycidyl copolymer chain extender (BASF ADR-4468), and antioxidant 1010 (RIANOX 1010 from Rianlon, with a chemical composition of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) were added into a twin-screw extruder at a mass ratio of 99.1:0.6:0.3, and melt-blended, extruded and granulated by the twin-screw extruder to obtain modified polylactic acid.
[0143] The temperature of the twin-screw extruder is 175°C in zone 1, 185°C in zone 2, 185°C in zone 3, 200°C in zone 4, 195°C in zone 5, 180°C in zone 6, the die temperature is 185°C, the material temperature is 185°C, and the screw speed is 160r / min, so that the time for the material to pass through the four zones is two minutes.
[0144] Example 8
[0145] Polylactic acid L130, styrene-methacrylate glycidyl copolymer chain extender (the same as in Example 7), and antioxidant 168 (RIANOX 168 from Rianlon, with a chemical composition of tris[2,4-di-tert-butylphenyl]phosphite) were added to a twin-screw extruder in a mass ratio of 99.1:0.6:0.3, and melt-blended, extruded and granulated by the twin-screw extruder to obtain modified polylactic acid.
[0146] The temperature of the twin-screw extruder is 175°C in zone 1, 185°C in zone 2, 185°C in zone 3, 200°C in zone 4, 195°C in zone 5, 180°C in zone 6, the die temperature is 185°C, the material temperature is 185°C, and the screw speed is 160r / min, so that the time for the material to pass through the four zones is two minutes.
[0147] Example 9
[0148] Polylactic acid L130, styrene-methacrylate glycidyl copolymer chain extender (the same as in Example 7), antioxidant 1010 (the same as in Example 7), and antioxidant 168 (the same as in Example 8) were melt-blended and extruded into granules in a mass ratio of 99.1:0.6:0.2:0.1 through a twin-screw extruder to obtain modified polylactic acid.
[0149] The temperature of the twin-screw extruder is 175°C in zone 1, 185°C in zone 2, 185°C in zone 3, 200°C in zone 4, 195°C in zone 5, 180°C in zone 6, the die temperature is 185°C, the material temperature is 185°C, and the screw speed is 160r / min, so that the time for the material to pass through the four zones is two minutes.
[0150] Example 10
[0151] Polylactic acid L130, styrene-methacrylate glycidyl copolymer chain extender (the same as in Example 7), antioxidant 1010 (the same as in Example 7), and antioxidant 168 (the same as in Example 8) were melt-blended and extruded into granules in a mass ratio of 99.1:0.6:0.1:0.2 through a twin-screw extruder to obtain modified polylactic acid.
[0152] The temperature of the twin-screw extruder is 175°C in zone 1, 185°C in zone 2, 185°C in zone 3, 200°C in zone 4, 195°C in zone 5, 180°C in zone 6, the die temperature is 185°C, the material temperature is 185°C, and the screw speed is 160r / min, so that the time for the material to pass through the four zones is two minutes.
[0153] Embodiment 11
[0154] Take polylactic acid L130, styrene-methacrylate glycidyl copolymer chain extender (the same as Example 7), antioxidant 1010 (the same as Example 7), and antioxidant 168 (the same as Example 8) at a mass ratio of 99.1:0.6:0.1:0.2 and add them into a twin-screw extruder, and melt-blend and extrude granulate through the twin-screw extruder to obtain modified polylactic acid.
[0155] The temperature of the twin-screw extruder is 175°C in zone 1, 185°C in zone 2, 185°C in zone 3, 200°C in zone 4, 195°C in zone 5, and 180°C in zone 6. The head temperature is 185°C, the material temperature is 185°C, and the screw speed is 180r / min, so that the time for the material to pass through the four zones is 1 minute.
[0156] Example 12
[0157] Take polylactic acid L130, styrene-methacrylate glycidyl copolymer chain extender (the same as Example 7), antioxidant 1010 (the same as Example 7), and antioxidant 168 (the same as Example 8) at a mass ratio of 99.1:0.6:0.1:0.2 and add them into a twin-screw extruder, and melt-blend and extrude granulate through the twin-screw extruder to obtain modified polylactic acid.
[0158] The temperature of the twin-screw extruder is 175°C in zone 1, 185°C in zone 2, 185°C in zone 3, 195°C in zone 4, 195°C in zone 5, and 180°C in zone 6. The head temperature is 185°C, the material temperature is 185°C, and the screw speed is 160r / min, so that the time for the material to pass through the four zones is 2 minutes.
[0159] The sample in Comparative Example 1 is prepared from pure polylactic acid, and the preparation process is the same as that in Example 1.
[0160] Comparative Example 2
[0161] Polylactic acid L130 and styrene (St)-methyl methacrylate (MMA)-glycidyl methacrylate chain extender (BASF ADR-4370) were added into a twin-screw extruder at a mass ratio of 99.4:0.6, and melt-blended, extruded and granulated by the twin-screw extruder to obtain modified polylactic acid.
[0162] The temperature of the twin-screw extruder is 180°C in zone 1, 185°C in zone 2, 185°C in zone 3, 200°C in zone 4, 195°C in zone 5, and 180°C in zone 6. The head temperature is 185°C, the material temperature is 185°C, and the screw speed is 160r / min, so that the time for the material to pass through the four zones is 2 minutes.
[0163] In the infrared spectrum of the chain extender, at 860cm -1 -870cm -1 The characteristic peak of epoxy group at 3000cm -1 -3300cm -1 The ratio of the carbon-hydrogen bond stretching vibration peak at is 1.7.
[0164] Comparative Example 3
[0165] Polylactic acid L130, styrene (St)-methyl methacrylate (MMA)-glycidyl methacrylate chain extender (BASF ADR-4370), antioxidant 1010 (the same as in Example 7), and antioxidant 168 (the same as in Example 8) were added into a twin-screw extruder at a mass ratio of 99.1:0.6:0.1:0.2, and melt-blended, extruded and granulated by the twin-screw extruder to obtain modified polylactic acid.
[0166] 2. Test methods
[0167] (1) Tensile strength and elongation at break test methods
[0168] The tensile strength and elongation at break are tested according to the national standard GB 13022-91 “Test method for tensile properties of plastics and films”.
[0169] (2) Melt index test method
[0170] The melt index is tested in accordance with the national standard ISO 1133-1:2022 "Plastics. Determination of melt mass flow rate (MFR) and melt volume flow rate (MVR) of thermoplastics. Part 1: Standard method". The test temperature is 190°C and the test load is 2.16 kg.
[0171] (3) Weight loss rate test method
[0172] The isothermal thermal weight loss rate was tested using a DHG-9075A electric constant temperature blast drying oven. The sample was placed in an electric oven in an air environment to accelerate aging under the action of heat and oxygen. The thermal weight loss rate was tested at 220°C for 4 hours of thermal oxygen aging. The calculation formula is:
[0173] W%=[(Wo-W) / Wo]×100%
[0174] Wherein, W% is the isothermal weight loss rate, Wo is the initial mass of the sample, and W is the residual mass of the sample after thermal oxidation aging at 220°C for 4 h.
[0175] (4) Weight average molecular weight test method
[0176] The weight average molecular weight of the modified polylactic acid was determined by gel permeation chromatography. The test method was to dissolve the sample in chloroform at room temperature and calibrate the molecular weight using a gel permeation chromatograph.
[0177] (5) Contact angle test method
[0178] The static contact angle method was used to measure the contact angle of the modified polylactic acid. The testing instrument was a contact angle meter and the testing standard was ISO 8296.
[0179] (6) Infrared spectrum testing method
[0180] Infrared spectra are used to characterize the functional groups of organic matter. The testing instrument is a Fourier infrared spectrometer and the testing method is a tablet pressing method.
[0181] 3. Performance data
[0182] The test results of the embodiments and comparative examples are shown in Table 1.
[0183] Table 1
[0184]
[0185] From the comparison of the embodiments and the comparative examples, it can be seen that the tensile strength of the modified polylactic acid provided in the present application is not less than 45 MPa, and the melt flow rate of the modified polylactic acid at 180°C-200°C and a load of 2kg-3kg is not less than 2g / 10min.
[0186] From the comparison between Example 2 and Examples 5 and 6, it can be seen that including a reaction at not less than 200° C. for not less than 2 minutes in the extrusion process can further improve the mechanical strength of the modified polylactic acid.
[0187] Table 2
[0188] serial number Chain extender mass content Weight average molecular weight Polydispersity coefficient Example 1 0.40% 107861 2.15 Example 2 0.60% 113782 1.93 Example 3 0.80% 118642 1.85 Example 4 1.0% 125459 1.72 Example 5 0.60% 109321 2.06 Example 6 0.60% 108731 2.11 Comparative Example 1 0 104692 2.3
[0189] Table 3
[0190]
[0191] From the comparison between the examples and the comparative examples in Table 3, it can be seen that the modified polylactic acid provided in the examples of the present application can take into account both mechanical properties and thermal stability.
[0192] From the comparison of Examples 7-10, it can be seen that the inclusion of both the primary antioxidant and the auxiliary antioxidant in the modified polylactic acid can further reduce the thermal weight loss rate of the polylactic acid.
[0193] From the comparison of Examples 10-12, it can be seen that the thermal weight loss rate of polylactic acid can be further reduced by including a reaction at not less than 200° C. for not less than 2 minutes during the extrusion process of the modified polylactic acid.
[0194] From the comparison between Example 11 and Comparative Example 3, it can be seen that the infrared spectrum of the chain extender in the modified polylactic acid is located at 860 cm -1 -870cm -1 The characteristic peak of epoxy group at 3000cm -1 -3300cm -1 The ratio of the carbon-hydrogen bond stretching vibration peaks at is not less than 2.1, which helps to further reduce the thermal weight loss rate of polylactic acid and achieve simultaneous improvement of thermal stability and mechanical properties.
[0195] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A modified polylactic acid, characterized in that: The tensile strength of the modified polylactic acid is not less than 45 MPa, and the melt flow rate of the modified polylactic acid is not less than 2 g / 10 min at 180° C.-200° C. and a load of 2 kg-3 kg.
2. The modified polylactic acid according to claim 1, characterized in that The tensile strength of the modified polylactic acid is 45MPa-100MPa, and can be optionally 50MPa-60MPa.
3. The modified polylactic acid according to claim 1 or 2, characterized in that: The melt flow rate of the modified polylactic acid is 2g / 10min-10g / 10min, and can be optionally 2g / 10min-6g / 10min.
4. The modified polylactic acid according to any one of claims 1 to 3, characterized in that The weight average molecular weight of the modified polylactic acid is 100,000-200,000, and can be 100,000-150,000; and / or The polydispersity coefficient of the modified polylactic acid is 1.7-2.
2.
5. The modified polylactic acid according to any one of claims 1 to 4, characterized in that The weight loss rate of the modified polylactic acid after heat aging for 4 hours in an air environment at 200° C.-230° C. is not higher than 0.8%, and can be optionally 0.1%-0.5%.
6. The modified polylactic acid according to any one of claims 1 to 5, characterized in that The elongation at break of the modified polylactic acid is not less than 2%, and can be selected to be 2.5%-4%.
7. The modified polylactic acid according to any one of claims 1 to 6, characterized in that The modified polylactic acid comprises a structure shown in formula I Wherein, A1 and A2 each independently include carboxyl, hydroxyl, At least one of; R includes R1, R2, R3, R4, R5, and R6 each independently include an organic group, x:y:z is (1-5):(3-7):(5-10), and the structural units are randomly copolymerized.
8. The modified polylactic acid according to any one of claims 1 to 7, characterized in that The contact angle of the modified polylactic acid is not less than 63°, and can be selected to be 63°-80°.
9. The modified polylactic acid according to any one of claims 1 to 8, characterized in that The modified polylactic acid comprises polylactic acid and a chain extender, wherein the chain extender is an epoxy chain extender, and the infrared spectrum of the chain extender is located at 860cm -1 -870cm -1 The characteristic peak of epoxy group at 3000cm -1 -3300cm -1 The ratio of the carbon-hydrogen bond stretching vibration peak at is not less than 2.
1.
10. The modified polylactic acid according to claim 9, characterized in that Based on the total mass of the modified polylactic acid, the mass percentage of the chain extender is 0.1%-2.0%, and can be optionally 0.4%-1.0%.
11. The modified polylactic acid according to any one of claims 1 to 10, characterized in that The modified polylactic acid also includes an antioxidant.
12. The modified polylactic acid according to claim 11, characterized in that The antioxidant includes a primary antioxidant and an auxiliary antioxidant. Optionally, the primary antioxidant includes at least one of a hindered phenol antioxidant and an aromatic amine antioxidant. The hindered phenol antioxidant includes at least one of 2,6-tert-butyl-4-methylphenol, bis(3,5-tert-butyl-4-hydroxyphenyl) sulfide, and pentaerythritol tetrakis[β-(3,5-tert-butyl-4-hydroxyphenyl) propionate. Optionally, the auxiliary antioxidant includes at least one of thiodipropionic acid diester and tris[2.4-di-tert-butylphenyl] phosphite.
13. The modified polylactic acid according to claim 11 or 12, characterized in that: Based on the total mass of the modified polylactic acid, the mass percentage of the antioxidant is 0.1%-1%, and can be optionally 0.1%-0.5%.
14. A method for preparing modified polylactic acid, characterized in that: The preparation method comprises: The polylactic acid is blended with a chain extender and an extrusion process is adopted to prepare the modified polylactic acid according to any one of claims 1 to 13.
15. The preparation method according to claim 14, characterized in that: The extrusion process includes reacting at a temperature not lower than 200° C. for not less than 2 minutes.
16. The preparation method according to claim 14 or 15, characterized in that: The extrusion process includes an extrusion screw speed of 150 to 170 rpm.
17. The preparation method according to any one of claims 14 to 16, characterized in that: The modified polylactic acid also includes an antioxidant.
18. A plastic substrate, characterized in that: The plastic substrate comprises the modified polylactic acid according to any one of claims 1 to 13 or the modified polylactic acid prepared by the preparation method according to any one of claims 14 to 17.
19. The plastic substrate according to claim 18, characterized in that The plastic substrate is non-woven fabric.
20. A plastic product, wherein the plastic product is prepared from the plastic substrate according to claim 18 or 19.
21. The plastic product according to claim 20, characterized in that The plastic product is a desiccant packaging product.