Polyglycolide composition as well as preparation method and application thereof
By in-situ initiating glycolide polymerization with cellulose, a polyglycolic acid composition with a bimodal molecular weight distribution is formed, which solves the problem of low molecular weight of polyglycolic acid and improves its application performance in the field of film products.
Patent Information
- Application Number
- CN202310555623.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-22
AI Technical Summary
The low molecular weight and fast melt flow rate of existing polyethylene glycol (PEG) limit its application in the field of film products, and its tensile strength, impact strength and thermal stability do not meet the requirements of general plastic products.
In situ polymerization of glycolide is initiated by cellulose to increase the molecular weight of polyethylene glycolide and its melt viscosity. A combination of cellulose surface-grafted polyethylene glycolide copolymer and polyethylene glycolide homopolymer is used to form a bimodal molecular weight distribution, thereby improving its processing performance.
It improves the thermal stability and processing window of polyglycolic acid, reduces melt flowability, enhances its applicability in casting and blown film applications, and improves tensile strength and elongation at break.
Smart Images

Figure CN118994608A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polymer materials, and more particularly to a polyglycolide composition and a preparation method and application thereof. Background Art
[0002] Polyglycolide (PGA) is one of the simplest polymers in biodegradable materials, with the characteristics of environmental friendliness and degradability. PGA is a highly crystalline polymer with a high melting point and excellent mechanical properties. However, the polyglycolide prepared by the traditional preparation method has a low molecular weight and a fast melt flow rate during melt processing, which limits its application in the field of membrane products. Cellulose is a natural renewable polymer with both biocompatibility and biodegradability, excellent mechanical properties and low price. Cellulose macromolecules are linked by β-1,4-glycosidic bonds, and contain a large number of hydroxyl groups on the molecular chain (one primary hydroxyl group and two secondary hydroxyl groups on each ring). They have the properties of general alcohol hydroxyl groups and can react with enzymatic and esterification reactions. The activity is stronger in primary hydroxyl groups. Cellulose can be obtained by acid hydrolysis or mechanical methods to obtain cellulose nanocrystals and cellulose nanofibers. Cellulose nanocrystals are a rod-shaped cellulose rod structure with a length of about several hundred nanometers and a diameter of less than one hundred nanometers. Cellulose nanofibers are nanocellulose with a diameter of less than one hundred nanometers, which has a reinforcing effect.
[0003] Chinese invention patent CN111825845A discloses a polylactic acid grafted modified natural fiber and PLA composite material and a preparation method thereof, wherein the method obtains a PLA composite material by performing a click chemical reaction between functional polylactic acid and functional natural fiber. The PLA composite material prepared by this method has better fracture strength, impact strength and heat resistance.
[0004] Chinese invention patent CN111647144A discloses a method for adjusting the molecular chain structure of polyglycolic acid, by adding some functional groups with special performance characteristics (hydrophilic and hydrophobic groups -OH, -COOR, etc.) or chain segments (branching, copolymerization, etc.) to change the molecular structure, thereby changing the original molecular properties of polyglycolic acid (molecular weight, melt index, etc.).
[0005] However, the existing technology does not solve its application in the field of film products. Therefore, it is necessary to study a polyglycolide composition. By grafting and modifying the polyglycolide, its strength can be improved and its melt fluidity can be reduced, thereby improving its processability in applications such as casting and blown film, and it can be applied to film products. Summary of the invention
[0006] In order to solve the technical problems existing in the prior art, the present invention provides a polyglycolide composition and a preparation method and application thereof.
[0007] The present invention aims at the technical problems that the current PGA has low molecular weight, high melt flow rate, tensile strength, impact strength, thermal stability, etc., which do not meet the requirements of general plastic products, and provides a preparation method and application of a polyglycolide composition. By selecting cellulose with high thermal stability, low toxicity, good biocompatibility and other properties to initiate glycolide polymerization in situ, the molecular weight of polyglycolide is increased, its melt viscosity is increased, and its thermal stability is also increased, and its processing window and applicability in high-viscosity fields are broadened, which effectively solves the technical problem, has good technical effects, and can be applied to the modification and processing application production of polyglycolide resin.
[0008] One of the objects of the present invention is to provide a polyglycolide composition.
[0009] The polyglycolide composition comprises a polyglycolide copolymer and a polyglycolide homopolymer grafted onto the surface of cellulose;
[0010] The structural formula of the cellulose surface grafted polyglycolide copolymer is:
[0011]
[0012]
[0013] Wherein, R1, R2, R3, R4, R5, and R6 are independently selected from hydrogen atoms or alkane groups or aromatic hydrocarbon groups with a molecular weight of 15 to 1000 g / mol, and R a , R b are independently selected from a hydrogen atom or Where R x R1, R2, R3, R4, R5 or R6, p is an integer greater than 10, preferably an integer of 200 to 10000; n is greater than 100, preferably 150 to 8000; p1, p2, p3, p4, p5, p6 are independently selected from integers greater than 10, preferably selected from integers of 200 to 10000; wherein the main chain end structure of the cellulose molecule is R1, R2, R3, R4, R5, R6, R a or R b The starch and the polyglycolide side chain of the cellulose-polyglycolide graft copolymer are linked by an ester bond, which is the primary hydroxyl group at the 6th position of the glucose repeating unit. and secondary hydroxyl grafting at positions 2 and 3
[0014] The structural formula of the polyglycolide homopolymer is:
[0015]
[0016] Among them, M1, M2, ..., M iare the same or different and are independently selected from imino, nitro or ether bonds; R is a hydrogen atom (when i=1) or an alkane or aromatic hydrocarbon group with a molecular weight of 15 to 1000 g / mol; n1, n2, ..., n i are all integers not equal to 0, and n1, n2, ..., n i The sum is not less than 50, preferably 50 to 3000; i is an integer of 1 to 20, preferably an integer of 2 to 6, for example 2, 3, 4, 5, 6.
[0017] According to the present invention, the cellulose-polyglycolide graft copolymer is obtained by a surface grafting method of cellulose (such as cellulose nanocrystals, cellulose nanofibers, etc.). For example, the structure of the cellulose-polyglycolide graft copolymer grafted onto the surface of cellulose nanocrystals is shown in the following formula:
[0018]
[0019] The rod-like structure is a cellulose nanocrystal with a length of 10 to 100 nm and a diameter of 1 to 10 nm; a, m, n, x, y, and z are integers, preferably integers greater than 10.
[0020] In a preferred embodiment of the present invention,
[0021] The molecular weight distribution of the polyglycolide composition is a bimodal molecular weight distribution, preferably comprising an ultra-high molecular weight cellulose surface grafted polyglycolide copolymer peak and a polyglycolide homopolymer peak;
[0022] Preferably,
[0023] The weight average molecular weight M of the ultra-high molecular weight cellulose surface grafted polyglycolide copolymer w1 6.0×10 5 ~5.0×10 6 g / mol, preferably 8.0×10 5 ~3.0×10 6 g / mol; the molecular weight distribution index is 1.0 to 2.0, preferably 1.0 to 1.5;
[0024] The weight average molecular weight M of the polyglycolide homopolymer peak w2 6.0×10 4 ~2.0×10 5 g / mol; molecular weight distribution index is 1.2 to 3.0, preferably 1.5 to 2.5;
[0025] The weight average molecular weight M of the polyglycolide composition w At 8.0×10 4 ~2.0×10 6g / mol, preferably 9.0×10 4 ~3.0×10 5 g / mol, and the molecular weight distribution index is 1.5 to 15.0, preferably 1.5 to 3.5.
[0026] In a preferred embodiment of the present invention,
[0027] Taking the total mass of the polyglycolide composition as 100%, the content of the cellulose surface grafted polyglycolide copolymer is 1-50%, preferably 1-20%, and more preferably 4-20%; the content of the polyglycolic acid homopolymer is 50-99%, preferably 80-99%, and more preferably 80-96%.
[0028] In a preferred embodiment of the present invention,
[0029] The melt flow rate of the polyglycolide composition at 230° C. / 2.16 kg is not higher than 20 g / 10 min, preferably 4 to 15 g / 10 min.
[0030] According to the present invention, the elongation at break of the polyglycolide copolymer material is at least 50% higher than that of the polyglycolide homopolymer, and the tensile strength of the polyglycolide copolymer material is at least 5MPa higher than that of the polyglycolide homopolymer.
[0031] In a preferred embodiment of the present invention,
[0032] The polyglycolide composition comprises a polyglycolide chain segment that can be polymerized to obtain The raw materials include monomers, cellulose, and catalysts; preferably, the raw materials also include at least one of a small molecule co-initiator and an antioxidant; wherein the degree of polymerization p includes p1, p2,, p3, p4, p5, p6, n1, n2, ..., n i .
[0033] In a preferred embodiment of the present invention,
[0034] The polyglycolide chain segment can be obtained by polymerization The monomer is at least one of methyl glycolate, glycolic acid, and glycolide;
[0035] The cellulose is at least one of cellulose microcrystals, cellulose microfibers, cellulose nanofibers, cellulose nanocrystals, cellulose nanocrystal spheres, and modified cellulose; the modified cellulose is preferably partially esterified, etherified, hydrolyzed, or oxidatively modified cellulose, with a degree of substitution of 0.1 to 2.5;
[0036] The small molecule co-initiator is a small molecule substance containing hydroxyl or amino groups with a boiling point greater than 160° C., preferably having a molecular weight of no more than 1000 g / mol, more preferably a molecular weight of 60-300 g / mol, and more preferably at least one of ethylene glycol, butanediol, glycerol, serinol, leucinol, pentaerythritol, sorbitol, xylitol, amino acid, phenol, hydroquinone, resorcinol, benzyl alcohol, aniline, benzylamine, and p-phenylenediamine;
[0037] The catalyst is a salt compound of at least one of the metal elements of Group IIA-VA and transition metal elements or an organic guanidine catalyst; preferably, the catalyst is a salt compound of at least one of Sn, Bi, Mg, Al, Ca, Fe, Mn, Ti and Zn, and more preferably a Sn salt, such as stannous octoate;
[0038] The antioxidant is at least one of a hindered phenol antioxidant and a phosphite antioxidant, that is, it can be a hindered phenol antioxidant and a phosphite antioxidant and any combination thereof, including but not limited to 2,6-di-tert-butyl-p-cresol, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 2,2'-methylenebis(6-tert-butyl-4-methylphenol), hexanediol bis[β-(3,5-dibutyl-4-hydroxyphenyl)propionate], tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol (such as BASF's antioxidant 1010), N,N'-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine (such as antioxidant 1024), N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine (such as antioxidant 1098), β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid n-octadecyl ester (such as BASF's antioxidant 1076), 1,3,5-trimethyl-2,4,6-tri(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, triphenyl phosphite, tri(4-nonylphenyl) phosphite, diphenyl isooctyl phosphite, diphenyl isodecyl phosphite, diphenyl di(2-ethylhexyl) phosphite, phenyl diisodecyl phosphite, tri(2-ethylhexyl) phosphite, triisodecyl phosphite, tri(dodecyl) phosphite, pentaerythritol diisodecyl phosphite, tris[2.4-di-tert-butylphenyl] phosphite (such as antioxidant 168), bis(2,4-dicumylphenyl) pentaerythritol diphosphite (such as antioxidant 686) and bis(2,4-di-tert-butylphenyl) propionate] pentaerythritol diphosphite (such as antioxidant 626).
[0039] In a preferred embodiment of the present invention,
[0040] The size of the cellulose is micrometer or nanometer level; preferably,
[0041] The nano-scale cellulose has a length of 50 nm to 100 nm and a diameter of 1 to 10 nm;
[0042] The particle size of the micron-grade cellulose is 20 to 200 μm.
[0043] In a preferred embodiment of the present invention,
[0044] The polyglycolide chain segment can be obtained by polymerization The monomers are 100 parts by mass and include the following raw materials:
[0045]
[0046]
[0047] A second object of the present invention is to provide a method for preparing a polyglycolide composition, comprising:
[0048] The amount includes the polyglycolide chain segment that can be polymerized The monomers and cellulose raw materials are subjected to melt polymerization reaction in the presence of a catalyst, and then cooled to obtain the polyglycolide composition; preferably, the raw materials also include at least one of a small molecule co-initiator and an antioxidant;
[0049] Preferably, the temperature of the melt polymerization is 140 to 250° C., preferably 200 to 240° C.; the reaction time is 0.5 to 60 min, preferably 1 to 20 min, more preferably 2 to 5 min.
[0050] In a preferred embodiment of the present invention,
[0051] The melt polymerization reaction is carried out in a continuous melt mixing device, which is a series combination of one or more of a kettle reactor, a tubular reactor, an internal mixer, a Farrel continuous mixer, a Banbury mixer, a single screw extruder, a multi-screw extruder and a reciprocating single screw extruder, preferably an internal mixer or a twin-screw extruder;
[0052] The melt polymerization reaction is preferably carried out in a continuous twin-screw extruder, more preferably in at least two continuous twin-screw extruders connected in series, such as 2, 3, 4, etc. For example, when the reaction is carried out in multiple continuous twin-screw extruders, the polymerization reaction can be carried out in the first twin-screw extruder, and the volatile components such as unreacted monomers and small molecular products generated by the degradation of the polymer at high temperature are removed in the second (or second + third) twin-screw extruder, and various additives can also be added to the second (or second + third) twin-screw extruder;
[0053] Preferably, the processing conditions of the continuous twin-screw extruder include:
[0054] The processing temperature is 140-250°C, preferably 200-240°C;
[0055] The screw speed is 5 to 300 rpm, preferably 40 to 150 rpm;
[0056] The aspect ratio is 25-80, preferably 25-70.
[0057] The melt polymerization reaction can also be carried out in an internal mixer; preferably, the internal mixer temperature is 180-250°C, preferably 200-230°C, the rotation speed is 5-150 rpm, preferably 20-80 rpm, and the reaction time is 1-20 min, preferably 3-10 min.
[0058] The continuous twin-screw extruder equipment applicable to the present invention includes twin-screw extruders of different designs, such as the HAAKE Eurolab16 desktop parallel co-rotating twin-screw extruder produced by Thermo Fisher in the United States, the ZSK Mcc18 or ZSK 40 co-rotating parallel twin-screw extruders produced by Coperion in Germany, etc. The internal mixer equipment applicable to the present invention includes internal mixers of different designs, such as the PolyLab HAAKE produced by Thermo Fisher in the United States TM Rheomex OS 567-1000 internal mixer module, etc.
[0059] The third object of the present invention is to provide a polyglycolide composition obtained by the above preparation method.
[0060] A fourth object of the present invention is to provide an application of a polyglycolide composition in a composite material, preferably in a composite material plastic product, wherein the plastic product is a film, an injection molded product, a blister product or a fiber.
[0061] Compared with the prior art, the present invention has the following advantages:
[0062] The polyglycolide composition prepared by the invention has the characteristics of higher molecular weight and bimodal molecular weight distribution, so that it has both high strength and low melt fluidity, and improves its applicability in applications such as casting and film blowing.
[0063] At the same time, the preparation method of the polyglycolic acid composition of the present invention has high production efficiency, can realize continuous preparation on a twin-screw extruder, greatly reduces the reaction time, significantly reduces energy consumption and carbon emissions, overcomes the defects of high production cost and energy consumption caused by the slow polymerization reaction of polyglycolic acid in the prior art, and has extremely high promotion and application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] Figure 1 It is the GPC chart of the polyglycolide composition prepared in Examples 1-2 and Comparative Example 1. DETAILED DESCRIPTION
[0065] The present invention is described in detail below in conjunction with specific drawings and embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.
[0066] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.
[0067] The raw materials used in the present invention are all commercially available;
[0068] Glycolide (GA), purchased from Shenzhen Boli Biomaterials Co., Ltd., purity ≥99.5%;
[0069] Cellulose nanofibers and cellulose microcrystals were purchased from Northern Century (Jiangsu) Cellulose Materials Co., Ltd. with a purity of ≥99.9%;
[0070] Stannous octoate and 1,4-butanediol were purchased from Sinopharm Chemical Reagent Co., Ltd. The purity of stannous octoate was AR grade, and the purity of 1,4-butanediol was CP grade;
[0071] Antioxidant 1010 was purchased from BASF (China) Co., Ltd., and antioxidant 626 (THP-24) was purchased from Shanghai MacLean Biochemical Technology Co., Ltd., with a purity of ≥95%.
[0072] The present invention performs performance measurement according to the following method:
[0073] Gel Permeation Chromatography (GPC): The test instrument was PL-GPC50 gel permeation chromatograph from Angilent, USA, and the processing software was GPC offline. During the test, the mobile phase was hexafluoroisopropanol containing 5mmol / L sodium trifluoroacetate, the flow rate was 1mL / min, the column temperature was 40℃, the injection volume was 100μL, the standard sample was PMMA, and the sample concentration was 1mg / mL.
[0074] Thermogravimetric analysis (TGA): The test was conducted on the Discovery series thermogravimetric analyzer of THERMAL ANALYSIS. Before the test, the machine was turned on and preheated until the temperature of the balance cavity was stable at 40°C. During the test, 5-10 mg of sample was weighed and placed in a ceramic crucible. The test was conducted in an air atmosphere with a flow rate of 20 mL / min. The temperature rise range was 30-600°C and the heating rate was 10°C / min. The weight loss curve of the sample was recorded.
[0075] Melt flow index (MFR): Melt flow index measurement: The test was conducted on a CEAST MF20 melt flow rate tester from Instron, USA. The test temperature was 230°C, the load weight was 2.16 kg, and the preheating time was 4 minutes.
[0076] Injection molding processing method and tensile test: The samples were injection molded into 5A tensile specimens (thickness: 2 mm) on a HAAKE MiniJet micro-injection molding machine according to GB / T 1040.2-2006. The barrel temperature and mold temperature were 240°C and 50°C, respectively, the injection pressure and time were 400 bar and 5 s, respectively, and the holding pressure and time were 100 bar and 10 s, respectively. Then, the tensile test was carried out on a 3344 material testing machine of Instron Company of the United States, with a tensile rate of 50 mm / min and a clamp spacing of 50 mm.
[0077] [Example 1]
[0078] The above-mentioned glycolide, cellulose nanofibers, 1,4-butanediol, antioxidant 1010, antioxidant 626, and stannous octoate were fully premixed according to the mass ratio of 1000:0.5:0.5:5:5:1, and the polymer was extruded and granulated using a HAAKE EuroLab 16 desktop co-rotating twin-screw extruder (screw diameter 16mm, L / D=25). The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. The calibrated feeder is used to feed the blend into the twin screw at a feed rate of 1000g / hr. The temperatures of sections 2-11 of the extruder are: 140℃, 200℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, and 220℃, respectively, and the screw speed is set at 150rpm. Under the conditions of this embodiment, the residence time of the material in the extruder is about 150 seconds on average, and the reaction time can be considered to be about 150 seconds. The extruder is equipped with a circular die with a diameter of 3 mm. After the spline is extruded from the die and water-cooled, it is cut into cylindrical particles with a length of about 3 mm by a pelletizer, collected, dried and packaged for later use.
[0079] The obtained polyglycolide composition comprises a cellulose surface grafted polyglycolide copolymer and a polyglycolide homopolymer; the structural formula of the cellulose surface grafted polyglycolide copolymer is:
[0080]
[0081] Wherein, R1, R2, R3, R4, R5, and R6 are independently selected from hydrogen atoms or alkane groups or aromatic hydrocarbon groups with a molecular weight of 92 g / mol or less. a , R b are independently selected from a hydrogen atom or Where R x is R1, R2, R3, R4, R5 or R6.
[0082] The structural formula of polyglycolide homopolymer is:
[0083]
[0084] [Example 2]
[0085] The above-mentioned glycolide, cellulose nanofibers, 1,4-butanediol, antioxidant 1010, antioxidant 626, and stannous octoate were fully premixed according to the mass ratio of 1000:0.3:0.5:5:5:1, and the polymer was extruded and granulated using a Labtech parallel co-rotating twin-screw extruder (screw diameter: 20 mm, aspect ratio: 40). The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. The calibrated feeder is used to feed the blend into the twin screw at a feed rate of 1000 g / hr. The temperatures of sections 2-11 of the extruder are 180°C, 200°C, 220°C, 220°C, 220°C, 220°C, 230°C, 235°C and 240°C, respectively, and the screw speed is set at 150 rpm. Under the conditions of this embodiment, the average residence time of the material in the extruder is about 240 seconds, and the reaction time can be considered to be about 240 seconds. The extruder is equipped with a circular die with a diameter of 3 mm. After the spline is extruded from the die and water-cooled, it is cut into cylindrical particles with a length of about 3 mm by a pelletizer, collected, dried and packaged for later use.
[0086] The obtained polyglycolide composition comprises a cellulose surface grafted polyglycolide copolymer and a polyglycolide homopolymer; the structural formulas of the cellulose surface grafted polyglycolide copolymer and the polyglycolide homopolymer are the same as those of Example 1.
[0087] [Example 3]
[0088] The above-mentioned glycolide (GA), cellulose microcrystals, 1,4-butanediol, antioxidant 1010, antioxidant 626, and stannous octoate were fully premixed according to the mass ratio of 1000:0.5:0.5:5:5:1, and the polymer was extruded and granulated using a Labtech parallel co-rotating twin-screw extruder (screw diameter: 20 mm, aspect ratio: 40). The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. The calibrated feeder is used to feed the blend into the twin screw at a feed rate of 1000 g / hr. The temperatures of sections 2-11 of the extruder are 180°C, 200°C, 220°C, 220°C, 220°C, 220°C, 230°C, 235°C and 240°C, respectively, and the screw speed is set at 150 rpm. Under the conditions of this embodiment, the average residence time of the material in the extruder is about 240 seconds, and the reaction time can be considered to be about 240 seconds. The extruder is equipped with a circular die with a diameter of 3 mm. After the spline is extruded from the die and water-cooled, it is cut into cylindrical particles with a length of about 3 mm by a pelletizer, collected, dried and packaged for later use.
[0089] The obtained polyglycolide composition comprises a cellulose surface grafted polyglycolide copolymer and a polyglycolide homopolymer; the structural formulas of the cellulose surface grafted polyglycolide copolymer and the polyglycolide homopolymer are the same as those of Example 1.
[0090] [Example 4]
[0091] The above-mentioned glycolide (GA), cellulose nanofibers, 1,4-butanediol, antioxidant 1010, antioxidant 626, and stannous octoate were fully premixed according to the mass ratio of 1000:2:0.1:15:15:2, and the polymer was extruded and granulated using a Labtech parallel co-rotating twin-screw extruder (screw diameter: 20 mm, aspect ratio: 40). The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. The calibrated feeder is used to feed the blend into the twin screw at a feed rate of 1000 g / hr. The temperatures of sections 2-11 of the extruder are: 160°C, 200°C, 220°C, 220°C, 220°C, 220°C, 220°C, 220°C, 220°C, and 220°C, respectively, and the screw speed is set at 150 rpm. Under the conditions of this embodiment, the average residence time of the material in the extruder is about 240 seconds, and the reaction time can be considered to be about 240 seconds. The extruder is equipped with a circular die with a diameter of 3 mm. After the spline is extruded from the die and water-cooled, it is cut into cylindrical particles with a length of about 3 mm by a pelletizer, collected, dried and packaged for later use.
[0092] The obtained polyglycolide composition comprises a cellulose surface grafted polyglycolide copolymer and a polyglycolide homopolymer; the structural formulas of the cellulose surface grafted polyglycolide copolymer and the polyglycolide homopolymer are the same as those of Example 1.
[0093] [Example 5]
[0094] The above-mentioned glycolide (GA), cellulose nanofibers, 1,4-butanediol, antioxidant 1010, antioxidant 626, and stannous octoate were fully premixed according to the mass ratio of 1000:0.01:2:5:5:0.2, and the polymer was extruded and granulated using a Labtech parallel co-rotating twin-screw extruder (screw diameter: 20 mm, aspect ratio: 40). The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. The calibrated feeder is used to feed the blend into the twin screw at a feed rate of 1000 g / hr. The temperatures of sections 2-11 of the extruder are 160°C, 200°C, 220°C, 220°C, 220°C, 220°C, 220°C, 220°C, 220°C, and 220°C, respectively, and the screw speed is set at 150 rpm. Under the conditions of this embodiment, the average residence time of the material in the extruder is about 240 seconds, and the reaction time can be considered to be about 240 seconds. The extruder is equipped with a circular die with a diameter of 3 mm. After the spline is extruded from the die and water-cooled, it is cut into cylindrical particles with a length of about 3 mm by a pelletizer, collected, dried and packaged for later use.
[0095] [Comparative Example 1]
[0096] The above-mentioned glycolide (GA), 1,4-butanediol, antioxidant 1010, antioxidant 626, and stannous octoate were fully premixed in a mass ratio of 1000:1:5:5:1, and the polymer was extruded and granulated using a Labtech parallel co-rotating twin-screw extruder (screw diameter: 20 mm, aspect ratio: 40). The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. The calibrated feeder is used to feed the blend into the twin screw at a feed rate of 1000 g / hr. The temperatures of sections 2-11 of the extruder are 180°C, 200°C, 220°C, 220°C, 220°C, 220°C, 230°C, 235°C and 240°C, respectively, and the screw speed is set at 150 rpm. Under the conditions of this embodiment, the average residence time of the material in the extruder is about 240 seconds, and the reaction time can be considered to be about 240 seconds. The extruder is equipped with a circular die with a diameter of 3 mm. After the spline is extruded from the die and air-cooled, it is cut into cylindrical particles with a length of about 3 mm by a pelletizer, collected, dried, and packaged for later use.
[0097] The obtained product is a polyglycolide homopolymer.
[0098] [Comparative Example 2]
[0099] Commercially available pure PGA, GMP grade glycolide homopolymer, brand: PURASORB PG S.
[0100] Table 1 shows the molecular weight and molecular weight distribution of the polyglycolide polymers of Examples 1 to 5 and Comparative Examples 1 to 2, the mass ratio of the graft copolymer to the homopolymer, and the degree of polymerization of the graft copolymer. As shown in Table 1, the polyglycolide compositions prepared in Examples 1 to 5 have the characteristics of a relatively high molecular weight and a bimodal molecular weight distribution, and the weight average molecular weight (M w ) is greater than 5×10 5 g / mol.
[0101] Figure 1 The GPC diagram of the polyglycolide composition prepared in Examples 1 to 2 and Comparative Example 1 is shown in FIG. Figure 1 It can be seen that the PGA obtained without adding cellulose has a unimodal molecular weight distribution and a LogMW of less than 5.25, while Examples 1 and 2 have a bimodal molecular weight distribution, with a peak with a LogMW greater than 6.25 (cellulose-polyglycolide graft copolymer) and a peak with a LogMW less than 5.25 (polyglycolide homopolymer), which also proves that the polyglycolide composition has a higher molecular weight and a bimodal molecular weight distribution.
[0102] Table 1 Molecular weight and distribution of polyglycolide polymers in Examples 1 to 5 and Comparative Examples 1 to 2 The mass ratio of graft copolymer to homopolymer and the degree of polymerization of graft copolymer
[0103]
[0104] * Calculated from the integrated area ratio of the GPC curve. (M n is the number average molecular weight, M w is the weight-average molecular weight. The ordinate and abscissa of the GPC curve are related to the mass and molecular weight of the polymer, respectively. Therefore, the corresponding component mass can be obtained by integrating the curve, that is, the ratio of the integral area to the total integral area is the corresponding mass ratio.
[0105] **The degree of polymerization n is the statistical average of the degrees of polymerization p1, p2, p3, p4, p5, and p6, and is calculated by the following formula: 324*10*X / (58*Y), the high molecular weight fraction X% obtained by integrating the GPC curve and the cellulose fraction Y (glycolide is calculated as 1000) at the time of initial feeding.
[0106] Table 2 shows the melt flow rate test results of the polyglycolide compositions of Examples 1 to 2, 4, and Comparative Examples 1 to 2. As can be seen from Table 2, the melt flow rates of Examples 1 to 2, 4 are significantly lower than those of Comparative Examples 1 to 2, proving that the polyglycolide composition prepared by the present invention has a high molecular weight and thus a low melt flow rate, while the melt strength and melt toughness are greatly improved, thereby improving its processability in applications such as casting and blown film, and is beneficial to its application in the fields of casting and blown film processing.
[0107] Table 2 Melt flow rate test results of some embodiments and comparative examples
[0108]
[0109] Table 3 shows the mechanical property test results of Examples 1, 3, and Comparative Examples 1-2. It can be seen from Table 3 that the tensile strength of Example 1, Example 3 and Comparative Example 2 is equivalent, but the elongation at break is significantly improved; compared with Comparative Example 1, the elongation at break and the tensile strength of Examples 1 and 3 are significantly increased, which proves that the mechanical properties of the polyglycolide composition obtained by the present invention are significantly improved compared with the polyglycolide homopolymer.
[0110] Table 3 Mechanical properties test results of some embodiments and comparative examples
[0111]
[0112] Table 4 shows the thermogravimetric analysis test results of Examples 1 to 2, 4 and Comparative Examples 1 to 2. It can be seen from Table 4 that the T d5% Compared with the T of the polyglycolide homopolymer of Comparative Examples 1 to 2 d5% Compared with MgO, the thermal stability is improved to a certain extent.
[0113] Table 4 Thermogravimetric analysis test results of some embodiments and comparative examples
[0114]
[0115] The polyglycolide compositions prepared in Examples 1 to 5 have the characteristics of relatively high molecular weight and bimodal molecular weight distribution, so that they have both high strength and low melt fluidity, thereby improving their applicability in applications such as casting and blown film.
Claims
1. A polyglycolide composition comprising a cellulose surface grafted polyglycolide copolymer and a polyglycolide homopolymer; The structural formula of the cellulose surface grafted polyglycolide copolymer is: in, R1, R2, R3, R4, R5, and R6 are independently selected from hydrogen atoms or alkyl or aromatic hydrocarbon groups with a molecular weight of 15 to 1000 g / mol. a , R b are independently selected from a hydrogen atom or Where R x is R1, R2, R3, R4, R5 or R6, p is an integer greater than 10, preferably an integer from 200 to 10000; n is greater than 100, preferably 150 to 8000; p1, p2, p3, p4, p5, p6 are independently selected from integers greater than 10, preferably from 200 to 10000; The structural formula of the polyglycolide homopolymer is: Among them, M1, M2, ..., M i are the same or different, and are independently selected from imino, nitro or ether bonds, and R is a hydrogen atom or an alkane or aromatic hydrocarbon group with a molecular weight of 15 to 1000 g / mol; n1, n2, ..., n i are all integers not equal to 0, and n1, n2, ..., n i The sum is not less than 50, preferably 50-3000; i is an integer of 1-20, preferably an integer of 2-6.
2. The polyglycolide composition according to claim 1, characterized in that: The molecular weight distribution of the polyglycolide composition is a bimodal molecular weight distribution, preferably comprising an ultra-high molecular weight cellulose surface grafted polyglycolide copolymer peak and a polyglycolide homopolymer peak; Preferably, The weight average molecular weight M of the ultra-high molecular weight cellulose surface grafted polyglycolide copolymer w1 6.0×10 5 ~5.0×10 6 g / mol, preferably 8.0×10 5 ~3.0×10 6 g / mol; a molecular weight distribution index of 1.0 to 2.0, preferably 1.0 to 1.5; and / or, The weight average molecular weight M of the polyglycolide homopolymer peak w2 6.0×10 4 ~2.0×10 5 g / mol; a molecular weight distribution index of 1.2 to 3.0, preferably 1.5 to 2.5; and / or, The weight average molecular weight M of the polyglycolide composition w 8.0×10 4 ~2.0×10 6 g / mol, preferably 9.0×10 4 ~3.0×10 5 g / mol; the molecular weight distribution index is 1.5 to 15.0, preferably 1.5 to 3.
5.
3. The polyglycolide composition according to claim 1, characterized in that: Taking the total mass of the polyglycolide composition as 100%, the content of the cellulose surface grafted polyglycolide copolymer is 1-50%, preferably 1-20%, and more preferably 4-20%; the content of the polyglycolic acid homopolymer is 50-99%, preferably 80-99%, and more preferably 80-96%.
4. The polyglycolide composition according to claim 1, characterized in that: The melt flow rate of the polyglycolide composition at 230° C. / 2.16 kg is not higher than 20 g / 10 min, preferably 4 to 15 g / 10 min.
5. The polyglycolide composition according to claim 1, characterized in that: The polyglycolide composition comprises a polyglycolide chain segment that can be polymerized to obtain The raw materials are prepared from raw materials including monomers, cellulose, and catalysts; preferably, the raw materials also include at least one of a small molecule co-initiator and an antioxidant.
6. The polyglycolide composition according to claim 5, characterized in that: The polyglycolide chain segment can be polymerized The monomer is at least one of methyl glycolate, glycolic acid and glycolide; and / or, The cellulose is at least one of cellulose microcrystals, cellulose microfibers, cellulose nanofibers, cellulose nanocrystals, cellulose nanocrystal spheres, and modified cellulose; the modified cellulose is preferably partially esterified, etherified, hydrolyzed, or oxidized modified cellulose, with a degree of substitution of 0.1 to 2.5; and / or, The small molecule co-initiator is a small molecule substance containing hydroxyl or amino groups with a boiling point greater than 160° C., preferably with a molecular weight of no more than 1000 g / mol, more preferably with a molecular weight of 60 to 300 g / mol, and more preferably at least one of ethylene glycol, butanediol, glycerol, serinol, leucinol, pentaerythritol, sorbitol, xylitol, amino acid, phenol, hydroquinone, resorcinol, benzyl alcohol, aniline, benzylamine, and p-phenylenediamine; and / or, The catalyst is a salt compound of at least one of Group IIA-VA metal elements and transition metal elements or an organic guanidine catalyst; preferably, the catalyst is a salt compound of at least one of Sn, Bi, Mg, Al, Ca, Fe, Mn, Ti and Zn; and / or, The antioxidant is at least one of a hindered phenol antioxidant and a phosphite antioxidant.
7. The polyglycolide composition according to claim 6, characterized in that: The size of the cellulose is micrometer or nanometer level; preferably, The nano-scale cellulose has a length of 50 nm to 100 nm and a diameter of 1 to 10 nm; and / or, The particle size of the micron-grade cellulose is 20 to 200 μm.
8. The polyglycolide composition according to claim 5, characterized in that: The polyglycolide chain segment can be obtained by polymerization The monomers are 100 parts by mass and include the following raw materials:
9. A method for preparing the polyglycolide composition according to any one of claims 1 to 8, comprising: The amount includes the polyglycolide chain segment that can be polymerized The monomers and cellulose raw materials are subjected to melt polymerization reaction in the presence of a catalyst, and then cooled to obtain the polyglycolide composition; preferably, the raw materials also include at least one of a small molecule co-initiator and an antioxidant; Preferably, the temperature of the melt polymerization is 140 to 250° C., preferably 200 to 240° C.; the reaction time is 0.5 to 60 min, preferably 1 to 20 min, more preferably 2 to 5 min.
10. The preparation method according to claim 9, characterized in that: The melt polymerization reaction is carried out in a continuous melt mixing device; the melt polymerization reaction is preferably carried out in a continuous twin-screw extruder, more preferably in at least two continuous twin-screw extruders connected in series; Preferably, the processing conditions of the continuous twin-screw extruder include: The processing temperature is 140 to 250°C, preferably 200 to 240°C; and / or, The screw speed is 5 to 300 rpm, preferably 40 to 150 rpm; and / or, The aspect ratio is 25-80, preferably 25-70.
11. A polyglycolide composition obtained according to the preparation method of claim 9 or 10.
12. Use of the polyglycolide composition according to any one of claims 1 to 8 and 11 in a composite material, preferably in a composite plastic product, wherein the plastic product is a film, an injection molded product, a blister product or a fiber.