Production and manufacturing process of glass fiber reinforced plastic material

By adding carbon fiber, accelerator and carbon powder to the fiberglass material, and using antioxidants and flame retardants, the problems of simple composition and insufficient strength of the existing fiberglass material have been solved, and a significant improvement in strength and service life has been achieved.

CN118994660APending Publication Date: 2024-11-22南京精恒复合材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411139932.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing fiberglass material has simple composition and lacks flame retardant function, and its strength needs to be improved.

Method used

A fiberglass material production and manufacturing process is adopted to improve the strength and service life of the material by adding carbon fiber, accelerator and carbon powder, combining antioxidants and flame retardants. The process includes steps of raw material preparation, treatment, resin impregnation and curing, and the specific steps include stirring, precuring and high temperature curing.

Benefits of technology

The strength and service life of fiberglass are significantly improved. Example 3 is the best example, with a strength increase of 16% and a life increase of 23%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994660A_ABST
    Figure CN118994660A_ABST
Patent Text Reader

Abstract

The invention discloses a production and manufacturing process of a glass fiber reinforced plastic material. The production and manufacturing process comprises the following steps: S1, preparing raw materials; s2, raw material treatment; s3, preparing an additive; s4, resin impregnation; s5, curing is conducted; s6, post-treatment, in the step S1, the following raw materials need to be prepared: glass fibers, carbon fibers, unsaturated polyester, epoxy resin, phenolic resin, a curing agent, a diluent, an accelerant, carbon powder, an antioxidant, a flame retardant and dye, the curing agent is prepared by mixing fatty acid anhydride, aromatic acid anhydride and isopropanolamine according to the ratio of (1-5): (2-4): (1-7), and the diluent is prepared by mixing fatty acid anhydride, aromatic acid anhydride and isopropanolamine according to the ratio of (1-5): (2-4): (1-7). The diluent is prepared by mixing cyclohexane, methyl cyclohexane and butanediol according to a ratio of (1-8): (2-3): (1-5), and the accelerant is prepared by mixing ethanediamine, vinyl amine and methyl cyclohexanedione phenol. According to the invention, the carbon fiber, the accelerant and the carbon powder are added into the glass fiber reinforced plastic in the prior art, so that the strength of the glass fiber reinforced plastic can be greatly improved; by adding the antioxidant and the flame retardant, the service life of the glass fiber reinforced plastic can be greatly prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass fiber reinforced plastics, and in particular to a production process of glass fiber reinforced plastics materials. Background Art

[0002] Glass fiber reinforced plastic (FRP) is also called GFRP, which means fiber reinforced plastic. It generally refers to reinforced plastics that use glass fiber to reinforce unsaturated polyester, epoxy resin and phenolic resin matrix. Glass fiber or its products are used as reinforcement materials. It is called glass fiber reinforced plastic, or fiber reinforced plastic, which is different from tempered glass. The scientific name of FRP is fiber reinforced plastic, commonly known as FRP (Fiber Reinforced Plastics), which is fiber reinforced composite plastic. According to the different fibers used, it can be divided into glass fiber reinforced composite plastic (GFRP), carbon fiber reinforced composite plastic (CFRP), boron fiber reinforced composite plastic, etc. It is a composite material with glass fiber and its products (glass cloth, tape, felt, yarn, etc.) as reinforcing materials and synthetic resin as matrix material. Fiber reinforced composite materials are composed of reinforcing fibers and matrix. The diameter of the fiber (or whisker) is very small, generally less than 10μm, with fewer and smaller defects, and a fracture strain of about 30 thousandths. It is a brittle material that is easily damaged, broken and corroded. Compared with the fiber, the matrix has much lower strength and modulus, but it can withstand large strains, often has viscoelasticity and elastoplasticity, and is a tough material; However, the glass fiber reinforced plastics in the prior art have relatively simple components, lack flame retardant function, and their strength needs to be improved. Therefore, the present invention proposes a glass fiber reinforced plastic material production process to solve the above problems. Summary of the invention

[0003] Based on the technical problems that the background technology has that the glass fiber reinforced plastic has a relatively simple composition, lacks flame retardant function, and the strength needs to be improved, the present invention proposes a glass fiber reinforced plastic material production and manufacturing process.

[0004] A glass fiber reinforced plastic material production process proposed by the present invention comprises the following steps: S1: Raw material preparation; S2: Raw material processing; S3: Additive preparation; S4: resin impregnation; S5: curing; S6: Post-processing.

[0005] Preferably, in the step S1, the following raw materials need to be prepared: glass fiber, carbon fiber, unsaturated polyester, epoxy resin, phenolic resin, curing agent, diluent, accelerator, carbon powder, antioxidant, flame retardant and dye. Carbon fiber refers to high-strength and high-modulus fiber with a carbon content of more than 90%. It has the best high-temperature resistance among all chemical fibers. It is made of acrylic fiber and viscose fiber as raw materials and is made by high-temperature oxidation and carbonization. It is an excellent material for manufacturing high-tech equipment such as aerospace. Glass fiber (Fiberglass) is an inorganic non-metallic material with excellent performance and a wide variety. Its advantages are good insulation, strong heat resistance, good corrosion resistance and high mechanical strength, but its disadvantages are brittleness and poor wear resistance. It is made of six kinds of ores, namely pyrophyllite, quartz sand, limestone, dolomite, calcium borate and magnesium borate, as raw materials through high-temperature melting, wire drawing, winding, weaving and other processes. The diameter of its single filament is from several microns to more than twenty microns, which is equivalent to 1 / 20-1 / 5 of a hair. Each bundle of fiber strands is composed of hundreds or even thousands of single filaments. Glass fiber is commonly used as reinforcing material in composite materials, electrical insulation and thermal insulation materials, circuit substrates and other fields of the national economy.

[0006] Preferably, the curing agent is a mixture of aliphatic anhydride, aromatic anhydride and isopropanolamine, and the ratio is 1-5:2-4:1-7; the diluent is a mixture of cyclohexane, methylcyclohexane and butanediol, and the ratio is 1-8:2-3:1-5; the accelerator is a mixture of ethylenediamine, vinylamine and methylcyclohexanedionephenol, and the ratio is 1-3:2-8:1-5; the antioxidant is a mixture of dithiodiisobutyrate, di-tert-butyl-p-cresol and trimethylolpropane phosphate, and the ratio is 1-4:2-3:1-8; the flame retardant is a mixture of hexabromobiphenyl, hexabromodiphenyl ether and triphenyl phosphate, and the ratio is 1-3:3-8:1-7.

[0007] Preferably, in the step S2, unsaturated polyester, epoxy resin, phenolic resin, carbon powder and dye are added to the inner side of a mixer for heating and stirring, and the parameters of the mixer are 50-80 revolutions per minute, a temperature of 50-60 degrees Celsius, and a stirring time of 10-20 minutes to obtain a resin mixture.

[0008] Preferably, in the step S3, the curing agent, diluent, accelerator, antioxidant and flame retardant are added to the inner side of the mixer for heating and stirring. The parameters of the mixer are 80-120 revolutions per minute, the temperature is 50-60 degrees Celsius, and the stirring time is 20-30 minutes to obtain a modified resin mixture.

[0009] Preferably, in the step S4, the glass fibers and carbon fibers are laid flat in an impregnation mold, and then the modified resin mixture is poured into the mold to complete resin impregnation.

[0010] Preferably, in the step S5, the mold is first pre-cured, and the mold is placed at room temperature for 10-15 minutes to allow the modified resin to cross-link with the glass fiber and carbon fiber, and then the mold is added to a curing machine for fixation, the temperature of which is set at 80-120 degrees Celsius, and cured for 20-120 minutes to obtain fiberglass reinforced plastics.

[0011] Preferably, in step S6, after the fiberglass reinforced plastic is manufactured, the fiberglass reinforced plastic is removed from the mold and cut and polished.

[0012] Beneficial effects of the present invention: The invention can greatly increase the strength of the glass fiber reinforced plastic by adding carbon fiber, accelerator and carbon powder to the glass fiber reinforced plastic in the prior art, and can greatly increase the service life of the glass fiber reinforced plastic by adding antioxidant and flame retardant. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 The working flow chart proposed by the present invention. DETAILED DESCRIPTION

[0014] The present invention will be further explained below in conjunction with specific embodiments.

[0015] Reference Figure 1 , Embodiment 1 In this embodiment, a glass fiber reinforced plastic material production process is proposed, including the following steps: S1: Raw material preparation. The following raw materials need to be prepared: glass fiber, carbon fiber, unsaturated polyester, epoxy resin, phenolic resin, curing agent, diluent, accelerator, carbon powder, antioxidant, flame retardant and dye. It refers to high-strength and high-modulus fiber with a carbon content of more than 90%. It ranks first among all chemical fibers in high temperature resistance. It is made of acrylic and viscose fibers as raw materials and is made by high-temperature oxidation and carbonization. It is an excellent material for manufacturing high-tech equipment such as aerospace. Glass fiber (Fiberglass) is an inorganic non-metallic material with excellent performance and a wide variety. Its advantages are good insulation, strong heat resistance, good corrosion resistance and high mechanical strength, but its disadvantages are brittleness and poor wear resistance. It is made of six kinds of ores, namely pyrophyllite, quartz sand, limestone, dolomite, calcium borate and magnesium borate, as raw materials through high-temperature melting, wire drawing, winding, weaving and other processes. The diameter of its single filament ranges from several microns to more than twenty microns, which is equivalent to 1 / 20-1 / 5 of a hair. Each bundle of fiber strands is composed of hundreds or even thousands of single filaments. Glass fiber is usually used as a reinforcing material in composite materials, electrical insulation materials and thermal insulation materials, circuit substrates and other fields of the national economy. The curing agent is a mixture of aliphatic anhydride, aromatic anhydride and isopropanolamine, and the ratio is 2:3:3. The diluent is a mixture of cyclohexane, methylcyclohexane and butanediol, and the ratio is 1:2:1. The accelerator is a mixture of ethylenediamine, vinylamine and methylcyclohexanedionephenol, and the ratio is 1:2:1. The antioxidant is a mixture of dimercapto diisobutyrate, di-tert-butyl-p-cresol and trimethylolpropane phosphate, and the ratio is 1:2:1. The flame retardant is a mixture of hexabromobiphenyl, hexabromodiphenyl ether and triphenyl phosphate, and the ratio is 1:3:1. S2: raw material processing, adding unsaturated polyester, epoxy resin, phenolic resin, carbon powder and dye into the inner side of the mixer for heating and stirring, the parameters of the mixer are 50 revolutions per minute, the temperature is 50 degrees Celsius, and the stirring time is 10 minutes to obtain a resin mixture; S3: Preparation of additives, adding curing agent, diluent, accelerator, antioxidant and flame retardant into the inner side of the mixer for heating and stirring, the parameters of the mixer are 80 revolutions per minute, the temperature is 50 degrees Celsius, and the stirring time is 20 minutes to obtain a modified resin mixture; S4: Resin impregnation, laying the glass fiber and carbon fiber flat in the impregnation mold, and then pouring the modified resin mixture into the mold to complete the resin impregnation; S5: Curing, first pre-curing the mold, placing the mold at room temperature for 10 minutes to allow the modified resin to cross-link with the glass fiber and carbon fiber, and then adding the mold to a curing machine for fixing, the temperature of which is set at 80 degrees Celsius, and curing for 20 minutes to obtain FRP; S6: Post-processing: After the FRP is made, remove it from the mold and cut and grind it.

[0016] Reference Figure 1 , Embodiment 2 In this embodiment, a glass fiber reinforced plastic material production process is proposed, including the following steps: S1: Raw material preparation. The following raw materials need to be prepared: glass fiber, carbon fiber, unsaturated polyester, epoxy resin, phenolic resin, curing agent, diluent, accelerator, carbon powder, antioxidant, flame retardant and dye. It refers to high-strength and high-modulus fiber with a carbon content of more than 90%. It ranks first among all chemical fibers in high temperature resistance. It is made of acrylic and viscose fibers as raw materials and is made by high-temperature oxidation and carbonization. It is an excellent material for manufacturing high-tech equipment such as aerospace. Glass fiber (Fiberglass) is an inorganic non-metallic material with excellent performance and a wide variety. Its advantages are good insulation, strong heat resistance, good corrosion resistance and high mechanical strength, but its disadvantages are brittleness and poor wear resistance. It is made of six kinds of ores, namely pyrophyllite, quartz sand, limestone, dolomite, calcium borate and magnesium borate, as raw materials through high-temperature melting, wire drawing, winding, weaving and other processes. The diameter of its single filament ranges from several microns to more than twenty microns, which is equivalent to 1 / 20-1 / 5 of a hair. Each bundle of fiber strands is composed of hundreds or even thousands of single filaments. Glass fiber is usually used as a reinforcing material in composite materials, electrical insulation materials and thermal insulation materials, circuit substrates and other fields of the national economy. The curing agent is a mixture of aliphatic anhydride, aromatic anhydride and isopropanolamine, and the ratio is 3:2:5. The diluent is a mixture of cyclohexane, methylcyclohexane and butanediol, and the ratio is 4:3:2. The accelerator is a mixture of ethylenediamine, vinylamine and methylcyclohexanedionephenol, and the ratio is 2:6:3. The antioxidant is a mixture of dithiodiisobutyrate, di-tert-butyl-p-cresol and trimethylolpropane phosphate, and the ratio is 3:2:4. The flame retardant is a mixture of hexabromobiphenyl, hexabromodiphenyl ether and triphenyl phosphate, and the ratio is 2:5:5. S2: raw material processing, adding unsaturated polyester, epoxy resin, phenolic resin, carbon powder and dye into the inner side of the mixer for heating and stirring, the parameters of the mixer are 75 revolutions per minute, the temperature is 55 degrees Celsius, and the stirring time is 15 minutes to obtain a resin mixture; S3: Preparation of additives, adding curing agent, diluent, accelerator, antioxidant and flame retardant into the inner side of the mixer for heating and stirring, the parameters of the mixer are 95 revolutions per minute, the temperature is 56 degrees Celsius, and the stirring time is 28 minutes to obtain a modified resin mixture; S4: Resin impregnation, laying the glass fiber and carbon fiber flat in the impregnation mold, and then pouring the modified resin mixture into the mold to complete the resin impregnation; S5: Curing, first pre-curing the mold, placing the mold at room temperature for 10-15 minutes to allow the modified resin to cross-link with the glass fiber and carbon fiber, and then adding the mold to a curing machine for fixing, the temperature of which is set at 100 degrees Celsius, and curing for 110 minutes to obtain FRP; S6: Post-processing: After the FRP is made, remove it from the mold and cut and grind it.

[0017] Reference Figure 1 , Embodiment 3 In this embodiment, a glass fiber reinforced plastic material production process is proposed, including the following steps: S1: Raw material preparation. The following raw materials need to be prepared: glass fiber, carbon fiber, unsaturated polyester, epoxy resin, phenolic resin, curing agent, diluent, accelerator, carbon powder, antioxidant, flame retardant and dye. It refers to high-strength and high-modulus fiber with a carbon content of more than 90%. It ranks first among all chemical fibers in high temperature resistance. It is made of acrylic and viscose fibers as raw materials and is made by high-temperature oxidation and carbonization. It is an excellent material for manufacturing high-tech equipment such as aerospace. Glass fiber (Fiberglass) is an inorganic non-metallic material with excellent performance and a wide variety. Its advantages are good insulation, strong heat resistance, good corrosion resistance and high mechanical strength, but its disadvantages are brittleness and poor wear resistance. It is made of six kinds of ores, namely pyrophyllite, quartz sand, limestone, dolomite, calcium borate and magnesium borate, as raw materials through high-temperature melting, wire drawing, winding, weaving and other processes. The diameter of its single filament ranges from several microns to more than twenty microns, which is equivalent to 1 / 20-1 / 5 of a hair. , each bundle of fiber strands is composed of hundreds or even thousands of single filaments. Glass fiber is usually used as reinforcing material in composite materials, electrical insulation materials and thermal insulation materials, circuit substrates and other fields of the national economy. The curing agent is a mixture of aliphatic anhydride, aromatic anhydride and isopropanolamine, and the ratio is 2:2:3. The diluent is a mixture of cyclohexane, methylcyclohexane and butanediol, and the ratio is 5:2:2. The accelerator is a mixture of ethylenediamine, vinylamine and methylcyclohexanedionephenol, and the ratio is 2:2-8:1-5. The antioxidant is a mixture of dithiodiisobutyrate, di-tert-butyl-p-cresol and trimethylolpropane phosphate, and the ratio is 3:2:5. The flame retardant is a mixture of hexabromobiphenyl, hexabromodiphenyl ether and triphenyl phosphate, and the ratio is 2:4:2. S2: raw material processing, adding unsaturated polyester, epoxy resin, phenolic resin, carbon powder and dye into the inner side of the mixer for heating and stirring, the parameters of the mixer are 50-80 revolutions per minute, the temperature is 55 degrees Celsius, and the stirring time is 15 minutes to obtain a resin mixture; S3: Preparation of additives, adding curing agent, diluent, accelerator, antioxidant and flame retardant into the inner side of the mixer for heating and stirring, the parameters of the mixer are 90 revolutions per minute, the temperature is 55 degrees Celsius, and the stirring time is 25 minutes to obtain a modified resin mixture; S4: Resin impregnation, laying the glass fiber and carbon fiber flat in the impregnation mold, and then pouring the modified resin mixture into the mold to complete the resin impregnation; S5: Curing, first pre-curing the mold, placing the mold at room temperature for 12 minutes to allow the modified resin to cross-link with the glass fiber and carbon fiber, and then adding the mold to a curing machine for fixing, the temperature of which is set at 90 degrees Celsius, and curing for 50 minutes to obtain FRP; S6: Post-processing: After the FRP is made, remove it from the mold and cut and grind it.

[0018] Reference Figure 1 , Embodiment 4 In this embodiment, a glass fiber reinforced plastic material production process is proposed, including the following steps: S1: Raw material preparation. The following raw materials need to be prepared: glass fiber, carbon fiber, unsaturated polyester, epoxy resin, phenolic resin, curing agent, diluent, accelerator, carbon powder, antioxidant, flame retardant and dye. It refers to high-strength and high-modulus fiber with a carbon content of more than 90%. It ranks first among all chemical fibers in high temperature resistance. It is made of acrylic and viscose fibers as raw materials and is made by high-temperature oxidation and carbonization. It is an excellent material for manufacturing high-tech equipment such as aerospace. Glass fiber (Fiberglass) is an inorganic non-metallic material with excellent performance and a wide variety. Its advantages are good insulation, strong heat resistance, good corrosion resistance and high mechanical strength, but its disadvantages are brittleness and poor wear resistance. It is made of six kinds of ores, namely pyrophyllite, quartz sand, limestone, dolomite, calcium borate and magnesium borate, as raw materials through high-temperature melting, wire drawing, winding, weaving and other processes. The diameter of its single filament ranges from several microns to more than twenty microns, which is equivalent to 1 / 20-1 / 5 of a hair. , each bundle of fiber strands is composed of hundreds or even thousands of single filaments. Glass fiber is usually used as reinforcing material in composite materials, electrical insulation materials and thermal insulation materials, circuit substrates and other fields of the national economy. The curing agent is a mixture of aliphatic anhydride, aromatic anhydride and isopropanolamine, and the ratio is 3:2-4:5. The diluent is a mixture of cyclohexane, methylcyclohexane and butanediol, and the ratio is 4:2:3. The accelerator is a mixture of ethylenediamine, vinylamine and methylcyclohexanedionephenol, and the ratio is 3:5:3. The antioxidant is a mixture of dithiodiisobutyrate, di-tert-butyl-p-cresol and trimethylolpropane phosphate, and the ratio is 2:2:5. The flame retardant is a mixture of hexabromobiphenyl, hexabromodiphenyl ether and triphenyl phosphate, and the ratio is 2:4:5. S2: raw material processing, adding unsaturated polyester, epoxy resin, phenolic resin, carbon powder and dye into the inner side of the mixer for heating and stirring, the parameters of the mixer are 58 revolutions per minute, the temperature is 52 degrees Celsius, and the stirring time is 15 minutes to obtain a resin mixture; S3: Preparation of additives, adding curing agent, diluent, accelerator, antioxidant and flame retardant into the inner side of the mixer for heating and stirring, the parameters of the mixer are 100 revolutions per minute, the temperature is 55 degrees Celsius, and the stirring time is 25 minutes to obtain a modified resin mixture; S4: Resin impregnation, laying the glass fiber and carbon fiber flat in the impregnation mold, and then pouring the modified resin mixture into the mold to complete the resin impregnation; S5: Curing: first pre-curing the mold, placing the mold at room temperature for 12 minutes to allow the modified resin to cross-link with the glass fiber and carbon fiber, and then adding the mold to a curing machine for fixing, with the temperature set at 85 degrees Celsius, and curing for 45 minutes to obtain FRP; S6: Post-processing: After the FRP is made, remove it from the mold and cut and grind it.

[0019] Reference Figure 1 Embodiment 5 In this embodiment, a glass fiber reinforced plastic material production process is proposed, including the following steps: S1: Raw material preparation. The following raw materials need to be prepared: glass fiber, carbon fiber, unsaturated polyester, epoxy resin, phenolic resin, curing agent, diluent, accelerator, carbon powder, antioxidant, flame retardant and dye. It refers to high-strength and high-modulus fiber with a carbon content of more than 90%. It ranks first among all chemical fibers in high temperature resistance. It is made of acrylic and viscose fibers as raw materials and is made by high-temperature oxidation and carbonization. It is an excellent material for manufacturing high-tech equipment such as aerospace. Glass fiber (Fiberglass) is an inorganic non-metallic material with excellent performance and a wide variety. Its advantages are good insulation, strong heat resistance, good corrosion resistance and high mechanical strength, but its disadvantages are brittleness and poor wear resistance. It is made of six kinds of ores, namely pyrophyllite, quartz sand, limestone, dolomite, calcium borate and magnesium borate, as raw materials through high-temperature melting, wire drawing, winding, weaving and other processes. The diameter of its single filament ranges from several microns to more than twenty microns, which is equivalent to 1 / 20-1 / 5 of a hair. Each bundle of fiber strands is composed of hundreds or even thousands of single filaments. Glass fiber is usually used as reinforcing material in composite materials, electrical insulation materials and thermal insulation materials, circuit substrates and other fields of the national economy. The curing agent is a mixture of aliphatic anhydride, aromatic anhydride and isopropanolamine, and the ratio is 5:4:7. The diluent is a mixture of cyclohexane, methylcyclohexane and butanediol, and the ratio is 8:3:5. The accelerator is a mixture of ethylenediamine, vinylamine and methylcyclohexanedionephenol, and the ratio is 3:8:5. The antioxidant is a mixture of dithiodiisobutyrate, di-tert-butyl-p-cresol and trimethylolpropane phosphate, and the ratio is 4:3:8. The flame retardant is a mixture of hexabromobiphenyl, hexabromodiphenyl ether and triphenyl phosphate, and the ratio is 3:8:7. S2: raw material processing, adding unsaturated polyester, epoxy resin, phenolic resin, carbon powder and dye into the inner side of the mixer for heating and stirring, the parameters of the mixer are 80 revolutions per minute, the temperature is 60 degrees Celsius, and the stirring time is 20 minutes to obtain a resin mixture; S3: Preparation of additives, adding curing agent, diluent, accelerator, antioxidant and flame retardant into the inner side of the mixer for heating and stirring, the parameters of the mixer are 80-120 revolutions per minute, the temperature is 60 degrees Celsius, and the stirring time is 30 minutes to obtain a modified resin mixture; S4: Resin impregnation, laying the glass fiber and carbon fiber flat in the impregnation mold, and then pouring the modified resin mixture into the mold to complete the resin impregnation; S5: Curing, first pre-curing the mold, placing the mold at room temperature for 15 minutes to allow the modified resin to cross-link with the glass fiber and carbon fiber, and then adding the mold to a curing machine for fixing, the temperature of which is set at 120 degrees Celsius, and curing for 120 minutes to obtain FRP; S6: Post-processing: After the FRP is made, remove it from the mold and cut and grind it.

[0020] Comparing conventional pre-glass reinforced plastics with the pre-glass reinforced plastics obtained in Examples 1 to 5, the pre-glass reinforced plastics obtained in Examples 1 to 5 are shown in the following table: Example one two three Four five Increased strength 12% 17% 18% 16% 15% Increased lifespan 22% 21% 23% 20% 23% It can be seen from the above table that the production process of the glass fiber reinforced plastic material proposed by the present invention has been significantly improved, and implementation three is the best implementation example.

[0021] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A glass fiber reinforced plastic material production process, characterized in that: The following steps are involved: S1: Raw material preparation; S2: Raw material processing; S3: Additive preparation; S4: resin impregnation; S5: curing; S6: Post-processing.

2. A glass fiber reinforced plastic material production process according to claim 1, characterized in that: In the step S1, the following raw materials need to be prepared: glass fiber, carbon fiber, unsaturated polyester, epoxy resin, phenolic resin, curing agent, diluent, accelerator, carbon powder, antioxidant, flame retardant and dye.

3. A glass fiber reinforced plastic material production process according to claim 2, characterized in that: The curing agent is prepared by mixing aliphatic anhydride, aromatic anhydride and isopropanolamine, and the ratio is 1-5:2-4:1-7; the diluent is prepared by mixing cyclohexane, methylcyclohexane and butanediol, and the ratio is 1-8:2-3:1-5; the accelerator is prepared by mixing ethylenediamine, vinylamine and methylcyclohexanedionephenol, and the ratio is 1-3:2-8:1-5; the antioxidant is prepared by mixing dimercapto diisobutyrate, di-tert-butyl-p-cresol and trimethylolpropane phosphate, and the ratio is 1-4:2-3:1-8; the flame retardant is prepared by mixing hexabromobiphenyl, hexabromodiphenyl ether and triphenyl phosphate, and the ratio is 1-3:3-8:1-7.

4. A glass fiber reinforced plastic material production process according to claim 1, characterized in that: In the step S2, unsaturated polyester, epoxy resin, phenolic resin, carbon powder and dye are added into the inner side of a mixer for heating and stirring. The parameters of the mixer are 50-80 revolutions per minute, a temperature of 50-60 degrees Celsius, and a stirring time of 10-20 minutes to obtain a resin mixture.

5. A glass fiber reinforced plastic material production process according to claim 1, characterized in that: In the step S3, the curing agent, diluent, accelerator, antioxidant and flame retardant are added to the inner side of the mixer for heating and stirring. The parameters of the mixer are 80-120 revolutions per minute, the temperature is 50-60 degrees Celsius, and the stirring time is 20-30 minutes to obtain a modified resin mixture.

6. A glass fiber reinforced plastic material production process according to claim 1, characterized in that: In the step S4, the glass fibers and carbon fibers are laid flat in an impregnation mold, and then the modified resin mixture is poured into the mold to complete resin impregnation.

7. A glass fiber reinforced plastic material production process according to claim 1, characterized in that: In the step S5, the mold is first pre-cured, and the mold is placed at room temperature for 10-15 minutes to allow the modified resin to cross-link with the glass fiber and carbon fiber, and then the mold is added to a curing machine for fixing, the temperature of which is set at 80-120 degrees Celsius, and cured for 20-120 minutes to obtain fiberglass reinforced plastics.

8. A glass fiber reinforced plastic material production process according to claim 1, characterized in that: In step S6, after the glass fiber reinforced plastic is manufactured, the glass fiber reinforced plastic is removed from the mold and cut and polished.