Preparation method of polyimide hybrid membrane with relatively strong adhesive force with inorganic membrane layer
By introducing silane coupling agent and silica sol into the polyimide film, a silicon-based network is solved, and the adhesion and device are significantly improved stability.
Patent Information
- Application Number
- CN202411112540.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
AI Technical Summary
The lack of adhesion between the polyimide film and the inorganic film layer leads to problems such as interlayer peeling, cracking, warping, and curling during application of flexible OLED devices, affecting the stability of the device.
By adopting a preparation method, by reacting diamine monomer and acid anhydride monomer in an aprotic polar solvent, adding silane monomer to form a polyamic acid solution with a silane end cap, and combining it with a silica sol, through rotation Coating and high-temperature cyclization form a silicon-based network, which significantly improves the adhesion between the polyimide film and the inorganic film layer.
It significantly improves the adhesion between the polyimide film and the inorganic film layer, improves the stability of the device, and the surface energy of the silicone segment is lower than that of the imide segment, promotes the penetration of the molecular chain and enhances the thermal pressure. Performance and bonding properties.
Smart Images

Figure CN118994674A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of optoelectronic display, in particular to a method for preparing a polyimide hybrid film having strong adhesion to an inorganic film layer. Background Art
[0002] Polyimide materials are suitable choices for optoelectronic display substrate materials due to their excellent thermal stability, mechanical properties, and insulation properties. They are currently widely used in OLED display devices. However, as an organic material, they have a high water vapor transmission rate (WVTR), which means that moisture will pass through the polymer layer to destroy the TFT characteristics and the stability of the device. Therefore, the flexible PI substrate is composed of two layers of PI film and two layers of inorganic insulation layer. The superposition of inorganic and organic materials ensures the stability of the device. However, in the flexible application process, there are certain requirements for the adhesion between the organic and inorganic layers. Poor adhesion will cause interlayer peeling, cracking, warping, curling, etc. in the device, which directly affects the stability of subsequent devices. Therefore, improving the adhesion between the polyimide film and the inorganic film layer is one of the research focuses.
[0003] Flexible OLED substrate composition diagram, such as Figure 1 As shown, currently, the polyimide substrate for flexible display has no improvement in adhesion performance with the inorganic film layer, and mainly relies on its inherent adhesion caused by residual stress. This adhesion performance will gradually decrease with the development of time, which has certain risks. Summary of the invention
[0004] The purpose of the present invention is to solve the above problems and to design a method for preparing a polyimide hybrid film having strong adhesion to an inorganic film layer.
[0005] To achieve the above object, the technical solution of the present invention is a method for preparing a polyimide hybrid film having strong adhesion to an inorganic film layer, comprising the following steps:
[0006] Step 1: adding a diamine monomer and an acid anhydride monomer into a non-protonic polar solvent, wherein the diamine monomer and the acid anhydride monomer react in a non-equimolar ratio;
[0007] Step 2: Add silane monomer ICTOS or γAPS to a polyamic acid solution having an amino or anhydride reactive group and stir for 4-10 hours until all the active end groups are converted into silane end groups to synthesize a polyamic acid solution capped with a silane end cap;
[0008] Step 3: prepare TMOS or TEOS, water and aprotic polar solvent into a sol according to a volume ratio, and add the polyamic acid solution with silane end capping in step 2;
[0009] Step 4: The silica sol-polyamic acid hybrid obtained in step 3 was plated on the surface of 5×5 cm A SiO2 inorganic film layer of a certain thickness is placed on a glass plate and spin-coated at different speeds according to the viscosity of the solution.
[0010] As a further description of the technical solution, in the step 1, after reacting at -5 to 60° C. for 12 to 24 hours, a polyamic acid solution having segments with amino or anhydride reactive groups is obtained.
[0011] As a further description of the technical solution, in the step three, stirring is performed for 24-48 hours to obtain a silica sol-polyamic acid hybrid; the ratio of TMOS, NMP, and DI water is always fixed at 6.8:4:9.2.
[0012] As a further description of the present technical solution, in the step four, pre-drying is performed in a vacuum oven for 15 minutes, followed by evaporation for 20 minutes at 80°C and 10Pa to evaporate most of the solvent, and then the temperature is raised to 450°C in a nitrogen atmosphere for cyclization. After cooling, the film is peeled off to obtain a polyimide hybrid film with strong adhesion to the inorganic film layer.
[0013] As a further description of the technical solution, in the step 1, the diamine monomer and the anhydride monomer are one or more of the following structures, and the diamine monomer structure is as follows:
[0014]
[0015] The structure of anhydride monomer is as follows:
[0016]
[0017] As a further description of the technical solution, in step 1, the non-protonic polar solvent includes: one of N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; and the solid content of the polymerization is 12wt% to 18wt%.
[0018] As a further description of the technical solution, in the step 2, the molar ratio of the added silane monomer is 102% of the active end groups, so as to ensure that all the active end groups are converted into silane end groups.
[0019] As a further description of the technical solution, in step three, the volume ratio of TMOS or TEOS to the aprotic polar solvent and water is 1.7:1:2.3.
[0020] As a further description of the technical solution, in step 4, the high temperature cyclization procedure is 100°C, 30 min; 100-180°C, 30 min; 180-250°C, 30 min; 250°C, 30 min; 250-450°C, 30 min; 450°C, 30 min.
[0021] The beneficial effect lies in that, under the premise of ensuring that the comprehensive performance of the polyimide film meets the requirements of the display substrate, the adhesion between the polyimide film and the inorganic film layer is improved, and a silicon-based network is formed by introducing a silane coupling agent, wherein the surface energy of the siloxane chain segment is much lower than that of the imide chain segment, and the siloxane chain segment is easier to move and migrate to the film surface during hot pressing, which is beneficial to the penetration of the molecular chain at the bonding interface during thermal curing, thereby significantly improving the bonding performance and enhancing the adhesion to the inorganic film layer (SiOx, SiN and other components), so that the adhesion between the polyimide film and the inorganic film layer is significantly improved, and the stability of the device is ensured. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the composition diagram of the flexible OLED substrate DETAILED DESCRIPTION
[0023] The present invention will be described in detail below. A method for preparing a polyimide hybrid film having strong adhesion to an inorganic film layer comprises the following steps:
[0024] Step 1: adding a diamine monomer and an anhydride monomer to a non-protonic polar solvent, wherein the diamine monomer and the anhydride monomer react in a non-equimolar ratio; in the step 1, after reacting at -5 to 60° C. for 12 to 24 hours, a polyamic acid solution having amino or anhydride active reactive groups in the chain segments is obtained.
[0025] In the step 1, the diamine monomer and the anhydride monomer are one or more of the following structures, and the diamine monomer structure is as follows:
[0026]
[0027] The structure of anhydride monomer is as follows:
[0028]
[0029] In the step 1, the non-protonic polar solvent includes: one of N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; and the solid content of the polymerization is 12wt% to 18wt%.
[0030] Step 2: Add silane monomer ICTOS or γAPS to a polyamic acid solution having an amino or anhydride active reactive group and stir for 4-10 hours until all the active end groups are converted into silane end groups, thereby synthesizing a polyamic acid solution with a silane end cap; in the step 2, the molar ratio of the added silane monomer is 102% of the active end groups, thereby ensuring that all the active end groups are converted into silane end groups.
[0031] Step 3: TMOS or TEOS is prepared into a sol with water and a non-protonic polar solvent according to a volume ratio, and the polyamic acid solution with silane end capping in step 2 is added; in the step 3, stirring is performed for 24-48 hours to obtain a silica sol-polyamic acid hybrid; the ratio of TMOS, NMP and DI water is always fixed at 6.8:4:9.2, and in the step 3, the volume ratio of TMOS or TEOS to the non-protonic polar solvent and water is 1.7:1:2.3.
[0032] Step 4: The silica sol-polyamic acid hybrid obtained in step 3 was plated on the surface of 5×5 cm The invention relates to a method for preparing a polyimide hybrid film having a SiO2 inorganic film layer of a certain thickness, and spin coating at different rotation speeds according to the viscosity of the solution. In the step 4, pre-drying is performed in a vacuum oven for 15 minutes, and then evaporation is performed for 20 minutes at 80°C and 10Pa to evaporate most of the solvent, and then the temperature is gradually increased to 450°C in a nitrogen atmosphere for cyclization. After cooling, the film is peeled off to obtain a polyimide hybrid film with strong adhesion to the inorganic film layer. In the step 4, the high-temperature cyclization procedure is 100°C, 30min; 100-180°C, 30min; 180-250°C, 30min; 250°C, 30min; 250-450°C, 30min; 450°C, 30min.
[0033] The following will describe in detail with reference to the embodiments:
[0034] Example 1
[0035] (1) At room temperature, 0.0405 mol (8.1235 g) of 2-(4-aminophenyl)-5-aminobenzimidazole monomer and 0.0232 mol (5.1989 g) of 4,4'-diaminodiphenyl ether (ODA) were added to 150 ml of N,N-dimethylacetamide solvent and stirred until the monomers were completely dissolved, and then 0.058 mol (12.6412 g) of 1,2,4,5-pyromellitic dianhydride (PMDA) was added and stirred for 12 hours to obtain a polyamic acid solution with an amino end group having a solid content of 15 wt%;
[0036] (2) adding 0.0084 mol (2.115 g) of isocyanatepropyltriethoxysilane (ICTOS) to the polyamic acid solution and stirring at room temperature for 4 h until a silane-terminated polyamic acid solution is obtained;
[0037] (3) Add TMOS sol with a volume ratio of TMOS / DMAc / H2O of 1.7:1:2.3 (v / v / v) to the silane-terminated polyamic acid solution and stir at room temperature for 48 hours until the solution is evenly dispersed.
[0038] (4) Filter the solution and plate it The film was spin-coated on a glass plate with a SiO2 inorganic film layer of 100 μm thickness, pre-dried in a vacuum oven for 15 minutes (80°C, 10 Pa, 20 min) to evaporate most of the solvent, and then the temperature was gradually raised to 420°C in a nitrogen atmosphere for cyclization. After cooling, the film was peeled off to obtain a polyimide hybrid film with strong adhesion to the inorganic film layer, with a thickness of 10 μm.
[0039] Example 2
[0040] (1) At room temperature, 0.022 mol (4.9467 g) of 2-(4-aminophenyl)-5-aminobenzimidazole monomer and 0.0331 mol (6.6253 g) of 4,4'-diaminodiphenyl ether (ODA) were added to 150 ml of N,N-dimethylacetamide solvent and stirred until the monomers were completely dissolved, and then 0.0638 mol (13.231 g) of 1,2,4,5-pyromellitic dianhydride (PMDA) was added and stirred for 12 hours to obtain a polyamic acid solution with an amino end group having a solid content of 15 wt%;
[0041] (2) adding 0.0058 mol (1.283 g) of γ-aminopropyltriethoxysilane (APS) to the polyamic acid solution and stirring at room temperature for 4 h until a silane-terminated polyamic acid solution is obtained;
[0042] (3) adding TMOS sol with a volume ratio of TMOS / DMAc / H2O of 1.7:1:2.3 (v / v / v) to the silane-terminated polyamic acid solution and stirring at room temperature for 48 h until the solution is uniformly dispersed;
[0043] (4) Filter the solution and plate it The film was spin-coated on a glass plate with a SiO2 inorganic film layer of 100 μm thickness, pre-dried in a vacuum oven for 15 minutes (80°C, 10 Pa, 20 min) to evaporate most of the solvent, and then the temperature was gradually raised to 420°C in a nitrogen atmosphere for cyclization. After cooling, the film was peeled off to obtain a polyimide hybrid film with strong adhesion to the inorganic film layer, with a thickness of 10 μm.
[0044] Example 3
[0045] (1) At room temperature, 0.0607 mol (6.5694 g) of p-phenylenediamine (PDA) monomer was added to 150 ml of N-methylpyrrolidone solvent and stirred until the monomer was completely dissolved, and then 0.0573 mol (16.8617 g) of 3,3,4,4-biphenyltetracarboxylic dianhydride (BPDA) was added and stirred for 24 hours to obtain a polyamic acid solution with an amino end group having a solid content of 13 wt%;
[0046] (2) adding 0.0034 mol (0.8506 g) of isocyanatepropyltriethoxysilane (ICTOS) to the polyamic acid solution and stirring at room temperature for 6 h until a silane-terminated polyamic acid solution is obtained;
[0047] (3) adding TMOS sol with a volume ratio of TMOS / DMAc / H2O of 1.7:1:2.3 (v / v / v) to the silane-terminated polyamic acid solution and stirring at room temperature for 48 h until the solution is uniformly dispersed;
[0048] (4) Filter the solution and plate it The film was spin-coated on a glass plate with a SiO2 inorganic film layer of 100 μm thickness, pre-dried in a vacuum oven for 15 minutes (80°C, 10 Pa, 20 min) to evaporate most of the solvent, and then the temperature was raised to 450°C in a nitrogen atmosphere for cyclization. After cooling, the film was peeled off to obtain a polyimide hybrid film with strong adhesion to the inorganic film layer, with a thickness of 10 μm.
[0049] Example 4
[0050] (1) At room temperature, 0.0573 mol (6.1975 g) of p-phenylenediamine (PDA) monomer was added to 150 ml of N-methylpyrrolidone solvent and stirred until the monomer was completely dissolved, and then 0.063 mol (18.548 g) of 3,3,4,4-biphenyltetracarboxylic dianhydride (BPDA) was added and stirred for 24 hours to obtain a polyamic acid solution with an amino end group having a solid content of 13 wt%;
[0051] (2) adding 0.0057 mol (1.2387 g) of γ-aminopropyltriethoxysilane (APS) to the polyamic acid solution and stirring at room temperature for 6 h until a silane-terminated polyamic acid solution is obtained;
[0052] (3) adding TMOS sol with a volume ratio of TMOS / DMAc / H2O of 1.7:1:2.3 (v / v / v) to the silane-terminated polyamic acid solution and stirring at room temperature for 48 h until the solution is uniformly dispersed;
[0053] (4) Filter the solution and plate it The film was spin-coated on a glass plate with a SiO2 inorganic film layer of 100 μm thickness, pre-dried in a vacuum oven for 15 minutes (80°C, 10 Pa, 20 min) to evaporate most of the solvent, and then the temperature was raised to 450°C in a nitrogen atmosphere for cyclization. After cooling, the film was peeled off to obtain a polyimide hybrid film with strong adhesion to the inorganic film layer, with a thickness of 10 μm.
[0054] Comparative Example 1
[0055] (1) At room temperature, 0.0232 mol (5.1988 g) of 2-(4-aminophenyl)-5-aminobenzimidazole monomer and 0.0348 mol (6.963 g) of 4,4'-diaminodiphenyl ether (ODA) were added to 150 ml of N,N-dimethylacetamide solvent and stirred until the monomers were completely dissolved, and then 0.058 mol (13.9053 g) of 1,2,4,5-pyromellitic dianhydride (PMDA) was added and stirred for 12 hours to obtain a polyamic acid solution with an amino end group having a solid content of 15 wt%;
[0056] (2) Filter the solution and plate it The film was spin-coated on a glass plate with a SiO2 inorganic film layer of 100 μm thickness, pre-dried in a vacuum oven for 15 minutes (80°C, 10 Pa, 20 min) to evaporate most of the solvent, and then the temperature was gradually raised to 420°C in a nitrogen atmosphere for cyclization. After cooling, the film was peeled off to obtain a polyimide hybrid film with strong adhesion to the inorganic film layer, with a thickness of 10 μm.
[0057] Comparative Example 2
[0058] (1) At room temperature, 0.0573 mol (6.1975 g) of p-phenylenediamine (PDA) monomer was added to 150 ml of N-methylpyrrolidone solvent and stirred until the monomer was completely dissolved, and then 0.0573 mol (16.8618 g) of 3,3,4,4-biphenyltetracarboxylic dianhydride (BPDA) was added and stirred for 24 hours to obtain a polyamic acid solution with an amino end group having a solid content of 13 wt%;
[0059] (2) Filter the solution and plate it The film was spin-coated on a glass plate with a SiO2 inorganic film layer of 100 μm thickness, pre-dried in a vacuum oven for 15 minutes (80°C, 10 Pa, 20 min) to evaporate most of the solvent, and then the temperature was raised to 450°C in a nitrogen atmosphere for cyclization. After cooling, the film was peeled off to obtain a polyimide hybrid film with strong adhesion to the inorganic film layer, with a thickness of 10 μm.
[0060] In order to determine the adhesive force between the polyimide film and the inorganic film material, the peel strength of the material is measured. The peel strength refers to the force required to peel an adhesive tape of a certain width from the surface of a specific adhered material. It is one of the most important indicators of the tape. Here, this concept is used to evaluate the peel strength of the polyimide film. According to market application standards, the polyimide film and the glass substrate are cut into samples with a width of 25 mm and a length of 200 mm. The peeling angle is 180° and the peeling speed is 100 mm / min during the test. Table 1 is a peel strength table of comparative documents 1-2 and embodiments 1-4.
[0061] Table 1 Peel strength table of comparative documents 1-2 and examples 1-4
[0062] sample Peel strength (N / cm) Comparative Example 1 1 0.4 Comparative Example 2 2 0.3 Example 1 3 2.1 Example 2 4 1.9 Example 3 5 1.5 Example 4 6 1.7
[0063] The present invention improves the adhesion of the polyimide film to the inorganic film layer under the premise of ensuring that the comprehensive performance of the polyimide film meets the requirements of the display substrate. By introducing a silane coupling agent, a silicon-based network is formed, wherein the surface energy of the siloxane chain segment is much lower than that of the imide chain segment, and the siloxane chain segment is easier to move and migrate to the film surface during hot pressing, which is beneficial to the penetration of the molecular chain at the bonding interface during thermal curing, thereby significantly improving the bonding performance and improving the adhesion to the inorganic film layer (components such as SiOx and SiN), so that the adhesion between the polyimide film and the inorganic film layer is significantly improved, and the stability of the device is ensured.
[0064] The above technical solutions only reflect the preferred technical solutions of the technical solutions of the present invention. Some changes that may be made to certain parts thereof by technicians in this technical field all reflect the principles of the present invention and fall within the protection scope of the present invention.
Claims
1. A method for preparing a polyimide hybrid film having strong adhesion to an inorganic film layer, characterized in that: The following steps are involved: Step 1: adding a diamine monomer and an acid anhydride monomer into a non-protonic polar solvent, wherein the diamine monomer and the acid anhydride monomer react in a non-equimolar ratio; Step 2: Add silane monomer ICTOS or γAPS to a polyamic acid solution having an amino or anhydride reactive group and stir for 4-10 hours until all the active end groups are converted into silane end groups to synthesize a polyamic acid solution capped with a silane end cap; Step 3: prepare TMOS or TEOS, water and aprotic polar solvent into a sol according to a volume ratio, and add the polyamic acid solution with silane end capping in step 2; Step 4: The silica sol-polyamic acid hybrid obtained in step 3 was plated on the surface of 5×5 cm A SiO2 inorganic film layer of a certain thickness is placed on a glass plate and spin-coated at different speeds according to the viscosity of the solution.
2. The method for preparing a polyimide hybrid film having strong adhesion to an inorganic film layer according to claim 1, characterized in that: In the step 1, after reacting at -5 to 60° C. for 12 to 24 hours, a polyamic acid solution having amino or anhydride reactive groups in the chain segments is obtained.
3. The method for preparing a polyimide hybrid film having strong adhesion to an inorganic film layer according to claim 1, characterized in that: In the step 3, stirring is performed for 24-48 hours to obtain a silica sol-polyamic acid hybrid; the ratio of TMOS, NMP, and DI water is always fixed at 6.8:4:9.
2.
4. The method for preparing a polyimide hybrid film having strong adhesion to an inorganic film layer according to claim 1, characterized in that: In the step 4, pre-drying is performed in a vacuum oven for 15 minutes, followed by evaporation for 20 minutes at 80°C and 10Pa to evaporate most of the solvent, and then the temperature is raised to 450°C in a nitrogen atmosphere for cyclization. After cooling, the film is peeled off to obtain a polyimide hybrid film with strong adhesion to the inorganic film layer.
5. The method for preparing a polyimide hybrid film having strong adhesion to an inorganic film layer according to claim 1, characterized in that: In the step 1, the diamine monomer and the anhydride monomer are one or more of the following structures, and the structure of the diamine monomer is as follows: The structure of anhydride monomer is as follows:
6. The method for preparing a polyimide hybrid film having strong adhesion to an inorganic film layer according to claim 1, characterized in that: In the step 1, the aprotic polar solvent includes: one of N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; and the solid content of the polymerization is 12wt% to 18wt%.
7. The method for preparing a polyimide hybrid film having strong adhesion to an inorganic film layer according to claim 1, characterized in that: In the step 2, the molar ratio of the added silane monomer is 102% of the active end groups, so as to ensure that all the active end groups are converted into silane end groups.
8. The method for preparing a polyimide hybrid film having strong adhesion to an inorganic film layer according to claim 1, characterized in that: In the step 3, the volume ratio of TMOS or TEOS to the aprotic polar solvent and water is 1.7:1:2.
3.
9. The method for preparing a polyimide hybrid film having strong adhesion to an inorganic film layer according to claim 1, characterized in that: In the step 4, the high temperature cyclization procedure is 100°C, 30 min; 100-180°C, 30 min; 180-250°C, 30 min; 250°C, 30 min; 250-450°C, 30 min; 450°C, 30 min.