Efficient ABS (Acrylonitrile Butadiene Styrene) resin flame retardant and preparation method thereof
Through the formulation of raw materials such as magnesium hydroxide and aluminum hydroxide, high-efficiency ABS resin flame retardant was prepared, which solved the problems of toxic fumes, poor thermal stability and performance influence of existing ABS resin flame retardants, and achieved high flame retardant performance and Low environmental impact effect.
Patent Information
- Application Number
- CN202411394885.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing ABS resin flame retardants have toxic smoke, poor thermal stability, easy migration and impact on material properties, and cannot meet the needs of high flame retardant performance and low environmental impact.
Using raw materials such as magnesium hydroxide, aluminum hydroxide, red phosphorus, melamine polyphosphate, expanded graphite and nano-silica, through reasonable formulation and preparation technology, high-efficiency ABS resin flame retardant is prepared, with small additions and good Flame retardant properties and thermal stability, and suppress the generation of flue gas by phosphorus-containing metal salts.
It significantly improves flame retardant performance and thermal stability, avoids the generation of toxic fumes and corrosive gases, and does not affect the mechanical properties and processing properties of ABS resin.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame retardants, and in particular to a high-efficiency ABS resin flame retardant and a preparation method thereof. Background Art
[0002] ABS (Acrylonitrile Butadiene Styrene) resin refers to acrylonitrile-butadiene-styrene copolymer, which is a thermoplastic polymer material with high strength, good toughness and easy processing. It is used to prepare various parts such as instruments, electrical, electrical appliances, and machinery. ABS resin is an important engineering plastic with good comprehensive properties. However, the flammability of ABS resin limits its application in some fields that require high flame retardant properties. Therefore, the development of efficient ABS resin flame retardants has important practical significance.
[0003] At present, the commonly used flame retardants for ABS resin mainly include halogen flame retardants, phosphorus flame retardants and inorganic flame retardants. Although halogen flame retardants have good flame retardant effects, they will produce a large amount of toxic smoke and corrosive gases during the combustion process, causing serious harm to the environment and human health. Phosphorus flame retardants have good flame retardant effects, but there are problems such as poor thermal stability and easy migration. The flame retardant effect of inorganic flame retardants is relatively poor, and a large amount of addition is required to achieve a good flame retardant effect, which will affect the mechanical properties and processing properties of the material. Summary of the invention
[0004] The purpose of the present invention is to provide a high-efficiency ABS resin flame retardant, which is compounded with multiple raw materials, has a synergistic flame retardant effect, can significantly improve the flame retardant performance and thermal stability of the flame retardant, and the flame retardant is added in a small amount and will not have a significant effect on the mechanical properties and processing properties of the ABS resin. Another purpose of the present invention is to provide a preparation method of a high-efficiency ABS resin flame retardant.
[0005] To achieve the above object, the present invention provides a high-efficiency ABS resin flame retardant, which is composed of the following raw materials in parts by weight: 35-55 parts of a heat stabilizer, 2-10 parts of red phosphorus, 10-15 parts of melamine polyphosphate, 5-10 parts of a lubricant, 1-5 parts of a phosphorus-containing metal salt, 0.1-1 parts of an antimony-based synergist, 3-8 parts of nano-silicon dioxide, 10-15 parts of expanded graphite, 0.1-3 parts of a thermal conductor, and 1-3 parts of a surfactant.
[0006] A high-efficiency ABS resin flame retardant is composed of the following raw materials in parts by weight: 45 parts of a heat stabilizer, 8 parts of red phosphorus, 12 parts of melamine polyphosphate, 8 parts of a lubricant, 5 parts of a phosphorus-containing metal salt, 0.1 parts of an antimony-based synergist, 5 parts of nano-silicon dioxide, 12 parts of expanded graphite, 2 parts of a thermal conductor, and 2 parts of a surfactant.
[0007] Preferably, the heat stabilizer is magnesium hydroxide and aluminum hydroxide, and the mass ratio of magnesium hydroxide to aluminum hydroxide is 1.15-1.34.
[0008] Preferably, the mass ratio of the magnesium hydroxide to the aluminum hydroxide is 1.25.
[0009] Preferably, the lubricant is at least one of pentaerythritol, zinc stearate, barium stearate and polyethylene wax.
[0010] Preferably, the antimony-based synergist is selected from at least one of antimony trioxide and antimony pentoxide.
[0011] Preferably, the surfactant is an organic silane coupling agent or a titanate coupling agent.
[0012] Preferably, the thermal conductor is at least one of thermally conductive graphite, carbon nanotubes, and graphene.
[0013] A method for preparing a high-efficiency ABS resin flame retardant comprises the following steps: Step 1, drying the heat stabilizer, red phosphorus, melamine polyphosphate and nano silicon dioxide at 80-100° C. for 2-4 hours respectively; Step 2, adding the dried heat stabilizer, red phosphorus, melamine polyphosphate, nano silicon dioxide, expanded graphite, thermal conductor, and phosphorus-containing metal salt into a high-speed mixer, and mixing them evenly to obtain a mixed material; Step 3: Add the lubricant, antimony-based synergist and surfactant to the mixed material, and continue mixing for 10-20 minutes to obtain a high-efficiency ABS resin flame retardant.
[0014] Preferably, in step 2, the expanded graphite needs to be expanded at 150-200° C. for 1-2 h before being added to the high-speed mixer.
[0015] The advantages and positive effects of the high-efficiency ABS resin flame retardant and the preparation method thereof described in the present invention are: 1. The high-efficiency ABS resin flame retardant of the present invention uses magnesium hydroxide, aluminum hydroxide, red phosphorus, melamine polyphosphate, expanded graphite and nano-silicon dioxide as main raw materials, and has good flame retardant performance and thermal stability through reasonable formula design and preparation process. The addition of phosphorus-containing metal salts inhibits the smoke of antimony-based synergists, reduces the addition amount of antimony-based synergists, and prevents the flame retardant from generating toxic smoke and corrosive gases during combustion, which is harmless to the environment and human health. At the same time, the addition amount of the flame retardant is small, and will not have a significant effect on the mechanical properties and processing properties of the ABS resin.
[0016] 2. Magnesium hydroxide and aluminum hydroxide have good thermal stability and flame retardant properties. They can absorb a large amount of heat during the combustion process and reduce the surface temperature of the resin. At the same time, the water vapor produced by decomposition can dilute the combustible gas and play a flame retardant role.
[0017] 3. Expanded graphite can expand rapidly at high temperatures to form a heat-insulating layer, preventing the transfer of heat and the entry of oxygen, thereby improving flame retardant properties.
[0018] 4. Melamine polyphosphate can produce non-combustible gases, such as ammonia and nitrogen, during the combustion process, which dilute the combustible gas and reduce the combustion intensity. At the same time, the carbon layer formed can prevent the transfer of heat and the entry of oxygen, playing a flame retardant role.
[0019] 5. Organic silane coupling agent can improve the interfacial compatibility between flame retardants and plastics, improve the dispersibility and stability of flame retardants in plastics, thereby improving the mechanical properties and flame retardant properties of plastics.
[0020] The technical solution of the present invention is further described in detail below through embodiments. DETAILED DESCRIPTION
[0021] The technical solution of the present invention is further illustrated by the following examples.
[0022] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.
[0023] Example 1
[0024] A high-efficiency ABS resin flame retardant is composed of the following raw materials in parts by weight: 45 parts of heat stabilizer, 8 parts of red phosphorus, 12 parts of melamine polyphosphate, 8 parts of lubricant, 5 parts of phosphorus-containing metal salt, 0.1 parts of antimony-based synergist, 5 parts of nano-silicon dioxide, 12 parts of expanded graphite, 2 parts of thermal conductor, and 2 parts of surfactant. The heat stabilizer is magnesium hydroxide and aluminum hydroxide, the mass ratio of magnesium hydroxide to aluminum hydroxide is 1.25, magnesium hydroxide is 25 parts, aluminum hydroxide is 20 parts, and the phosphorus-containing metal salt is calcium phosphate.
[0025] A method for preparing a high-efficiency ABS resin flame retardant comprises the following steps: Step 1, drying magnesium hydroxide, aluminum hydroxide, red phosphorus, melamine polyphosphate and nano silicon dioxide at 90° C. for 3 hours respectively; Step 2, expanding the expanded graphite at 150° C. for 1.5 h; Step 3, adding the dried magnesium hydroxide, aluminum hydroxide, red phosphorus, melamine polyphosphate, nano-silicon dioxide, expanded graphite, graphene, and calcium phosphate into a high-speed mixer, mixing evenly to obtain a mixed material; Step 4: Add pentaerythritol, antimony trioxide and organosilane coupling agent to the mixture, and continue mixing for 15 minutes to obtain a high-efficiency ABS resin flame retardant.
[0026] Example 2
[0027] A high-efficiency ABS resin flame retardant is composed of the following raw materials in parts by weight: 35 parts of heat stabilizer, 6 parts of red phosphorus, 10 parts of melamine polyphosphate, 6 parts of lubricant, 4 parts of phosphorus-containing metal salt, 0.3 parts of antimony-based synergist, 6 parts of nano-silicon dioxide, 10 parts of expanded graphite, 1 part of thermal conductor, and 1 part of surfactant. The heat stabilizer is magnesium hydroxide and aluminum hydroxide, the mass ratio of magnesium hydroxide to aluminum hydroxide is 1.33, magnesium hydroxide is 20 parts, and aluminum hydroxide is 15 parts.
[0028] A method for preparing a high-efficiency ABS resin flame retardant comprises the following steps: Step 1, drying magnesium hydroxide, aluminum hydroxide, red phosphorus, melamine polyphosphate and nano silicon dioxide at 80° C. for 3 hours respectively; Step 2, expansing the expanded graphite at 160° C. for 1 h; Step 3, adding the dried magnesium hydroxide, aluminum hydroxide, red phosphorus, melamine polyphosphate, nano silicon dioxide, expanded graphite, thermal conductive graphite, and calcium hydrogen phosphate into a high-speed mixer, and mixing them evenly to obtain a mixed material; Step 4: Add zinc stearate, antimony trioxide and titanate coupling agent to the mixture, and continue mixing for 18 minutes to obtain a high-efficiency ABS resin flame retardant.
[0029] Example 3
[0030] A highly efficient ABS resin flame retardant is composed of the following raw materials in parts by weight: 55 parts of heat stabilizer, 10 parts of red phosphorus, 13 parts of melamine polyphosphate, 8 parts of lubricant, 3 parts of phosphorus-containing metal salt, 0.5 parts of antimony-based synergist, 8 parts of nano silicon dioxide, 11 parts of expanded graphite, 1.5 parts of thermal conductor, and 2 parts of surfactant. The heat stabilizer is magnesium hydroxide and aluminum hydroxide, the mass ratio of magnesium hydroxide to aluminum hydroxide is 1.2, magnesium hydroxide is 30 parts, and aluminum hydroxide is 25 parts.
[0031] A method for preparing a high-efficiency ABS resin flame retardant comprises the following steps: Step 1, drying magnesium hydroxide, aluminum hydroxide, red phosphorus, melamine polyphosphate and nano silicon dioxide at 80° C. for 3 hours respectively; Step 2, expansing the expanded graphite at 180° C. for 1 h; Step 3, adding the dried magnesium hydroxide, aluminum hydroxide, red phosphorus, melamine polyphosphate, nano silicon dioxide, expanded graphite, thermal conductive graphite, and iron phosphate into a high-speed mixer, and mixing them evenly to obtain a mixed material; Step 4: Add polyethylene wax, antimony trioxide and organosilane coupling agent to the mixture, and continue mixing for 20 minutes to obtain a high-efficiency ABS resin flame retardant.
[0032] Example 4
[0033] A high-efficiency ABS resin flame retardant is composed of the following raw materials in parts by weight: 55 parts of heat stabilizer, 5 parts of red phosphorus, 11 parts of melamine polyphosphate, 5 parts of lubricant, 1.5 parts of phosphorus-containing metal salts such as calcium phosphate and 1.5 parts of calcium hydrogen phosphate, 0.6 parts of antimony-based synergist, 3 parts of nano-silicon dioxide, 14 parts of expanded graphite, 2 parts of thermal conductor, and 1 part of surfactant. The heat stabilizer is magnesium hydroxide and aluminum hydroxide, the mass ratio of magnesium hydroxide to aluminum hydroxide is 1.16, magnesium hydroxide is 29.5 parts, and aluminum hydroxide is 25.5 parts.
[0034] A method for preparing a high-efficiency ABS resin flame retardant comprises the following steps: Step 1, drying magnesium hydroxide, aluminum hydroxide, red phosphorus, melamine polyphosphate and nano silicon dioxide at 80° C. for 3 hours respectively; Step 2, expansing the expanded graphite at 180° C. for 1 h; Step 3, adding the dried magnesium hydroxide, aluminum hydroxide, red phosphorus, melamine polyphosphate, nano silicon dioxide, expanded graphite, thermal conductive graphite, calcium phosphate and calcium hydrogen phosphate into a high-speed mixer, mixing evenly to obtain a mixed material; Step 4: Add polyethylene wax, antimony trioxide and organosilane coupling agent to the mixture, and continue mixing for 20 minutes to obtain a high-efficiency ABS resin flame retardant.
[0035] Example 5
[0036] A high-efficiency ABS resin flame retardant is composed of the following raw materials in parts by weight: 55 parts of heat stabilizer, 9 parts of red phosphorus, 10 parts of melamine polyphosphate, 7 parts of lubricant, 2 parts of calcium phosphate and 2 parts of iron phosphate as phosphorus-containing metal salt, 0.6 parts of antimony-based synergist, 5 parts of nano-silicon dioxide, 12 parts of expanded graphite, 0.8 parts of thermal conductor, and 1.5 parts of surfactant. The heat stabilizer is magnesium hydroxide and aluminum hydroxide, the mass ratio of magnesium hydroxide to aluminum hydroxide is 1.29, magnesium hydroxide is 31 parts, and aluminum hydroxide is 24 parts.
[0037] A method for preparing a high-efficiency ABS resin flame retardant comprises the following steps: Step 1, drying magnesium hydroxide, aluminum hydroxide, red phosphorus, melamine polyphosphate and nano silicon dioxide at 85° C. for 2 hours respectively; Step 2, expanding the expanded graphite at 190° C. for 1 h; Step 3, adding the dried magnesium hydroxide, aluminum hydroxide, red phosphorus, melamine polyphosphate, nano silicon dioxide, expanded graphite, thermal conductive graphite, calcium phosphate and iron phosphate into a high-speed mixer, mixing evenly to obtain a mixed material; Step 4: Add polyethylene wax, antimony trioxide and organosilane coupling agent to the mixture, and continue mixing for 25 minutes to obtain a high-efficiency ABS resin flame retardant.
[0038] Comparative Example 1
[0039] An ABS resin flame retardant is composed of the following raw materials in parts by weight: 25 parts of magnesium hydroxide, 20 parts of aluminum hydroxide, 8 parts of red phosphorus, 8 parts of pentaerythritol, 5 parts of nano silicon dioxide, and 2 parts of organic silane coupling agent.
[0040] A method for preparing an ABS resin flame retardant comprises the following steps: Step 1, drying magnesium hydroxide, aluminum hydroxide, red phosphorus, and nano silicon dioxide at 90° C. for 1.5 hours respectively; Step 2, adding the dried magnesium hydroxide, aluminum hydroxide, red phosphorus and nano silicon dioxide into a high-speed mixer, mixing them evenly to obtain a mixed material; Step 3: Add pentaerythritol and organic silane coupling agent to the mixture, and continue mixing for 15 minutes to obtain ABS resin flame retardant.
[0041] Comparative Example 2
[0042] An ABS resin flame retardant is composed of the following raw materials in parts by weight: 10 parts of red phosphorus, 13 parts of melamine polyphosphate, 8 parts of pentaerythritol, 8 parts of nano silicon dioxide, 5 parts of calcium phosphate, 0.1 parts of antimony trioxide, 11 parts of expanded graphite, 1.5 parts of graphene, and 2 parts of organic silane coupling agent.
[0043] A method for preparing an ABS resin flame retardant comprises the following steps: Step 1, drying red phosphorus, melamine polyphosphate and nano silicon dioxide at 90° C. for 1.5 hours respectively; Step 2: Expanding the expanded graphite at 180° C. for 1.5 h.
[0044] Step 3, adding the dried red phosphorus, melamine polyphosphate, nano-silicon dioxide, expanded graphite, graphene, and calcium phosphate into a high-speed mixer, and mixing them evenly to obtain a mixed material; Step 4: Add pentaerythritol, antimony trioxide and organosilane coupling agent to the mixture, and continue mixing for 15 minutes to obtain ABS resin flame retardant.
[0045] Comparative Example 3
[0046] An ABS resin flame retardant is composed of the following raw materials in parts by weight: 25 parts of magnesium hydroxide, 20 parts of aluminum hydroxide, 12 parts of melamine polyphosphate, 8 parts of pentaerythritol, 1 part of antimony trioxide, 5 parts of nano silicon dioxide, 2 parts of graphene, and 2 parts of organic silane coupling agent.
[0047] A method for preparing an ABS resin flame retardant comprises the following steps: Step 1, drying magnesium hydroxide, aluminum hydroxide, melamine polyphosphate and nano silicon dioxide at 90° C. for 3 hours respectively; Step 2, adding the dried magnesium hydroxide, aluminum hydroxide, melamine polyphosphate, nano-silicon dioxide, and graphene into a high-speed mixer, and mixing them evenly to obtain a mixed material; Step 3: Add pentaerythritol, antimony trioxide and organosilane coupling agent to the mixture, and continue mixing for 15 minutes to obtain ABS resin flame retardant.
[0048] The flame retardants prepared in Examples 1-5 and Comparative Examples 1-3 were added to ABS resin respectively, with the addition amount of the flame retardant being 20%. Standard specimens were prepared by injection molding, and their flame retardant properties and mechanical properties were tested. The results are shown in Table 1.
[0049] Table 1 Performance test results
[0050] Note: In Table 1, "A" means that the smoke exhausted during combustion will hardly leak to the outside; "B" means that there is a small amount of smoke leakage; "C" means that there is a large amount of smoke leakage.
[0051] As can be seen from the results of Table 1, the high-efficiency ABS resin flame retardant prepared by Examples 1-5 of the present invention has good flame retardant properties and mechanical properties. Compared with Comparative Examples 1-3, the flame retardant of the present invention has obvious improvements in limiting oxygen index, vertical combustion grade, etc., and has little effect on the mechanical properties of ABS resin. It can be seen from the performance test data of Examples 1-5 that Example 1 is the best embodiment. No phosphorus-containing metal salt, antimony-based synergist, expanded graphite, thermal conductor, or melamine polyphosphate was added to Comparative Example 1, and the vertical combustion grade of Comparative Example 1 was the lowest. It shows that antimony-based synergist, expanded graphite, thermal conductor, and melamine polyphosphate cooperate with each other and have a greater impact on flame retardant properties. No magnesium hydroxide or aluminum hydroxide was added to Comparative Example 2, and the flame retardant time of Comparative Example 2 was the shortest. The flame retardant time refers to the time that the material remains non-combustible at a certain temperature. The longer the time, the better the flame retardancy. On the contrary, the flame retardancy is low. It shows that magnesium hydroxide and aluminum hydroxide play a role in improving flame retardancy.
[0052] Comparative Example 3 does not add phosphorus-containing metal salt, red phosphorus and expanded graphite, and a large amount of smoke is generated during combustion of Comparative Example 3, which indicates that the combination of phosphorus-containing metal salt, expanded graphite and red phosphorus reduces the smoke generated by the combustion of the material.
[0053] The flame retardants prepared in Examples 1-5 were added to ABS resin respectively, with the addition amount of the flame retardant being 30%. Standard specimens were prepared by injection molding, and their flame retardant properties and mechanical properties were tested. The results are shown in Table 2.
[0054] Table 2 Performance test results
[0055] Note: "A" in Table 2 means that the smoke exhausted during combustion will hardly leak to the outside.
[0056] It can be seen from the data in Table 2 that the mechanical properties of the ABS resin are not greatly affected by increasing the amount of flame retardant added, which shows that the present invention has a synergistic flame retardant effect through the compounding of multiple raw materials, and can significantly improve the flame retardant performance and thermal stability of the flame retardant. The amount of the flame retardant added is small, and will not have a significant effect on the mechanical properties and processing properties of the ABS resin.
[0057] Therefore, the present invention adopts the above-mentioned high-efficiency ABS resin flame retardant and its preparation method, which is compounded by multiple raw materials, has a synergistic flame retardant effect, can significantly improve the flame retardant performance and thermal stability of the flame retardant, and the addition amount of the flame retardant is small, and will not have a significant effect on the mechanical properties and processing properties of the ABS resin.
[0058] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A high-efficiency ABS resin flame retardant, characterized in that: The invention is composed of the following raw materials in parts by weight: 35-55 parts of heat stabilizer, 2-10 parts of red phosphorus, 10-15 parts of melamine polyphosphate, 5-10 parts of lubricant, 1-5 parts of phosphorus-containing metal salt, 0.1-1 parts of antimony-based synergist, 3-8 parts of nano silicon dioxide, 10-15 parts of expanded graphite, 0.1-3 parts of thermal conductor and 1-3 parts of surfactant.
2. A high-efficiency ABS resin flame retardant according to claim 1, characterized in that: The invention is composed of the following raw materials in parts by weight: 45 parts of heat stabilizer, 8 parts of red phosphorus, 12 parts of melamine polyphosphate, 8 parts of lubricant, 5 parts of phosphorus-containing metal salt, 0.1 parts of antimony-based synergist, 5 parts of nano silicon dioxide, 12 parts of expanded graphite, 2 parts of thermal conductor and 2 parts of surfactant.
3. The high-efficiency ABS resin flame retardant according to claim 1, characterized in that: The heat stabilizer is magnesium hydroxide and aluminum hydroxide, and the mass ratio of magnesium hydroxide to aluminum hydroxide is 1.15-1.
34.
4. The high-efficiency ABS resin flame retardant according to claim 3, characterized in that: The mass ratio of the magnesium hydroxide to the aluminum hydroxide is 1.
25.
5. The high-efficiency ABS resin flame retardant according to claim 1, characterized in that: The lubricant is at least one of pentaerythritol, zinc stearate, barium stearate and polyethylene wax.
6. The high-efficiency ABS resin flame retardant according to claim 1, characterized in that: The antimony-based synergist is selected from at least one of antimony trioxide and antimony pentoxide.
7. The high-efficiency ABS resin flame retardant according to claim 1, characterized in that: The surfactant is an organic silane coupling agent or a titanate coupling agent.
8. The high-efficiency ABS resin flame retardant according to claim 1, characterized in that: The thermal conductor is at least one of thermally conductive graphite, carbon nanotubes, and graphene.
9. A method for preparing a high-efficiency ABS resin flame retardant according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1, drying the heat stabilizer, red phosphorus, melamine polyphosphate and nano silicon dioxide at 80-100° C. for 2-4 hours respectively; Step 2, adding the dried heat stabilizer, red phosphorus, melamine polyphosphate, nano silicon dioxide, expanded graphite, thermal conductor, and phosphorus-containing metal salt into a high-speed mixer, and mixing them evenly to obtain a mixed material; Step 3: Add the lubricant, antimony-based synergist and surfactant to the mixed material, and continue mixing for 10-20 minutes to obtain a high-efficiency ABS resin flame retardant.
10. The method for preparing a high-efficiency ABS resin flame retardant according to claim 9, characterized in that: In step 2, the expanded graphite needs to be expanded at 150-200° C. for 1-2 hours before being added to the high-speed mixer.
Citation Information
Patent Citations
Novel fireproof sealing material and preparation method thereof
CN110317421A
Flame retardant, preparation method thereof and wires and cables
CN110396240A
KR20210044982A
Cited By
Flame-retardant ABS modified material and preparation method thereof
CN120966190A