Anti-puncture sole material and preparation method thereof
By combining homemade modified EVA, the rigid cage-type POSS structure and sulfur-nitrogen structure are introduced, which solves the problem of insufficient puncture resistance of EVA foamed materials, achieves high puncture resistance and good rebound, and improves the sole material Puncture resistance.
Patent Information
- Application Number
- CN202411106704.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The puncture resistance of EVA foamed materials is insufficient. When the prior art dopant hard fillers or the introduction of crosslinked materials, the material density increases, the service life is shortened or the rebound is reduced, which affects the wear comfort.
Using a compound homemade modified EVA, the amide compound with terminal thiol group and hydroxyl group is formed by transesterification of methyl 3-mercaptopropionate and diethanolamine, and double bond click addition with octavinyl-POSS to introduce The rigid cage-type POSS structure enhances the puncture resistance of the material, and at the same time, it uses sulfur-nitrogen structure and zinc oxide to improve the strengthening effect of the material.
It greatly improves the puncture resistance of the shoe material, maintains moderate visual density and good rebound, forms countless microscopic soft and hard structures, increases the penetration resistance, and hinders the directional penetration of the puncture objects.
Smart Images

Figure BDA0004991030670000081 
Figure BDA0004991030670000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of EVA foam materials, and in particular relates to a puncture-proof sole material and a preparation method thereof. Background Art
[0002] Ethylene-vinyl acetate copolymer (EVA) is one of the core materials for shoes. Among them, EVA foam is still the first choice for most casual shoes and jogging shoes on the market. Compared with rubber soles, it has lower density, good impact resistance, shock resistance and elasticity, and is light and comfortable to wear, which makes it widely loved by people.
[0003] However, the puncture resistance of EVA materials is insufficient. In some specific environments, such as wild jungles and construction sites, it is impossible to effectively prevent sharp objects such as bamboo sticks and steel nails from penetrating the soles, which limits the application of EVA materials to a certain extent. In the prior art, by adding hard fillers to EVA materials, the puncture resistance of EVA can be improved to a certain extent. However, these fillers form internal defects in the EVA materials, resulting in an increase in the density of the EVA materials. Especially in foamed materials, when the materials are deformed by force, these fillers puncture the pore walls, shortening the service life of the materials. Introducing cross-linked materials into EVA materials can also improve the puncture resistance to a certain extent by promoting the cross-linking degree of EVA, but it will reduce the resilience of EVA and affect the wearing comfort. Therefore, based on the existing EVA foaming system, this application discloses an EVA foaming material for puncture-resistant shoes. Summary of the invention
[0004] In order to solve the technical problems mentioned in the background technology, the object of the present invention is to provide a puncture-proof sole material and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A puncture-proof sole material, comprising the following raw materials in parts by weight:
[0007] 100 parts of EVA masterbatch, 10-15 parts of POE masterbatch, 25-35 parts of modified EVA, 10-13 parts of filler, 5.2-6.5 parts of foaming agent, 0.9-1.2 parts of bridging agent, 1.4-1.8 parts of accelerator and 2.5-3 parts of lubricant.
[0008] Wherein, modified EVA is prepared by the following method:
[0009] Step A1: methyl 3-mercaptopropionate, diethanolamine and anhydrous tetrahydrofuran are mixed, nitrogen is introduced for protection, the temperature is raised to 55-65° C., stirring is applied at 120-150 rpm and reflux is performed, sodium hydride is slowly added, and the total reaction time of sodium hydride addition is controlled to be 2.5-3 h. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation to obtain an intermediate;
[0010] In the above reaction, the usage ratio of methyl 3-mercaptopropionate, diethanolamine, sodium hydride and anhydrous tetrahydrofuran is 0.1 mol: 0.1 mol: 30-40 mg: 25-40 mL. Under the catalysis of sodium hydride, methyl 3-mercaptopropionate and diethanolamine undergo amine ester exchange.
[0011] Step A2: Mix octavinyl-POSS and dimethylacetamide, then add the intermediate and dimethylphenylphosphine, and mix them. Pass nitrogen protection, heat to 80-90°C, stir at 60-90 rpm, and apply 150-200 W / m 2 UV irradiation, reaction for 4.5-5.5h, adding water for washing after the reaction, removing the aqueous phase and vacuum drying to obtain a modifier;
[0012] In the above reaction, the usage ratio of octavinyl-POSS, intermediate, dimethylphenylphosphine and dimethylacetamide is 10mmol:0.1mol:10-20mg:50-60mL. Under the initiation of dimethylphenylphosphine and ultraviolet radiation, the thiol group in the intermediate and the double bond of octavinyl-POSS undergo click addition.
[0013] Step A3: EVA-g-MAH, a modifier, anhydrous sodium acetate and xylene are mixed, nitrogen is introduced for protection, the temperature is raised to 100-120° C., stirring is applied at 30-55 rpm, the reaction is carried out for 1.5-2.2 hours, and xylene is evaporated under reduced pressure after the reaction is completed to obtain modified EVA;
[0014] In the above reaction, the dosage ratio of EVA-g-MAH, modifier, anhydrous sodium acetate and xylene is 100g:8-12mmol:0.8-1.1g:200-280mL. Under the catalysis of anhydrous sodium acetate, the polyol hydroxyl groups in the modifier molecules are esterified with the acid anhydride between the EVA-g-MAH side chains, and the modifier is introduced between the molecular chains of EVA-g-MAH.
[0015] A method for preparing a puncture-resistant sole material comprises the following steps:
[0016] Step S1: adding various raw materials for making the sole material into a stirrer according to weight proportions and mixing them evenly to obtain a batch material;
[0017] Step S2: transferring the batch material into a foaming machine, kneading at 120-130° C. for 15-20 min, squeezing into a mold, foaming at 165-180° C. for 11-15 min, cooling and demoulding to obtain the puncture-resistant sole material.
[0018] Preferably, the filler is selected from calcium carbonate micropowder with a fineness of not less than 325 mesh.
[0019] Preferably, the foaming agent is compounded from foaming agent AC-3000 and foaming agent AK-3.
[0020] Preferably, the bridging agent is prepared by compounding triallyl isocyanurate and di-tert-butyl peroxyisopropylbenzene.
[0021] Preferably, the accelerator is selected from zinc oxide.
[0022] Preferably, the lubricant is selected from stearic acid.
[0023] Beneficial effects of the present invention:
[0024] The invention discloses a foamed EVA sole material. The puncture resistance of the shoe material is greatly improved by compounding homemade modified EVA, and the shoe material has moderate apparent density, good resilience and folding resistance. The modified EVA is prepared by amine ester exchange of 3-mercaptopropionic acid methyl ester and diethanolamine to prepare an amide compound with terminal thiol and hydroxyl, i.e., an intermediate. Then, the active thiol of the intermediate and the double bond of octavinyl-POSS are click-added to graft the intermediate to the molecular end of octavinyl-POSS to obtain a modifier. Finally, under the catalysis of anhydrous sodium acetate, the polyol hydroxyl in the modifier molecule is esterified with the acid anhydride between the EVA-g-MAH side chain, and the modifier is introduced into the molecular chain of the EVA-g-MAH. The modified EVA is mainly composed of an EVA macromolecular chain and has good compatibility with a substrate EVA. A rigid cage-type POSS structure is introduced into the substrate EVA during the blending process, so as to improve the compatibility of the EVA-g-MAH with the substrate EVA. The VA substrate is strengthened to improve the puncture resistance of the material. On the other hand, the rigid cage-type POSS structure is dispersed in the EVA soft chain to form countless microscopic soft and hard uneven structures. When subjected to external puncture, the soft chain is easily deformed by puncture, while the rigid cage-type POSS structure is not easily deformed, forming anchor points, and forming countless microscopic local stretching at the puncture position, so that the modified EVA material is fully attached to the surface of the punctured object, increasing the penetration resistance. At the same time, the uneven rigid cage-type POSS structure changes the force uniformity of the material, forming force anisotropy at the penetration position, hindering the directional penetration of the punctured object; in the preparation process of the modified EVA, the sulfur-nitrogen structure introduced by the intermediate forms a chelation effect, and chelates with the filler calcium carbonate and the promoter zinc oxide during the blending and foaming process, thereby improving the strengthening effect of these inorganic particles on the EVA matrix, and at the same time compounding with the rigid cage-type POSS structure in situ to strengthen the anchoring effect of the rigid chain segment. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Example 1, preparation of puncture-resistant sole material, the specific implementation process is as follows:
[0027] (1) Preparation of modified EVA
[0028] Step A1: Mix methyl 3-mercaptopropionate, diethanolamine and anhydrous tetrahydrofuran, introduce nitrogen protection, heat to 55°C, stir at 120rpm and reflux, slowly add sodium hydride, the addition time is 1.5h, and after the sodium hydride is completely added, continue the constant temperature reflux reaction, and control the total reaction time of the addition of sodium hydride to be 3h, wherein the amount ratio of methyl 3-mercaptopropionate, diethanolamine, sodium hydride and anhydrous tetrahydrofuran is 0.1mol:0.1mol:30mg:25mL. After the reaction is completed, remove tetrahydrofuran by rotary evaporation to obtain an intermediate.
[0029] Step A2: Mix octavinyl-POSS and dimethylacetamide, then add the intermediate and dimethylphenylphosphine, and pass nitrogen protection, heat to 80°C, stir at 60 rpm, and apply 150 W / m 2 The reaction was carried out under ultraviolet irradiation for 5.5 hours, wherein the usage ratio of octavinyl-POSS, intermediate, dimethylphenylphosphine and dimethylacetamide was 10 mmol: 0.1 mol: 10 mg: 50 mL. After the reaction was completed, water was added for washing, and the aqueous phase was removed and vacuum dried to obtain a modifier.
[0030] Step A3: Take EVA-g-MAH, modifier, anhydrous sodium acetate and xylene, mix them, introduce nitrogen protection, heat to 100°C, stir at 30 rpm, and react for 2.2 hours. In the process of EVA-g-MAH implementation, Dow Chemical's Bynel E418 type raw material is used, and the amount ratio of EVA-g-MAH, modifier, anhydrous sodium acetate and xylene is 100g:8mmol:0.8g:200mL. After the reaction, xylene is evaporated under reduced pressure to obtain modified EVA.
[0031] (2) Preparation of puncture-resistant sole materials
[0032] Step S1: Take the raw materials according to the weight ratio, 100 parts of EVA masterbatch, SF45 raw material of Taiwan Plastics Industry Co., Ltd. is used in the implementation process; 15 parts of POE masterbatch, 8003 raw material of Dow Chemical is used in the implementation process; 25 parts of modified EVA, which is self-made in this embodiment; 13 parts of filler, industrial grade 325 mesh calcium carbonate is used in the implementation process; 5.2 parts of foaming agent, AC-3000 foaming agent of Zhejiang Haitai New Materials Technology Co., Ltd. and AK -3 type foaming agent, the two are pre-mixed and compounded in a weight ratio of 2:1; 0.9 parts of bridging agent, industrial-grade triallyl isocyanurate and di-tert-butyl peroxy isopropylbenzene are used in the implementation process, the two are compounded in a weight ratio of 10:1 and mixed during the preparation; 1.6 parts of accelerator, rubber-grade zinc oxide of Shanghai Changjiu Chemical Co., Ltd. is used in the implementation process; 3 parts of lubricant, 1801 type stearic acid of Shanghai Changjiu Chemical Co., Ltd. is used in the implementation process; add each raw material into a stirrer, mix at 600rpm for 15min, and obtain a batch material.
[0033] Step S2: The batch material is transferred into a foaming machine, kneaded at 120° C. for 20 min, extruded into a mold, foamed at 165° C. for 15 min, cooled and demoulded to obtain the puncture-resistant sole material.
[0034] Example 2, preparation of puncture-resistant sole material, the specific implementation process is as follows:
[0035] (1) Preparation of modified EVA
[0036] Step A1: Mix methyl 3-mercaptopropionate, diethanolamine and anhydrous tetrahydrofuran, introduce nitrogen protection, heat to 65°C, stir at 150rpm and reflux, slowly add sodium hydride, the addition time is 1 hour, continue the constant temperature reflux reaction after the sodium hydride is completely added, and control the total reaction time of the addition of sodium hydride to be 2.5 hours, wherein the amount ratio of methyl 3-mercaptopropionate, diethanolamine, sodium hydride and anhydrous tetrahydrofuran is 0.1 mol: 0.1 mol: 40 mg: 40 mL, and after the reaction is completed, remove tetrahydrofuran by rotary evaporation to obtain an intermediate.
[0037] Step A2: Mix octavinyl-POSS and dimethylacetamide, then add the intermediate and dimethylphenylphosphine, and pass nitrogen protection, heat to 90°C, stir at 90 rpm, and apply 200 W / m 2 The reaction was carried out under ultraviolet irradiation for 4.5 hours, wherein the usage ratio of octavinyl-POSS, intermediate, dimethylphenylphosphine and dimethylacetamide was 10 mmol: 0.1 mol: 20 mg: 60 mL. After the reaction was completed, water was added for washing, and the aqueous phase was removed and vacuum dried to obtain a modifier.
[0038] Step A3: Take EVA-g-MAH, modifier, anhydrous sodium acetate and xylene, mix them, introduce nitrogen protection, heat to 120°C, stir at 55 rpm, and react for 1.5 hours. In the process of EVA-g-MAH implementation, Dow Chemical's Bynel E418 type raw material is used, and the amount ratio of EVA-g-MAH, modifier, anhydrous sodium acetate and xylene is 100g:12mmol:1.1g:280mL. After the reaction, xylene is evaporated under reduced pressure to obtain modified EVA.
[0039] (2) Preparation of puncture-resistant sole materials
[0040] Step S1: Take the raw materials according to the weight ratio, 100 parts of EVA masterbatch, SF45 raw material of Taiwan Plastics Industry Co., Ltd. is used in the implementation process; 10 parts of POE masterbatch, 8003 raw material of Dow Chemical is used in the implementation process; 35 parts of modified EVA, which is self-made in this embodiment; 10 parts of filler, industrial grade 325 mesh calcium carbonate is used in the implementation process; 6.5 parts of foaming agent, AC-3000 foaming agent of Zhejiang Haitai New Materials Technology Co., Ltd. and AK- Type 3 foaming agent, the two are pre-mixed and compounded in a weight ratio of 2:1; 1.1 parts of bridging agent, industrial-grade triallyl isocyanurate and di-tert-butyl peroxyisopropylbenzene are used in the implementation process, the two are compounded in a weight ratio of 10:1 and mixed during the formulation; 1.8 parts of accelerator, rubber-grade zinc oxide of Shanghai Changjiu Chemical Co., Ltd. is used in the implementation process; 2.5 parts of lubricant, 1801 type stearic acid of Shanghai Changjiu Chemical Co., Ltd. is used in the implementation process; add each raw material into a stirrer, mix at 600rpm for 15min, and obtain a batch material.
[0041] Step S2: The batch material is transferred into a foaming machine, kneaded at 130° C. for 15 min, extruded into a mold, foamed at 180° C. for 11 min, cooled and demoulded to obtain a puncture-resistant sole material.
[0042] Example 3, preparation of puncture-resistant sole material, the specific implementation process is as follows:
[0043] (1) Preparation of modified EVA
[0044] Step A1: Mix methyl 3-mercaptopropionate, diethanolamine and anhydrous tetrahydrofuran, introduce nitrogen protection, heat to 60°C, stir at 120rpm and reflux, slowly add sodium hydride, the addition time is 1.3h, and after the sodium hydride is completely added, continue the constant temperature reflux reaction, and control the total reaction time of the addition of sodium hydride to be 2.8h, wherein the amount ratio of methyl 3-mercaptopropionate, diethanolamine, sodium hydride and anhydrous tetrahydrofuran is 0.1mol:0.1mol:35mg:40mL. After the reaction is completed, remove tetrahydrofuran by rotary evaporation to obtain an intermediate.
[0045] Step A2: Mix octavinyl-POSS and dimethylacetamide, then add the intermediate and dimethylphenylphosphine, and pass nitrogen protection, heat to 85°C, stir at 90 rpm, and heat at 180 W / m 2 The reaction was carried out under ultraviolet irradiation for 5.2 hours, wherein the usage ratio of octavinyl-POSS, intermediate, dimethylphenylphosphine and dimethylacetamide was 10 mmol: 0.1 mol: 15 mg: 60 mL. After the reaction was completed, water was added for washing, and the aqueous phase was removed and dried in vacuo to obtain a modifier.
[0046] Step A3: Take EVA-g-MAH, modifier, anhydrous sodium acetate and xylene, mix them, introduce nitrogen protection, heat to 110°C, stir at 55rpm, and react for 2h, wherein the EVA-g-MAH implementation process uses Dow Chemical's Bynel E418 type raw material, and the amount ratio of EVA-g-MAH, modifier, anhydrous sodium acetate and xylene is 100g:10mmol:1.1g:240mL. After the reaction is completed, xylene is evaporated under reduced pressure to obtain modified EVA.
[0047] (2) Preparation of puncture-resistant sole materials
[0048] Step S1: Take the raw materials according to the weight ratio, 100 parts of EVA masterbatch, SF45 raw material of Taiwan Plastics Industry Co., Ltd. is used in the implementation process; 12 parts of POE masterbatch, 8003 raw material of Dow Chemical is used in the implementation process; 30 parts of modified EVA, which is self-made in this embodiment; 11 parts of filler, industrial grade 325 mesh calcium carbonate is used in the implementation process; 5.8 parts of foaming agent, AC-3000 foaming agent of Zhejiang Haitai New Materials Technology Co., Ltd. and AK- Type 3 foaming agent, the two are pre-mixed and compounded in a weight ratio of 2:1; 1.2 parts of bridging agent, industrial-grade triallyl isocyanurate and di-tert-butyl peroxy isopropylbenzene are used in the implementation process, the two are compounded in a weight ratio of 10:1 and mixed during the formulation; 1.4 parts of accelerator, rubber-grade zinc oxide of Shanghai Changjiu Chemical Co., Ltd. is used in the implementation process; 2.7 parts of lubricant, 1801 type stearic acid of Shanghai Changjiu Chemical Co., Ltd. is used in the implementation process; add each raw material into a stirrer, mix at 600rpm for 15min, and obtain a batch material.
[0049] Step S2: The batch material is transferred into a foaming machine, kneaded at 130° C. for 17 min, extruded into a mold, foamed at 170° C. for 13 min, cooled and demoulded to obtain a puncture-resistant sole material.
[0050] Comparative Example 1
[0051] This comparative example is a reference example of Example 3, except that 30 parts of modified EVA in the raw materials are replaced by 26 parts of Bynel E418 type EVA-g-MAH and 4 parts of octavinyl-POSS, and the rest of the implementation process is exactly the same.
[0052] Comparative Example 2
[0053] This comparative example refers to the prior art, without adding modified EVA, and prepares the sole material by increasing the amount of filler and bridging agent. The specific ingredients are: 100 parts of EVA masterbatch, 12 parts of POE masterbatch, 22 parts of filler, 5.2 parts of foaming agent, 3.5 parts of bridging agent, 1.4 parts of accelerator and 2.7 parts of lubricant. The specific process for preparing the sole material is the same as Example 3.
[0054] Comparative Example 3
[0055] This comparative example is the EVA sole material of the TM3161 sports safety shoes of Ruian Hongshun Shoes Co., Ltd.
[0056] Samples were taken from the above sole materials, and the density test was carried out according to the HG / T 2872-2009 standard; the puncture test was carried out according to the GB / T12017-1989 standard; the resilience test was carried out according to the HG / T 4993-2016 standard; and the folding resistance test was carried out according to the GB / T3903.1-2017 standard. The specific test results are shown in the following table:
[0057]
[0058]
[0059] It can be seen from the test results in the above table that the sole material of the embodiment has moderate apparent density, good resilience and folding resistance, and a puncture force of more than 900N, showing excellent puncture resistance compared to the comparative example.
[0060] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0061] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A puncture-proof sole material, characterized in that: The following raw materials are included by weight: 100 parts of EVA masterbatch, 10-15 parts of POE masterbatch, 25-35 parts of modified EVA, 10-13 parts of filler, 5.2-6.5 parts of foaming agent, 0.9-1.2 parts of bridging agent, 1.4-1.8 parts of accelerator and 2.5-3 parts of lubricant; The modified EVA is prepared by the following method: Step A1: methyl 3-mercaptopropionate, diethanolamine and anhydrous tetrahydrofuran are mixed, nitrogen is introduced for protection, the temperature is raised to 55-65° C., stirred under reflux, sodium hydride is slowly added, and the total reaction time of sodium hydride addition is controlled to be 2.5-3 h. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation to obtain an intermediate; Step A2: Mix octavinyl-POSS and dimethylacetamide, then add the intermediate and dimethylphenylphosphine, add nitrogen protection, heat to 80-90°C, stir and add 150-200W / m 2 UV irradiation, reaction for 4.5-5.5h, adding water for washing after the reaction, removing the water phase and vacuum drying to obtain a modifier; Step A3: EVA-g-MAH, a modifier, anhydrous sodium acetate and xylene are mixed, nitrogen is introduced for protection, the temperature is raised to 100-120° C., and the reaction is stirred for 1.5-2.2 hours. After the reaction is completed, the xylene is evaporated under reduced pressure to obtain modified EVA.
2. The puncture-resistant sole material according to claim 1, characterized in that: The usage ratio of methyl 3-mercaptopropionate, diethanolamine, sodium hydride and anhydrous tetrahydrofuran is 0.1 mol: 0.1 mol: 30-40 mg: 25-40 mL.
3. The puncture-resistant sole material according to claim 2, characterized in that: The usage ratio of octavinyl-POSS, intermediate, dimethylphenylphosphine and dimethylacetamide is 10mmol:0.1mol:10-20mg:50-60mL.
4. The puncture-resistant sole material according to claim 3, characterized in that: The usage ratio of EVA-g-MAH, modifier, anhydrous sodium acetate and xylene is 100 g: 8-12 mmol: 0.8-1.1 g: 200-280 mL.
5. The method for preparing a puncture-resistant sole material according to claim 4, characterized in that: The steps include: Step S1: adding the raw materials in proportion by weight into a stirrer and mixing them evenly to obtain a batch material; Step S2: transferring the batch material into a foaming machine, kneading at 120-130° C. for 15-20 min, squeezing into a mold, foaming at 165-180° C. for 11-15 min, cooling and demoulding to obtain the puncture-resistant sole material.
6. The method for preparing a puncture-resistant sole material according to claim 5, characterized in that: The filler is calcium carbonate powder with a fineness of not less than 325 mesh.
7. The method for preparing a puncture-resistant sole material according to claim 5, characterized in that: The foaming agent is compounded by foaming agent AC-3000 and foaming agent AK-3.
8. The method for preparing a puncture-resistant sole material according to claim 5, characterized in that: The bridging agent is prepared by compounding triallyl isocyanurate and di-tert-butyl peroxyisopropylbenzene.
9. The method for preparing a puncture-resistant sole material according to claim 5, characterized in that: The accelerator is zinc oxide.
10. The method for preparing a puncture-resistant sole material according to claim 5, characterized in that: The lubricant is stearic acid.
Citation Information
Patent Citations
Rubber and plastic puncture-proof multifunctional shoe sole and preparation method thereof
CN111543734A
High-wear-resistance EVA (Ethylene Vinyl Acetate) foaming material for shoes and preparation method thereof
CN113881130A
Insulated multilayer sheet, method of manufacture, and article using same
CN116710276A
Antibacterial breathable sole material and preparation method thereof
CN117586635A
Modified EVA (Ethylene Vinyl Acetate) foaming material for soles and preparation method thereof
CN117659556A
Cited By
Impact-resistant chlorinated polyvinyl chloride composite material and preparation method thereof
CN120775326A
Impact-resistant chlorinated polyvinyl chloride composite material and method for preparing the same
CN120775326B