Impact modifier composition and application thereof
By optimizing the block copolymer structure in the polyolefin composition by using a specific proportion of impact modifiers and additives, the balance of the polypropylene composition between impact resistance, transparency, stiffness and flow properties is solved. A comprehensive performance improvement has been achieved.
Patent Information
- Application Number
- CN202410607391.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2024-05-16
- Publication Date
- 2024-11-22
AI Technical Summary
Existing polypropylene compositions are difficult to achieve a good balance between impact resistance, transparency, high stiffness, tensile strength and flow properties, and traditional impact modifiers sacrifice other properties when improving impact resistance.
Using substantially 65-99% polypropylene homopolymer, 1-35% impact modifier (the first hydrogenated styrene-type block copolymer and at least one second hydrogenated styrene-type block A polyolefin composition composed of a copolymer or polyolefin copolymer) and up to 25% by weight of additives optimizes the performance of the composition by adjusting the structure and proportion of the block copolymer.
The impact resistance, transparency, high stiffness and tensile strength of the polyolefin composition are significantly improved, and a good balance between performance is achieved, which is specifically manifested as increased bending sewing modulus, reduced transmittance, and impact of the simple-supported beam notched Increased yield strain and increased elongation of break.
Smart Images

Figure BDA0004842466030000151 
Figure BDA0004842466030000161 
Figure BDA0004842466030000171
Abstract
Description
Technical Field
[0001] The present disclosure relates to impact modifiers, methods for their preparation, and their use in polyolefin compositions. Background Art
[0002] Polyolefin-based polymers and their compositions are used in large quantities. Among polyolefins, polypropylene compositions have many applications, including packaging materials, mechanical parts, automotive parts, electrical appliances, etc. For the desired end-use applications, such compositions need to have better mechanical properties, flexibility, scratch resistance, processability, heat resistance, etc. Impact resistance is an important property that competes with engineering thermoplastics in compositions.
[0003] In order to improve the impact resistance of compositions containing polypropylene, impact modifiers, such as rubber materials, have been used. By incorporating rubber materials, impact resistance can be achieved at the expense of reduced stiffness, flowability, transparency, etc. In order to improve the impact resistance of polyolefin compositions, impact modifiers based on styrenic block copolymers (SBCs) have been used.
[0004] There remains a need to provide an improved polypropylene composition with SBC having improved impact resistance and a good balance of clarity, high stiffness, tensile strength, flow properties, and the like. SUMMARY OF THE INVENTION
[0005] In one aspect, the present disclosure relates to a polyolefin composition comprising, consisting essentially of, or consisting of: (a) 65-99 wt% of a polypropylene homopolymer having a melt flow rate (MFR) of 0.25-100 dg / min, as measured at 230°C and 2.16 kg according to ASTM D1238; (B) 1-35 wt% of an impact modifier consisting essentially of: (a) a first hydrogenated styrenic block copolymer (first HSBC) and (b) at least one polymer selected from (i) a second hydrogenated styrenic block copolymer (second HSBC) and (ii) a polyolefin copolymer (POLC), and (C) up to 25 wt% of at least one additive, based on the total weight of the polyolefin composition. The first HSBC has a block A and a block B. Prior to hydrogenation, each block A is a polymer block of a vinyl aromatic monomer and each block B is a polymer block of a conjugated diene monomer. The vinyl content of block B is 70-95 wt % based on the total weight of the conjugated diene monomers polymerized in block B. The second HSBC has blocks A' and blocks B'. Before hydrogenation, each block A' is a polymer block of a vinyl aromatic monomer, and each block B' is a polymer block of a conjugated diene monomer. The vinyl content of block B' is 0-50 wt % based on the total weight of the conjugated diene monomers polymerized in block B'. The polyolefin copolymer has a viscosity of 0.850-0.920 g / cm2 as measured according to ASTM D792. 3 and a melt index (MI) of 0.5-100 dg / min measured at 190° C. and a load of 2.16 kg according to ASTM D1238. The weight ratio of (a) to (b) is 1:10 to 10:1. When the at least one polymer is a second HSBC, at least one of the first or second HSBC has a polystyrene content (PSC) of 15-50 wt%.
[0006] In a second aspect, the polyolefin composition has the following properties when compared to a polyolefin composition in the absence of an impact modifier: (i) an increase in 1% flexural secant modulus of >5% and (ii) a decrease in transmittance measured with a sample thickness of 1.6 mm of <10%; or (iii) an increase in Charpy notched impact measured at 0°C of >10% and (iv) a decrease in transmittance measured with a sample thickness of 1.6 mm of <5%; or (v) an increase in Charpy notched impact measured at 21°C of >5% and (v) a decrease in transmittance measured with a sample thickness of 1.6 mm of <5%. vi) a decrease in transmittance measured at a sample thickness of 1.6 mm of less than 10%; or (vii) an increase in the notched radial beam impact measured at 21°C of >10% and (viii) a decrease in transmittance measured at a sample thickness of 1.6 mm of less than 5%; or (ix) an increase in yield strain of >10%, (x) a decrease in transmittance measured at a sample thickness of 1.6 mm of less than 5%; or (xi) an increase in elongation at break of >5% and (xii) a decrease in transmittance measured at a sample thickness of 1.6 mm of less than 5%. The 1% bending secant modulus is measured in accordance with ASTM D790. The notched charpy impact measured at 0°C and the notched charpy impact measured at 21°C are both measured in accordance with ASTM D610. The notched radial beam impact measured at 21°C is measured in accordance with ISO 180. The yield strain is measured in accordance with ISO 527-2. The elongation at break is measured in accordance with ISO 527-2. The transmittance is measured in accordance with ASTM D1003.
[0007] In the third aspect, the at least one polymer is a second hydrogenated styrenic block copolymer.
[0008] In a fourth aspect, each block A and A' independently has a molecular weight (Mp) of 1 to 40 kg / mol as determined according to ASTM 5296. DETAILED DESCRIPTION OF THE INVENTION
[0009] The following terms will be used throughout this specification.
[0010] “Consisting essentially of…” means that the claimed composition mainly comprises the specified materials, and is allowed to contain additional components that do not substantially affect the new characteristics or functions of the claimed invention. If present, the amount of the additional components is <30%, or <20%, or <10%.
[0011] "At least one of [A, B, and C]" or "any one of [A, B, and C]" refers to a single member thereof, more than one member thereof, or a combination of members thereof. For example, at least one of A, B, and C includes, for example, only A, only B, or only C, as well as A and B, A and C, B and C, or A, B and C, or any other combination of A, B, and C. Embodiments presented as "A, B, or C" should be interpreted to include only A, only B, only C, "A or B", "A or C", "B or C", or "A, B, or C".
[0013] The "polystyrene content" or PSC of a block copolymer refers to the weight percent of polymerized vinyl aromatic monomer (e.g., styrene) in the block copolymer, calculated by summing the molecular weights of all vinyl aromatic units divided by the total molecular weight of the block copolymer. PSC can be determined using any suitable method, such as proton nuclear magnetic resonance (NMR).
[0014] "Vinyl content" refers to the content of conjugated diene monomers polymerized by 1,2-addition in the case of butadiene or by 3,4-addition in the case of isoprene (thus producing a monosubstituted olefin or vinyl group adjacent to the polymer backbone). Vinyl content can be determined by nuclear magnetic resonance spectroscopy (NMR).
[0015] "Molecular weight" or Mw refers to the polystyrene equivalent molecular weight of a polymer block or block copolymer in kg / mol. Mw can be measured by gel permeation chromatography (GPC) using polystyrene calibration standards, for example, according to ASTM 5296. The GPC detector can be an ultraviolet or refractive index detector or a combination thereof. The chromatograph is calibrated using commercially available polystyrene molecular weight standards. The Mw of a polymer measured using a GPC so calibrated is the polystyrene equivalent molecular weight or apparent molecular weight. The Mw shown herein is measured at the peak of the GPC trace, usually referred to as the polystyrene equivalent "peak molecular weight", expressed as M p。
[0016] A "bimodal" molecular weight of a polymer refers to two or more distinct molecular weight peaks readily discernible in a graph of (x) molecular weight versus (y) function showing the relative proportion of polymer of a given molecular weight, such as obtained by gel permeation chromatography (GPC) analysis of the polymer.
[0017] The present disclosure relates to a polyolefin composition comprising, consisting essentially of, or consisting of: (A) a polypropylene homopolymer; (B) an impact modifier consisting essentially of (a) a first hydrogenated styrenic block copolymer (first HSBC) and (b) at least one polymer selected from: i) a second hydrogenated styrenic block copolymer (second HSBC) and ii) a polyolefin copolymer (POLC); and (C) optional additives. The polyolefin composition exhibits improved impact resistance and a good balance of transparency, high stiffness, tensile strength, and flow properties.
[0018] Polypropylene homopolymer
[0019] The polypropylene homopolymer is a polypropylene homopolymer (eg, isotactic, syndiotactic, atactic, etc.) prepared by any process known in the art. The polypropylene homopolymer may be obtained from virgin or recycled sources, and may be petroleum-based or bio-based when first prepared.
[0020] In some embodiments, polypropylene blend is used in the polyolefin composition, for example the blend of random ethylene or butene copolymer of polypropylene and propylene or the combination of crystalline random copolymer of ethylene and propylene and rubbery ethylene-propylene copolymer.Polypropylene copolymer can be used, including the copolymer of propylene and copolymerizable comonomer (for example ethylene, 1-butene, 1-pentene, 1-hexene, 1-octene or one or more conjugated or non-conjugated dienes).Gross weight based on the polypropylene copolymer, the amount of the comonomer can be 0.05-40 or 0.5-30 or 1-20 or 5-30wt%.
[0021] In some embodiments the polypropylene homopolymer is bimodal or multimodal from a molecular weight point of view and has a molecular weight (Mp) of 10-2000, or 30-1500, or 50-1000, or 100-800, or 150-500 or 200-400 kg / mol.
[0022] In some embodiments, the polypropylene homopolymer has a melting temperature (Tm) of 100-180°C, or 110-170°C, or 120-160°C, or 125-150°C.
[0023] In some embodiments, the polypropylene homopolymer has a crystallinity of 20-70%, or 25-65%, or 30-60%, or 35-55%, or >35%, or >40%, or >50%, as determined by differential scanning calorimetry (DSC) heat of melting according to ASTM F2625.
[0024] In some embodiments, the polypropylene homopolymer has a melt flow rate (MFR) of <400, or <300, or <200, or 5-100, or 0.25-100, or 0.25-75, or 0.50-70, or 15-65, or 20-40 dg / min, measured at 230°C and a load of 2.16 kg according to ASTM D1238.
[0025] In some embodiments, the polypropylene homopolymer is used in an amount of 65-99, or 70-99, or 70-95, or 75-99, or 75-90 wt %, based on the total weight of the polyolefin composition.
[0026] Impact modifier
[0027] The impact modifier comprises, consists essentially of, or consists of: (a) a first HSBC having a vinyl content of 70-95 wt % prior to hydrogenation; and (b) at least one polymer selected from i) a second HSBC having a vinyl content of 0-50 wt % prior to hydrogenation, and ii) a POLC; the weight ratio of the first HSBC to the at least one polymer being 1:10-10:1, or 1:8-8:1, or 1:5-5:1, or 1:2-2:1.
[0028] Hydrogenated Styrenic Block Copolymer (HSBC)
[0029] The first HSBC and the second HSBC (if present) are independently obtained by hydrogenating an SBC precursor, which is any of a linear, branched or radial block copolymer having at least one block A or A' and at least one block B or B'.
[0030] In some embodiments, the SBC precursor is prepared by anionic polymerization using techniques known in the art. Other methods, such as cationic polymerization, may also be used. Anionic polymerization initiators are typically organometallic compounds, such as organolithium compounds, such as ethyl, propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, phenyl, hexylbiphenyl, hexamethylenediyl, butadienyl, isoprene, 1,1-diphenylhexyllithium or polystyryllithium. The amount of initiator required is calculated based on the molecular weight to be achieved, typically 0.002-5wt%, based on the amount of monomer to be polymerized. Suitable solvents for polymerization include aliphatic, cycloaliphatic or aromatic hydrocarbons having 4-12 carbon atoms, such as pentane, hexane, heptane, cyclopentane, cyclohexane, methylcyclohexane, decahydronaphthalene, isooctane, benzene, alkylbenzenes (such as toluene, xylene or ethylbenzene), and mixtures thereof. Polymer chain termination can be achieved by quenching with a proton donor or a compound having a leaving group that can be substituted by a carbon anion polymer chain.
[0031] In some embodiments, the general configuration of the SBC precursor is: ABA, BAB, ABAB, ABABA, (AB)n, (AB)n(A), (ABA)n, (ABA)nX, (AB)nX, (BAB)nX, (ABAB)nX, (ABABA)nX, A'-B'-A', B'-A'-B', A'-B'-A-B', A'-B'-A'-B'-A', (A'-B')n, (A'-B')n(A'), (A'-B'-A')n, (A'-B'-A')nX, (A'-B')nX, (B'-A'-B')n X, (A'-B'-A'-B')nX, (A'-B'-A'-B'-A')nX, (A'-B'-A'-B'-A')nX, or a mixture thereof; wherein n is an integer of 2-30; and X is a coupling agent residue. Each block A and A' are the same or different and independently derived from a vinyl aromatic monomer, and each block B and B' are the same or different and independently derived from a conjugated diene monomer.
[0032] In some embodiments, the coupling agent includes a difunctional or multifunctional compound, such as divinylbenzene, aliphatic or aromatic aliphatic hydrocarbon halides (e.g., 1,2-dibromoethane, bis(chloromethyl)benzene, silicon tetrachloride, dialkyl or diaryl silicon dichloride, alkyl or aryl silicon trichloride, tin tetrachloride), alkyl silicon methoxide, alkyl silicon ethoxide, multifunctional aldehyde (e.g., terephthalic acid dialdehyde), ketone, ester, anhydride or epoxide. In some embodiments, the coupling agent is selected from methyltrimethoxysilane (MTMS), methyltriethoxysilane (MTES), tetramethoxysilane (TMOS), dimethyl adipate, γ-glycidoxypropyltrimethoxysilane, and mixtures thereof.
[0033] In some embodiments, the vinyl aromatic monomer is selected from styrene, p-methylstyrene, p-ethylstyrene, p-n-propylstyrene, p-isopropylstyrene, p-n-butylstyrene, p-sec-butylstyrene, p-isobutylstyrene, p-tert-butylstyrene, isomers of p-decylstyrene, isomers of p-dodecylstyrene, o-substituted styrene, m-substituted styrene, α-methylstyrene, 1,1-diphenylethylene, and mixtures thereof.
[0034] In some embodiments, the conjugated diene monomer is selected from the group consisting of isoprene, 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 1-phenyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 3-butyl-1,3-octadiene, farnesene, myrcene, piperylene, cyclohexadiene, and mixtures thereof.
[0035] In some embodiments, each block A and A' independently has a molecular weight (Mp) of 1-40, or 1-35, or 1-30, or 1-25, or 1-20, or 1-10, or >1, or >2, or <40, or <35, or 25 kg / mol.
[0036] In some embodiments, the vinyl content of block B is ≥70, or >72, or >75, or 70-95, or 70-85, or 75-90, or 70-80 wt %, based on the total weight of polymerized conjugated diene monomers in block B.
[0037] In some embodiments, the vinyl content of block B' is ≤ 50, or 0-50, or 0-45, or < 45 wt %, based on the total weight of polymerized conjugated diene monomers in block B'.
[0038] In some embodiments, each block B and B' independently has a molecular weight (Mp) of 10-300, or 20-200, or 50-200, or 20-150 kg / mol.
[0039] In some embodiments, the polystyrene content (PSC) of the first HSBC is 5-50, or 10-45, or 5-40, or 10-40, or 5-35, or 10-35 wt % based on the total weight of the first HSBC.
[0040] In embodiments where the impact modifier includes both a first HSBC and a second HSBC, the second HSBC independently has a polystyrene content (PSC) of 5-50, or 10-45, or 5-40, or 10-40, or 5-35, or 10-35 wt %, based on the total weight of the second HSBC. In addition, the polystyrene content (PSC) in at least one of the first HSBC or the second HSBC is 15-50, or 15-35, or 18-40 wt %, based on the total weight of each of the first HSBC or the second HSBC.
[0041] In some embodiments, each of the first HSBC and the second HSBC (if present) independently has a molecular weight (Mp) of 10-500, or 20-300, or 50-250, or 20-240, or 40-220 kg / mol.
[0042] In some embodiments, each of the first HSBC and the second HSBC (if present) independently has a melt flow rate (MFR) at 230°C and a load of 2.16 kg of at least 1 dg / min, or >2, or >4, or >5, or 1-40, or 2-30, or 4-35, or 5-35 dg / min, as measured according to ASTM D 1238.
[0043] In some embodiments, the coupling efficiency (CE) of each of the first HSBC and the second HSBC (if present) is >60%, or >65%, or >70%, or 60-98%, or 65-95%.
[0044] In some embodiments, the first HSBC has a diblock content of <15, or <12, or <10, or 1-15, or 1-10 wt % based on the total weight of the first HSBC.
[0045] In some embodiments, each of the first HSBC and the second HSBC (if present) is independently functionalized with at least one functional group, such as a hydroxyl group, an amino group, a carboxyl group, anhydride group, an epoxy group, an isocyanate group, a silanol group, or the like.
[0046] Polyolefin copolymer (POLC)
[0047] The POLC is selected from the group consisting of polyolefin elastomers (POE), polyolefin plastomers (POP), and mixtures thereof.
[0048] In some embodiments, the POE is selected from ethylene-α-olefin copolymers (EOCs), propylene-α-olefin copolymers (POCs), and mixtures thereof. The EOC may be a copolymer of ethylene and at least one C3-C20 α-olefin, and may contain >50, or >60, or >70, or >80, or >90, or 50-90 wt% ethylene, based on the total weight of the EOC. In some embodiments, the POC is a copolymer of propylene and at least one C3-C20 α-olefin, and the POC contains >50, or >60, or >70, or >80, or >90, or 50-90 wt% propylene, based on the total weight of the POC.
[0049] In some embodiments, the POLC is a copolymer of ethylene and at least one C3-C20 α-olefin selected from the group consisting of propylene, isobutylene, 1-butene, 1-hexene, 1-pentene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, and the like.
[0050] The EOC may be selected from ethylene / butene (EB) copolymers, ethylene / hexene-1 copolymers, ethylene / octene copolymers, ethylene / α-olefin / diene modified (EAODM) interpolymers (e.g., ethylene / propylene / diene modified (EPDM) interpolymers, ethylene / propylene / octene terpolymers, etc.), ethylene / propylene copolymers, and the like.
[0051] Examples of POCs include copolymers such as propylene / ethylene, propylene / 1-butene, propylene / 1-hexene, propylene / 4-methyl-1-pentene, propylene / 1-octene, propylene / ethylene / 1-butene, propylene / ethylene / ENB, propylene / ethylene / 1-hexene, propylene / ethylene / 1-octene, propylene / styrene, and propylene / ethylene / styrene.
[0052] In some embodiments, the POE further comprises C4-C18 dienes and / or alkenylbenzenes.
[0053] In some embodiments, the POLC is prepared in a process employing a catalyst selected from a metallocene catalyst (or constrained geometry) or a Ziegler-Natta catalyst.
[0054] In some embodiments, POLC includes two polyolefin copolymer fractions POLC-1 and POLC-2 in suitable amounts, such as 1:10-10:1 or 1:5-5:1. POLC may have a bimodal molecular weight distribution. In some embodiments, the POLC composition has a weight ratio (MW) of the weight average molecular weight of the high molecular weight (HMW) fraction to the weight average molecular weight of the low molecular weight (LMW) fraction of 20-60, or 25-50, or 30-40. w-HMW / M w-LMW Compare).
[0055] In some embodiments, the density of POLC is 0.850-0.920, or 0.853-0.915, 0.855-0.910, or 0.852-0.905 g / cm2 as determined according to ASTM D792. 3 .
[0056] In some embodiments, the POLC has a melt index of 0.5-100, or 1-80, or 5-70, or 5-50, or 5-40 dg / min at 190°C and a load of 2.16 kg as determined according to ASTM D1238.
[0057] In some embodiments, the molecular weight (Mp) of the POLC is 20-400, or 30-350, or 40-300, or 50-400, or 70-350 kg / mol.
[0058] In some embodiments, the polydispersity index (Mw / Mn) of the POLC is 1.7-3.5, or 1.8-3, or 1.8-2.8, or 1.8-2.5.
[0059] In some embodiments, the glass transition temperature (Tg) of the POLC is < -10°C, or < -20°C, or < -30°C, or < -50°C.
[0060] In some embodiments, the melting point of the POLC is >20°C, or >30°C, or 20-140°C, or 25-130°C, or 30-125°C.
[0061] Polyolefin composition
[0062] In some embodiments, the polyolefin composition contains 1-35, or 1-30, or 5-30, or 10-30, or 5-25 wt % of the impact modifier, based on the total weight of the polyolefin composition.
[0063] In some embodiments, the polyolefin composition comprises 65-99 wt% of a polypropylene homopolymer; 1-35 wt% of an impact modifier comprising a first HSBC and a second HSBC in a weight ratio of 1:10-10:1, or a first HSBC and a POLC in a weight ratio of 1:10-10:1, based on the total weight of the composition; and up to 25 wt% of optional additives.
[0064] Optional additives
[0065] The optional additives are selected from activators, curing agents, stabilizers, neutralizers, thickeners, coalescing agents, slip agents, mold release agents, biocides, surfactants, antioxidants, antiozonants, color changing pH indicators, plasticizers, tackifiers, film forming additives, dyes, pigments, UV stabilizers, UV absorbers, catalysts, fillers, other resins, redox couples, fibers, flame retardants, viscosity modifiers, wetting agents, oxygen scavengers, toughening agents, tackifiers, colorants, heat stabilizers, light stabilizers, lubricants, flow modifiers, anti-drip agents, anti-caking agents, antistatic agents, processing aids, stress relief additives, foaming agents, foam nucleating agents, weld strength promoters, and mixtures thereof.
[0066] Examples of fillers include sand, talc, dolomite, calcium carbonate, clay, silica, mica, wollastonite, feldspar, aluminum silicate, aluminum oxide, hydrated aluminum oxide, glass beads, glass microspheres, ceramic microspheres, thermoplastic microspheres, barite, wood flour, glass fiber, wood fiber, carbon fiber, and mixtures thereof. The filler may be surface treated before being added to the polyolefin composition.
[0067] In some embodiments, additives are used in the polyolefin composition at up to 25 wt %, or 0.5-25, or 0.5-20, or 1-15, or 0.5-10, or >0.5, or <20 wt %, based on the total weight of the polyolefin composition.
[0068] In some embodiments, the polyolefin composition comprises 0.5-15, or 1-10, or 3-12 wt% talc, based on the total weight of the polyolefin composition.
[0069] In some embodiments, the polyolefin composition further comprises an impact modifier except the above-mentioned impact modifier.Examples include ethylene-propylene-diene (EPDM) monomer, ethylene-propylene (EPM) monomer, ethylene-propylene rubber (EPR), elastic polyolefin (POE), based on binary copolymers and terpolymers of ethylene and propylene, acrylonitrile-butadiene rubber (NBR), isobutylene (IB), chlorinated rubber, chlorinated polyethylene (CM), isoprene, ethylene-butylene, and mixtures and derivatives thereof.The amount of other impact modifiers (if present) is 0-10, or 0.5-8, or 1-5, or>1, or<10wt%, based on the gross weight of the polyolefin composition.
[0070] Preparation method of impact modifier
[0071] The composition can be prepared by using appropriate amounts of each component and dry blending or dry blending and melt extruding into granules. Dry blending and melt mixing can be performed by a single screw or twin screw extruder.
[0072] Processing method of polyolefin composition / article
[0073] The polyolefin composition can be processed according to methods known in the art, wherein the components are combined and blended by melt mixing / extrusion into pellets and subsequently formed into articles by known techniques, such as injection molding, stretch blow molding, overmolding, rotational molding, thermoforming, casting, extrusion, profile extrusion and blow molding.
[0074] In some embodiments, the polyolefin composition is compounded at any temperature of 80-250° C., or 100-240° C., or 120-220° C., or 150-230° C. The components can be added to each other and compounded in any order or simultaneously. In some embodiments, the additives are added in the form of a premixed masterbatch. The masterbatch can be conveniently formed by a melt compounding process.
[0075] Properties of polyolefin compositions
[0076] The polyolefin composition is characterized by having a balance of flexibility, impact, stiffness, clarity, tensile strength, flow and anisotropy for forming articles.
[0077] The polyolefin composition comprises: A) 65-99 wt% of a polypropylene homopolymer; B) 1-35 wt% of an impact modifier, comprising: a first HSBC and a second HSBC in a weight ratio of 1:10-10:1, or a first HSBC and a POLC in a weight ratio of 1:10-10:1; and C) up to 25 wt% of an additive, based on the total weight of the polyolefin composition, having at least one of the following properties:
[0078] The notched impact of the simply supported beam at 21°C is 28-75, or 28-72, or 29-70, or >28, or >30, or <50 kJ / m 2 ; Simple supported beam notched impact at 0°C is 3-20, 3-18, 3-15, >2 or <15 kJ / m 2 ; and the simply supported beam notched impact at -20°C is 3-10, or 3-8, or 3-6, or >3, or <8 kJ / m 2 ; All of these are measured according to ASTM D610.
[0079] The notched impact strength of the spiral beam at 21°C is 15-50, 16-45, 17-42, >18, or <40 kJ / m 2 ; and the notched impact of the spiral arm beam at -20°C is 2-10, or 2-8, or 3-7, or >2, or <8 kJ / m 2 ; All these are measured according to ISO 180.
[0080] The transmittance is >55%, or >60%, or >63%, or 50-100%, 52-95%, and the haze is <100%, or <98%, or 85-99%, or 88-98%, all of which are measured according to ASTM D1003 using a sample thickness of 3mm.
[0081] The transmittance is >70%, or >75%, or 70-100%, 75-95%, and the haze is <95%, or <90%, or <85%, or <80%, or 60-95%, or 60-90%, or 60-85%, all of which are measured according to ASTM D1003 using a sample thickness of 1.6mm.
[0082] The 1% flexural secant modulus is 700-1200, or 800-1100, or 830-1150, or >800, or >820, or <1150 MPa, measured according to ASTM D790.
[0083] The flexural strength is 25-50, or 25-45, or 26-42, or >25, or <40 MPa, measured according to ASTM D790.
[0084] The tensile modulus is 900-1600, or 920-1550, or 940-1500, or >930, or <1550 MPa, measured according to ISO 527-2.
[0085] The yield stress is 20-35, or 21-32, or 20-30, or >20, or <30 MPa, determined according to ISO 527-2.
[0086] The yield strain is 5-18%, or 6-15%, or >5%, or <15%, as determined according to ISO 527-2.
[0087] The elongation at break is 100-400%, or 110-370%, or 120-350%, or >110%, or <350%, determined according to ISO 527-2.
[0088] In some embodiments, the polyolefin composition has at least one of the following balanced properties compared to a polyolefin composition in the absence of an impact modifier (wherein the transmittance property is determined according to ASTM D1003):
[0089] (i) an increase in 1% flexural secant modulus of >5%, and (ii) a decrease in transmittance measured using a sample thickness of 1.6 mm of <10%; or
[0090] (iii) an increase of >10% in Charpy notched impact measured at 0°C, and (iv) a decrease of <5% in transmittance measured using a sample thickness of 1.6 mm; or
[0091] (v) an increase of >5% in Charpy notched impact measured at 21°C, and (vi) a reduction of <10% in transmittance measured using a sample thickness of 1.6 mm; or
[0092] (vii) an increase of >10% in notched radial impact measured at 21°C, and (viii) a decrease of <5% in transmittance measured using a sample thickness of 1.6 mm; or
[0093] (ix) an increase in yield strain of >10%, and (x) a decrease in transmittance measured with a sample thickness of 1.6 mm of <5%; or
[0094] (xi) an increase in elongation at break of >5%, and (xii) a decrease in transmittance measured with a sample thickness of 1.6 mm of <5%.
[0095] Application of polyolefin compositions
[0096] The polyolefin composition can be used to prepare various articles by injection blow molding, injection molding, extrusion blow molding (EBM), coextrusion, cast film extrusion, blown film extrusion, injection stretch blow molding (ISBM), rotational molding, thermoforming, hot melt, foam blowing, pultrusion, calendering, additive manufacturing or other known processing methods.
[0097] Hollow articles can be formed by continuous extrusion blow molding or intermittent extrusion blow molding of the polyolefin composition. In some embodiments, hollow articles include bottles, containers, fuel tanks, barrels, etc. Other molded articles include furniture, signs, wheels, toys, garden products, etc.
[0098] The polyolefin compositions can be used in pipes, packaging applications, films, geomembranes, roofing applications, pond liners, covers and closures, and core layers of multilayer polyolefin sheets or films, containers and household goods, medical moldings, bottles and caps. The polyolefin compositions can be used in automotive applications such as interior trim, inner jackets, door panels, dashboards, panels, lift gates, and consoles.
[0099] In some embodiments, the polyolefin composition is used to prepare textile fibers, which are then used to form spunbond fibers, staple fibers, multi-fiber yarns, knitted fabrics, woven fabrics, or nonwoven fabrics. Example
[0101] The following examples are non-limiting.
[0102] The components used in the examples include:
[0103] PP-1 is a polypropylene homopolymer having an MFR of 20 dg / min, measured at 230°C and a load of 2.16 kg, from Borealis.
[0104] POLC-1 is an ethylene-octene copolymer with a density of 0.857 g / cm 3 , MI is 10dg / min (190℃ / 2.16kg), Tg is -58℃, and melting temperature is 38℃.
[0105] POLC-2 is an ethylene-octene copolymer with a density of 0.868 g / cm 3 , MI is 10dg / min (190℃ / 2.16kg), Tg is -62℃, and melting temperature is 121℃.
[0106] POLC-3 is an ethylene-hexene copolymer with a density of 0.900 g / cm 3 , MI is 10dg / min (190℃ / 2.16kg).
[0107] Table 1 provides composition details of the first HSBC and the second HSBC. SEBS stands for poly(styrene-ethylene / butylene-styrene) and SEP stands for poly(styrene-ethylene / propylene).
[0108] Table 1
[0109] Examples 1-34
[0110] The polyolefin compositions were prepared by dry blending the components and then compounding in a 25 mm twin extruder using a 5 pound batch size. The melt temperature was maintained at approximately 245° C. The specimens for various determinations were prepared by injection molding with a hold time of approximately 6 seconds and a cooling time of approximately 30 seconds. The polyolefin compositions and mechanical properties of Examples 1-34 are shown in Tables 2-6.
[0111] Table 2 Table 3 Table 4 Table 5 Table 6
[0116] The term "comprising / including" as used herein means including the elements or steps identified after the term, but any such elements or steps are not exhaustive, and embodiments may include other elements or steps. Although the terms "comprising" and "including" have been used herein to describe various aspects, the terms "consisting essentially of" and "consisting of" may replace "comprising" or "including" to provide more specific aspects of the present disclosure, and are also disclosed.
Claims
1. A polyolefin composition comprising: (A) 65 to 99 wt% of a polypropylene homopolymer having a melt flow rate of 0.25 to 100 dg / min, as measured at 230°C and a load of 2.16 kg according to ASTM D1238; (B) 1 to 35 wt% of an impact modifier consisting essentially of: (a) a first hydrogenated styrenic block copolymer having blocks A and blocks B, wherein prior to hydrogenation, each block A is a polymer block of a vinyl aromatic monomer and each block B is a polymer block of a conjugated diene monomer, wherein the vinyl content of block B is from 70 to 95 weight percent, based on the total weight of the conjugated diene monomer polymerized in block B; and (b) at least one polymer selected from the group consisting of: (i) a second hydrogenated styrenic block copolymer having blocks A' and blocks B', wherein prior to hydrogenation, each block A' is a polymer block of a vinyl aromatic monomer and each block B' is a polymer block of a conjugated diene monomer, wherein the vinyl content of block B' is from 0 to 50 weight percent, based on the total weight of the conjugated diene monomer polymerized in block B', and (ii) a polyolefin copolymer having a molecular weight of 0.850-0.920 g / cm2 as measured according to ASTM D792 3 density and a melt index of 0.5-100 dg / min measured at 190°C and a load of 2.16 kg according to ASTM D1238, wherein the weight ratio of (a) to (b) is 1:10-10:1; and (C) up to 25 wt% of at least one additive, based on the total weight of the polyolefin composition; When the at least one polymer is a second hydrogenated styrenic block copolymer, at least one of the first hydrogenated styrenic block copolymer and the second hydrogenated styrenic block copolymer has a polystyrene content of 15 to 50 wt%.
2. The polyolefin composition of claim 1, wherein the polyolefin composition has the following properties when compared to a polyolefin composition in the absence of the impact modifier: (i) an increase in 1% flexural secant modulus of >5%, and (ii) a decrease in transmittance of <10%; or (iii) an increase of >10% in Charpy notched impact, measured at 0°C, and (iv) a decrease of <5% in transmittance; or (v) an increase of >5% in Charpy notched impact strength measured at 21°C, and (vi) a decrease in transmittance of <10%; or (vii) an increase of >10% in notched radial impact strength measured at 21°C, and (viii) a decrease in transmittance of <5%; or (ix) an increase in yield strain of >10%, and (x) a decrease in transmittance of <5%; or (xi) an increase in elongation at break of >5%, and (xii) a decrease in transmittance of <5%; and in, The bending secant modulus at 1% is measured according to ASTM D790, the Charpy notched impact measured at 0°C and the Charpy notched impact measured at 21°C are both measured according to ASTM D610, the Radial notched impact measured at 21°C is measured according to ISO 180, the yield strain is measured according to ISO 527-2, the elongation at break is measured according to ISO527-2, and the transmittance is measured according to ASTM D1003 using a sample thickness of 1.6 mm.
3. The polyolefin composition of any one of claims 1-2, wherein the at least one polymer is a second hydrogenated styrenic block copolymer.
4. The polyolefin composition according to any one of claims 1-2, wherein each block A and A' independently has a molecular weight (Mp) of 1-40 kg / mol, as determined according to ASTM 5296.
5. The polyolefin composition according to any one of claims 1 to 2, wherein block B has a vinyl content of 70 to 85 wt%, and block B' has a vinyl content of 0 to 45 wt%.
6. The polyolefin composition according to any one of claims 1-2, wherein one of the first hydrogenated styrenic block copolymer and the second hydrogenated styrenic block copolymer has a polystyrene content of 15-50 wt%, and the other has a polystyrene content of 5-50 wt%.
7. The polyolefin composition of any one of claims 1-2, wherein the first hydrogenated styrenic block copolymer has a diblock content of < 15 wt%.
8. The polyolefin composition according to any one of claims 1-2, wherein the at least one polymer is a polyolefin copolymer.
9. The polyolefin composition according to claim 8, wherein the polyolefin copolymer has a molecular weight of 0.853-0.915 g / cm 3 density.
10. The polyolefin composition according to claim 8, wherein the polyolefin copolymer has a melt index of 5 to 50 dg / min, measured at 190°C and a load of 2.16 kg.
11. The polyolefin composition of claim 8, wherein the polyolefin copolymer is a copolymer of ethylene and at least one C3-C20 α-olefin selected from the group consisting of propylene, isobutylene, 1-butene, 1-hexene, 1-pentene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, and mixtures thereof.
12. The polyolefin composition according to any one of claims 1-2, wherein the polyolefin composition has the following properties: Charpy notched impact according to ASTM D610: 28-75 kJ / m at 21°C 2 , 3-20kJ / m at 0℃ 2 ,and 3-10 kJ / m at –20°C 2 ;and Notched impact test according to ISO 180: 15-50 kJ / m at 21°C 2 ,and -2-10 kJ / m at 20°C 2 .
13. The polyolefin composition according to any one of claims 1-2, wherein the polyolefin composition has a transmittance > 70% and a haze < 95%, both measured according to ASTM D1003 with a sample thickness of 1.6 mm.
14. The polyolefin composition according to any one of claims 1-2, wherein the polyolefin composition has at least one of the following properties: a 1% flexural secant modulus of 700-1200 MPa, and a flexural strength of 25-50 MPa, both measured according to ASTM D790.
15. The polyolefin composition according to any one of claims 1-2, wherein the polyolefin composition has at least one of the following properties: a tensile modulus of 900-1600 MPa, a yield stress of 20-35 MPa, a yield strain of 5-18%, and an elongation at break of 100-400%; all of which are measured according to ISO 527-2.