High-cold-resistance PVC (polyvinyl chloride) composite material as well as preparation method and application thereof

By using alkyl-substituted aconitic acid monoesters with no more than 5 carbon atoms as plasticizers in PVC, the problems of poor compatibility and insufficient cold resistance of PVC plasticizers are solved, resulting in PVC composite materials with high cold resistance and good toughness, suitable for low-temperature environments.

CN118994808AActive Publication Date: 2024-11-22QINGDAO INST OF BIOENERGY & BIOPROCESS TECH CHINESE ACADEMY OF SCI

Patent Information

Application Number
CN202310580689.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-11-22
Estimated Expiration
2043-05-22

AI Technical Summary

Technical Problem

Existing PVC plasticizers have poor compatibility with PVC, resulting in reduced plasticity and flexibility of PVC, as well as insufficient cold resistance. Traditional plasticizers pose environmental and health hazards and are difficult to improve cold resistance while enhancing plasticity.

Method used

Aconitic acid monoester with alkyl substituents having no more than 5 carbon atoms is used as a plasticizer and scientifically formulated with PVC resin, cold-resistant modifier, lubricant and stabilizer to form a high cold-resistant PVC composite material. The material's toughness, stability and tensile properties are improved through strong support effect and good compatibility.

Benefits of technology

It effectively improves the compatibility and cold resistance of PVC composite materials, reduces the processing difficulty of materials, expands the application fields, and enhances the stability and toughness of materials through synergistic effects, making it suitable for low-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994808A_ABST
    Figure CN118994808A_ABST
Patent Text Reader

Abstract

The invention discloses a high-cold-resistance PVC (polyvinyl chloride) composite material as well as a preparation method and application thereof, and belongs to the technical field of PVC cold-resistant materials. The high-cold-resistant PVC composite material comprises the following components in parts by weight: 100 parts of PVC resin, 5-90 parts of aconitic acid monoester, 1-10 parts of a cold-resistant modifier, 0.5-10 parts of a lubricant and 3-20 parts of a stabilizer, and the Tg of the high-cold-resistant PVC composite material is not greater than 50 DEG C; r in the aconitic acid single ester is alkyl with the carbon atom number not larger than 5. According to the high-cold-resistance PVC composite material, alkyl substituent aconitic acid single ester with the carbon atom number not larger than 5 is adopted as the plasticizer, the compatibility of the plasticizer and PVC is effectively improved, and the composite material has excellent toughness, stability and tensile property and low glass transition temperature (Tg) and is endowed with excellent cold resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a highly cold-resistant PVC composite material and a preparation method and application thereof, belonging to the technical field of PVC cold-resistant materials. Background Art

[0002] PVC is a general-purpose plastic with excellent performance and wide application, but the plasticity of PVC is poor, and plasticizers need to be added to modify it. At present, there are two main plasticization modification methods for PVC: external plasticization and internal plasticization. External plasticization refers to adding plasticizers to PVC by physical blending, and internal plasticization refers to grafting plasticizers onto PVC molecular chains through chemical reactions. Both require good compatibility between plasticizers and PVC to achieve the purpose of improving PVC performance or enhancing certain characteristics.

[0003] Plasticizers mainly increase the plasticity of polymers by weakening the secondary van der Waals forces between polymer molecules, increasing the mobility of polymer molecular chains and reducing crystallinity. Phthalate plasticizers are traditional plastic plasticizers, such as dioctyl phthalate (DOP) and diisodecyl phthalate (DIDP). Their disadvantages are poor compatibility with PVC, poor cold resistance, and migration to the surface of plastic products after long-term use, resulting in reduced application performance of plastic products. Phthalate plasticizers are also harmful to the environment and human health.

[0004] Chinese patent CN102046694A discloses a bio-derived plasticizer for biopolymers, wherein the polyester plasticizer unit is formed by monomers comprising polyfunctional alcohols and aliphatic anhydrides or their equivalent dicarboxylic acids and ester derivatives, which can improve the flexibility of biopolymers without adversely affecting their modulus, but its glass transition temperature is relatively high, so its cold resistance and stability are relatively poor.

[0005] At present, some plasticizers have poor compatibility with PVC, which will also lead to poor plasticity and softness of PVC, making it easier for plasticizers to precipitate from PVC. Therefore, finding a highly compatible plasticizer is an important development direction of plasticizers today. However, some plasticizers with good compatibility are difficult to improve the cold resistance of PVC materials on the basis of improving their plastic properties. Summary of the invention

[0006] In order to solve the above problems, a high cold-resistant PVC composite material is provided. The high cold-resistant PVC composite material adopts a single ester of aconitic acid with an alkyl substituent having a carbon number of not more than 5 as a plasticizer, which effectively improves its compatibility with PVC, is not easy to phase separate when a large amount of plasticizer is added, and makes the composite material have excellent toughness, stability, tensile strength and a low glass transition temperature (T g ), giving the composite material excellent cold resistance.

[0007] According to one aspect of the present application, a highly cold-resistant PVC composite material is provided, which comprises, by weight: 100 parts of PVC resin, 5-90 parts of aconitic acid monoester, 1-10 parts of a cold-resistant modifier, 0.5-10 parts of a lubricant, and 3-20 parts of a stabilizer. The T g Not more than 50℃;

[0008] The structural formula of the aconitic acid single ester is as follows:

[0009]

[0010] Wherein R is an alkyl group having no more than 5 carbon atoms.

[0011] A single ester of aconitic acid is used, and each R substituent in its molecular structure is the same. The same substituent can make aconitic acid ester have uniform compatibility and dispersibility in different systems, and the uniform distribution can make the composite material maintain long-term stability. If R is a different molecular structure at a lower temperature, it will show a more uneven distribution at a lower free volume, resulting in poor local low-temperature performance of the material.

[0012] Preferably, the T of the highly cold-resistant PVC composite material g Not more than 30℃.

[0013] And when R is an alkyl group with a carbon number not greater than 5, it is added to the PVC material system as a plasticizer, and the main structure of its double bond is similar to the benzene ring structure and has strong rigidity. At the same time, under the joint action of three ester groups and the rigid main body on the molecule, the plasticizer plays a huge supporting role between the PVC molecular chains. The powerful supporting effect significantly increases the free volume of the PVC material, and the material must be reduced to the free volume when vitrification is formed at a lower temperature, so the glass transition temperature of the material is significantly reduced, and the low-temperature performance of the PVC composite material is improved. At the same time, the inventor found that the alkyl group with a carbon number not greater than 5 forms a short-chain ester, which has a strong polarity, further enhances the compatibility with the PVC molecular chain and the cold-resistant modifier, and good compatibility is the prerequisite for exerting the supporting effect of the aconitate structure, and only when the aconitate molecule can enter the molecular chain between the PVC molecular chain and the modified cold-resistant agent, the supporting effect of itself can be exerted, so good compatibility and excellent low-temperature resistance are produced by the short-chain ester of aconitate and the main rigid structure in coordination with each other, and both are indispensable. The single ester of aconitic acid used in the present application is a short-chain ester of aconitic acid. Due to its good compatibility, it effectively increases the dosage limit of the plasticizer, so that the composite material achieves higher plasticity. On the one hand, it can effectively reduce the processing difficulty of the material, and on the other hand, it expands the application field and use range of the material.

[0014] Optionally, the acid value of the aconitic acid single ester is less than 0.15 mgKOH / g, the water content is less than 0.2%, and the purity is greater than 97%.

[0015] Optionally, the solubility of the aconitic acid monoester in 100 parts of PVC resin is greater than or equal to 50 parts, the aconitic acid monoester is liquid at 25°C, and the aconitic acid monoester is colorless, transparent or light yellow at 25°C.

[0016] Preferably, the purity of the aconitic acid single ester is not less than 99%, and the chromaticity is not higher than 50Pt-Co.

[0017] The acid value of aconitic acid monoester can ensure that there will not be a large amount of acidic substances in the material during processing to corrode and age the material, and affect the basic performance and internal structure of the material, thereby steadily improving the compatibility and cold resistance of the composite material. The lower moisture content can prevent the phenomenon of insufficient effective ingredients in the material processing, thereby avoiding the material failing to achieve the expected plasticizing effect at the proper addition amount. The higher the purity of aconitic acid monoester, the less impurities therein. If there are too many impurities, the actual addition amount of aconitic acid monoester is smaller and the contact between the aconitic acid monoester and the PVC resin is less, thereby reducing the compatibility of aconitic acid monoester in PVC and improving the T of the composite material. g , thereby reducing the cold resistance. Therefore, the purity of the above-mentioned aconitic acid monoester can further improve the compatibility, plasticity and cold resistance of the aconitic acid monoester in PVC. And the chromaticity of the aconitic acid monoester is not higher than 50Pt-Co, which can reduce the coloring effect of the plasticizer on the PVC material, thereby improving the appearance controllability of the composite material.

[0018] Optionally, the PVC resin has a degree of polymerization of 650-1800, a polydispersity index of 3-5, and a K value of 55-77;

[0019] Preferably, the polydispersity index of the PVC resin is 3.5-4.5.

[0020] When the PVC resin with the above degree of polymerization is used, the obtained PVC material has better toughness because the macromolecular chains are entangled with each other and react with aconitic acid monoester, lubricant and stabilizer components to cross-link to form a stable cross-linked network structure, thereby having better toughness, plasticity, tensile strength and cold resistance.

[0021] The inventors found that when the polydispersity index of the PVC resin used is 3-5, the composite material has the best toughness and plasticity. This may be because when the polydispersity index of the PVC resin is 3-5, the material contains a variety of PVC resins with different molecular weights, and the mixing of resin materials with different molecular weights can better increase the free volume inside the PVC, effectively increase the dissolution amount of the aconitate plasticizer, and can effectively combine to increase the interaction between the plasticizer and the molecular chain, so that the prepared PVC material has high toughness, high stability and plasticity, and good stability, and is not prone to problems such as phase separation.

[0022] Optionally, the cold-resistant modifier is at least one of chlorinated polyethylene (CPE) and ethylene-vinyl acetate copolymer (EVA);

[0023] Preferably, the chlorine content in the chlorinated polyethylene is not less than 25%, and the VA content in the ethylene-vinyl acetate copolymer is 5-40%.

[0024] The inventors found that the cold-resistant modifier itself has a lower T g , such as CPE's T g At around -25℃, the T g At about -34°C, the chlorine content in chlorinated polyethylene is not less than 25%, and the VA content in ethylene-vinyl acetate copolymer is 5-40%. The above substances are added to the composite material as cold-resistant modifiers to effectively improve the cold resistance of PVC. However, the above cold-resistant modifiers are generally compatible with PVC, and the aconitic acid single ester used in this application can play a strong solvent effect, effectively making the cold-resistant modifier and PVC compatible, and promoting uniform mixing between the three. In addition to plasticizing PVC, the aconitic acid single ester also plays a role in increasing the volume of the cold-resistant modifier, so the aconitic acid ester and the cold-resistant modifier play a synergistic role, and the two further improve the low-temperature performance of the PVC composite material.

[0025] Optionally, the lubricant is 2-4 parts;

[0026] The lubricant is at least one of oxidized polyethylene wax, glyceryl stearate, ethylene bisstearamide synthetic wax, paraffin wax and polyethylene wax, preferably ethylene bisstearamide synthetic wax.

[0027] The lubricant can lubricate the PVC resin and aconitic acid monoester, help the aconitic acid monoester to quickly contact the PVC resin, further improve the dispersion speed of the aconitic acid monoester, and the addition of the lubricant can lubricate the molecular chain of the PVC resin, thereby increasing the activity of the molecular chain, thereby promoting the aconitic acid ester to reduce the T of the composite material. g , improve the cold resistance of composite materials.

[0028] Optionally, the stabilizer is 4-7 parts;

[0029] The stabilizer is at least one of a heat stabilizer and a light stabilizer;

[0030] Preferably, the weight ratio of the heat stabilizer to the light stabilizer is 2-10:0.5-4, preferably 3-5:1-2.

[0031] The combination of the above-mentioned light stabilizer and heat stabilizer can enhance the light stability and heat stability of the composite material, thereby improving the light resistance and heat resistance of the composite material and broadening the use temperature range of the composite material.

[0032] Optionally, the heat stabilizer is selected from calcium stearate and zinc stearate in a weight ratio of 0.1-5:1.

[0033] When calcium stearate and zinc stearate in the above weight ratio are used as heat stabilizers, they can work synergistically with light stabilizers to further inhibit the degradation of PVC resin, and the plasticizing effect is enhanced. The reason is that calcium stearate and zinc stearate are easy to disperse and have high compatibility in the system added with short-chain aconitic acid monoester. When the two are used in combination, they can be effectively dispersed in the system without excessive migration. With the aconitic acid monoester of the specific structure, the prepared PVC composite material can have low hardness, high toughness, cold resistance and plasticity.

[0034] Optionally, the light stabilizer is at least one of benzophenone, benzotriazole or triazine;

[0035] The benzophenones include at least one of UV-9, UV-531, UV-356, and UV-284;

[0036] The benzotriazoles include at least one of UV-327, UV-P, UV-320, UV-328, UV-350, UV-326, and UV-234.

[0037] According to another aspect of the present application, a method for preparing the highly cold-resistant PVC composite material described in any one of the above items is provided, comprising the following steps:

[0038] S1: mixing the aconitic acid mixed ester, PVC resin, stabilizer and lubricant to obtain a premix;

[0039] S2: adding the premix to a high-speed mixer, mixing at 30-80° C. for 10-60 min, and then adding the premix to a two-roll mill, mixing at 130-190° C. for 5-20 min to obtain a mixed material;

[0040] S3: placing the mixed material in a flat vulcanizer and vulcanizing it at 140-190° C. and 10-15 MPa for 5-15 min.

[0041] According to another aspect of the present application, the application of any of the above-mentioned highly cold-resistant PVC composite materials is provided, including PVC plastic films used in greenhouses in winter, refrigerator sealing strips, snow boot soles, skis and blood storage bags. The use temperature of the above-mentioned applications is relatively low, generally minus 30°C to 0°C. The composite material prepared in the present application still has the properties of sealing, heat preservation, anti-slip, good softness, etc. at the use temperature, and can meet the requirements of long-term use.

[0042] The beneficial effects of this application include but are not limited to:

[0043] 1. The highly cold-resistant PVC composite material of the present application adopts aconitic acid single ester as a plasticizer. The aconitic acid in the plasticizer is a non-toxic, environmentally friendly bio-acid derived from microbial fermentation. As the main structure, it can improve the plasticizing efficiency of the plasticizer and effectively reduce the use of petrochemical raw materials. The substituent of the aconitic acid single ester is an alkyl group with a carbon number of not more than 5, which can give the aconitic acid ester a higher compatibility, so that it can be better mixed with the material matrix, providing better performance for subsequent products.

[0044] 2. The highly cold-resistant PVC composite material of the present application uses aconitic acid monoester as a plasticizer added to PVC. The macromolecular structure and benzene ring-like structure of the aconitic acid monoester both improve its compatibility with PVC, achieving the effect of highly efficient plasticization of PVC.

[0045] 3. The highly cold-resistant PVC composite material of the present application uses a single ester of aconitic acid containing a large number of short-chain ester parts, which has better compatibility with the PVC molecular chain, effectively improving the dosage limit of the plasticizer, so that the composite PVC material can achieve higher plasticity, which reduces the processing difficulty of the material on the one hand, and expands the application field and use range of the material on the other hand.

[0046] 4. The highly cold-resistant PVC composite material of the present application adopts a specific aconitic acid single ester plasticizer, which has better compatibility with PVC materials compared with traditional plasticizers. It is also used in combination with specific cold-resistant modifiers, stabilizers and lubricants. The scientific proportions of the components work synergistically to effectively enhance the stability, toughness, tensile strength and cold resistance of the composite material, and the composite material has no obvious phase separation under scanning electron microscopy. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0048] Figure 1 is a SEM electron microscope image of the composite material of Example 1;

[0049] Figure 2 is a SEM electron microscope image of the composite material of Example 2;

[0050] Figure 3 is a SEM electron microscope image of the composite material of Example 3;

[0051] Figure 4 This is a SEM electron microscope image of the composite material of Comparative Example 1;

[0052] Figure 5 This is a SEM electron microscope image of the composite material of Comparative Example 2;

[0053] Figure 6 This is a SEM electron microscope image of the composite material of Comparative Example 3;

[0054] Figure 7 This is the SEM electron microscope image of the composite material of Comparative Example 4. DETAILED DESCRIPTION

[0055] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0056] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0057] Example 1

[0058] This embodiment relates to a highly cold-resistant PVC composite material and a preparation method thereof, which comprises, by weight: 100 parts of PVC resin, 50 parts of triethyl aconitate, 5 parts of CPE, 4 parts of heat stabilizer, 1 part of UV-327 light stabilizer, and 1 part of ethylene bisstearamide synthetic wax lubricant, wherein the heat stabilizer is calcium stearate and zinc stearate in a weight ratio of 2:1, the acid value of triethyl aconitate is 0.03 mgKOH / g, the water content is 0.05%, and the purity is 97.5%; the chlorine content of CPE is 30%; the polymerization degree of PVC is 1251-1370, the polydispersity index is 4, and the K value is 71. The structural formula of triethyl aconitate is as follows:

[0059]

[0060] The preparation method of the composite material comprises the following steps:

[0061] S1: mixing triethyl aconitate, PVC resin, stabilizer and lubricant to obtain a premix;

[0062] S2: adding the premix to a high-speed mixer, mixing at 60°C for 40 minutes, and then adding it to a two-roll mill, mixing at 155°C for 20 minutes to obtain a mixed material;

[0063] S3: The mixed material is placed in a flat vulcanizer with a press pressure of 10 MPa and vulcanized at 165°C for 15 minutes. The SEM electron microscope image of the composite material is as follows: Figure 1 shown.

[0064] Example 2

[0065] The difference between this embodiment and embodiment 1 is that tripropyl aconitate is used, and the structural formula of tripropyl aconitate is as follows:

[0066]

[0067] The acid value of the tripropyl aconitate is 0.07 mgKOH / g, the water content is 0.06%, the purity is 98%, and the remaining components and preparation method are the same as those in Example 1. The SEM electron microscope image of the composite material is as follows: Figure 2 shown.

[0068] Example 3

[0069] The difference between this embodiment and embodiment 1 is that tributyl aconitate is used, and the structural formula of tributyl aconitate is as follows:

[0070]

[0071] The acid value of the tributyl aconitate is 0.005 mgKOH / g, the water content is 0.007%, the purity is 99%, and the remaining components and preparation method are the same as those in Example 1. The SEM electron microscope image of the composite material is as follows: Figure 3 shown.

[0072] Example 4

[0073] The difference between this embodiment and embodiment 1 is that trimethyl aconitate is used, and the structural formula of trimethyl aconitate is as follows:

[0074]

[0075] The trimethyl aconitate has an acid value of 0.02 mgKOH / g, a water content of 0.03%, a purity of 98%, and other components and a preparation method are the same as those in Example 1.

[0076] Example 5

[0077] The difference between this embodiment and embodiment 1 is that aconitate tripentyl ester is used, and the structural formula of aconitate tripentyl ester is as follows:

[0078]

[0079] The acid value of the tripentyl aconitate is 0.07 mgKOH / g, the water content is 0.07%, the purity is 97.5%, and the remaining components and preparation method are the same as those in Example 1.

[0080] Example 6

[0081] The difference between this embodiment and embodiment 1 is that triethyl aconitate and tributyl aconitate are used in a weight ratio of 1:1, the parameters of triethyl aconitate and tributyl aconitate are the same as those in embodiment 1 and embodiment 3, and the remaining components and preparation method are the same as those in embodiment 1.

[0082] Example 7

[0083] The difference between this embodiment and embodiment 1 is that the acid value of triethyl aconitate is 1.5 mgKOH / g, and the other components and preparation method are the same as those in embodiment 1.

[0084] Example 8

[0085] The difference between this embodiment and embodiment 1 is that the water content of triethyl aconitate is 2%, and the other components and preparation method are the same as those in embodiment 1.

[0086] Example 9

[0087] The difference between this embodiment and embodiment 1 is that the purity of triethyl aconitate is 90%, and the other components and preparation method are the same as those in embodiment 1.

[0088] Example 10

[0089] The difference between this embodiment and embodiment 1 is that the degree of polymerization of PVC is 1900-1950, and the other components and preparation method are the same as those in embodiment 1.

[0090] Embodiment 11

[0091] The difference between this embodiment and embodiment 1 is that the degree of polymerization of PVC is 450-500, and the other components and preparation method are the same as those in embodiment 1.

[0092] Example 12

[0093] The difference between this embodiment and embodiment 1 is that the polydispersity index of PVC is 5.5, and the other components and preparation method are the same as those in embodiment 1.

[0094] Embodiment 13

[0095] The difference between this embodiment and embodiment 1 is that the polydispersity index of PVC is 2.5, and the other components and preparation method are the same as those in embodiment 1.

[0096] Embodiment 14

[0097] The difference between this embodiment and embodiment 1 is that 1 part of CPE is used, the chlorine content of CPE is 20%, and the other components and preparation method are the same as those in embodiment 1.

[0098] Embodiment 15

[0099] The difference between this embodiment and embodiment 1 is that 10 parts of EVA are used as the cold-resistant modifier, the content of VA in the EVA is 30%, and the other components and preparation method are the same as those in embodiment 1.

[0100] Example 16

[0101] The difference between this embodiment and embodiment 1 is that oxidized polyethylene wax is used as the lubricant, and the other components and preparation method are the same as those in embodiment 1.

[0102] Embodiment 17

[0103] The difference between this embodiment and embodiment 1 is that 2 parts of heat stabilizer and 3 parts of UV-327 light stabilizer are used, and the composition of the heat stabilizer, other components and preparation method are the same as those in embodiment 1.

[0104] Embodiment 18

[0105] The difference between this embodiment and embodiment 1 is that the heat stabilizer is calcium stearate and zinc stearate in a weight ratio of 8:1, and the other components and preparation method are the same as those in embodiment 1.

[0106] Comparative Example 1

[0107] The difference between this comparative example and Example 1 is that dioctyl phthalate is used to replace triethyl aconitate, and the remaining components and preparation method are the same as those in Example 1. The SEM electron microscope image of the composite material is as follows: Figure 4 shown.

[0108] Comparative Example 2

[0109] The difference between this comparative example and Example 1 is that triethyl aconitate is replaced by tri-n-butyl acetyl citrate, and the remaining components and preparation method are the same as those in Example 1. The SEM electron microscope image of the composite material is as follows: Figure 5 shown.

[0110] Comparative Example 3

[0111] The difference between this comparative example and Example 1 is that dibutyl phthalate is used to replace triethyl aconitate, and the remaining components and preparation method are the same as those in Example 1. The SEM electron microscope image of the composite material is as follows: Figure 6 shown.

[0112] Comparative Example 4

[0113] The difference between this comparative example and Example 1 is that dioctyl terephthalate is used to replace triethyl aconitate, and the remaining components and preparation method are the same as those in Example 1. The SEM electron microscope image of the composite material is as follows: Figure 7 shown.

[0114] Comparative Example 5

[0115] The difference between this comparative example and Example 1 is that epoxidized soybean oil is used to replace triethyl aconitate, and the other components and preparation method are the same as those in Example 1.

[0116] Comparative Example 6

[0117] The difference between this comparative example and Example 1 is that triethyl aconitate is replaced by trihexyl aconitate, and the structural formula of trihexyl aconitate is as follows:

[0118] The remaining components and preparation methods are the same as those in Example 1.

[0119] Comparative Example 7

[0120] The difference between this comparative example and Example 1 is that dibutyl-isooctyl aconitate is used to replace triethyl aconitate, and the structural formula of dibutyl-isooctyl aconitate is as follows:

[0121] The remaining components and preparation methods are the same as those in Example 1.

[0122] Comparative Example 8

[0123] The difference between this comparative example and Example 1 is that CPE is not contained, and the other components and preparation method are the same as those of Example 1.

[0124] Comparative Example 9

[0125] The difference between this comparative example and Example 1 is that the amount of triethyl aconitate is 4 parts, and the other components and preparation method are the same as those in Example 1.

[0126] Test Case

[0127] The composite materials prepared in the above examples and comparative examples were tested for performance, and the results are shown in Tables 1 and 2. The test methods are as follows:

[0128] 1. Hardness: Samples were made and tested according to GB / T531-2008 "Indentation hardness test method, Shore durometer method". Three points were selected for each group of samples, each point was measured once, and the median value was taken. The hardness / Shore A in Table 1 is the test result at 25°C, and the A-type durometer was used for the test. The hardness / Shore D in Table 2 is the test result at -5°C, and the D-type durometer was used for the test. In order to facilitate the comparison of the hardness change of the composite material at low temperature, the Shore D hardness actually measured in Table 2 was converted into the hardness / Shore A value in Table 2 according to D=A-50.

[0129] 2.100% tensile stress, elongation at break, elastic modulus: According to GB / T1040-2006 "Plastic Tensile Properties Test", the tensile speed is 50mm / min, the temperature is 25℃, the results are shown in Table 1, and the elastic modulus of the material is tested at -5℃ using the same method, the results are shown in Table 2.

[0130] 3. Compatibility: The water price method is used for testing. Since water molecules are polar, the compatibility of plasticizers with water can characterize the compatibility of plasticizers with polar materials (PVC, PLA and nitrile rubber). When a certain plasticizer has good compatibility with water, it has good compatibility with PVC, and vice versa. In the experiment, 2.5g of plasticizer and 25g of acetone were added to a beaker, and titrated with a burette filled with deionized water, stirring while titrating until turbidity appeared, and the volume of deionized water consumed was recorded.

[0131] 4. Glass transition temperature (T g ): The glass transition temperature was tested by a dynamic mechanical analyzer. The test conditions were: nitrogen as the carrier gas, the test temperature range was -40-80°C, the heating rate was 3°C / min, and the frequency was 1 Hz.

[0132] Table 1

[0133]

[0134]

[0135] Table 2

[0136]

[0137]

[0138] According to the contents of Table 1 and Table 2, the short-chain aconitic acid ester has good compatibility with the material and can maintain a good plasticizing effect at low temperatures. When the aconitic acid index cannot meet the patent requirements, its plasticizing performance, especially the plasticizing performance at low temperatures, will be significantly reduced. In addition, compared with other commonly used commercial plasticizer plasticized composite materials, the PVC material formed by the aconitic acid ester composite used in the present invention has obvious advantages in compatibility and low temperature performance.

[0139] According to the comparison between Example 7 and Example 1, the higher the acid value of aconitic acid single ester, the more acidic substances will be produced in the composite material during processing, thereby corroding and aging the composite material, causing the hardness, 100% tensile stress and elastic modulus of the composite material to increase, and the elongation at break, compatibility and cold resistance to decrease.

[0140] According to the comparison between Example 8 and Example 1, the increase in the water content of aconitic acid monoester will reduce the plasticizing effect of aconitic acid monoester on PVC resin and the synergistic effect with the cold-resistant modifier, so that the hardness, 100% tensile stress and elastic modulus of the composite material increase, but the elongation at break and cold resistance decrease.

[0141] According to the comparison between Example 9 and Example 1, it can be seen that the purity of aconitic acid monoester decreases, and the impurity content introduced into the composite material is higher, so the contact between aconitic acid monoester and PVC and cold-resistant modifier will be reduced, the plasticizing performance of the composite material will be reduced, and the cold resistance will decrease.

[0142] According to the comparison between Examples 10-11 and Example 1, the higher the degree of polymerization of PVC, the higher the hardness, 100% tensile stress and elastic modulus of the composite material, the lower the elongation at break, and the lower the cold resistance. The higher the degree of polymerization, the more the molecular chains are entangled with each other, the lower the mobility of the molecular chains, the smaller the modification of the plasticizer and the cold-resistant modifier on the PVC material, but the compatibility with aconitic acid monoester remains unchanged. Therefore, the degree of polymerization of PVC in the range of 650-1800 can react and cross-link with aconitic acid monoester, cold-resistant modifier, lubricant and stabilizer components to form a stable cross-linked network structure, so that the composite material has better toughness, plasticity, tensile strength and cold resistance.

[0143] According to the comparison between Examples 13-14 and Example 1, the polydispersity index of the PVC resin is in the range of 3-5, which enables PVC resin materials of different molecular weights to contact with aconitic acid monoester, and improves the synergistic effect of aconitic acid monoester and the cold-resistant modifier, thereby effectively improving the toughness and cold resistance of the composite material.

[0144] According to the comparison of Examples 14-15, Comparative Examples 8-9 and Example 1, it can be seen that when no cold-resistant modifier is added, the relative proportion of the plasticizer increases. Although the plasticizing performance increases, the cold resistance of the composite material decreases. The type, parameters and addition amount of the cold-resistant modifier can affect the plasticizing effect of aconitic acid ester on the composite material and change the cold resistance of the composite material. The addition amount of the cold-resistant modifier and the aconitic acid ester can cooperate with each other to achieve the technical effect of 1+1>2.

[0145] According to the comparison between Examples 16-18 and Example 1, the types and ratios of lubricants and heat stabilizers affect the plasticizing effect of aconitic acid ester on the composite material, and also affect the effect of the cold-resistant modifier and aconitic acid ester in synergistically improving the cold resistance of the composite material.

[0146] According to the comparison between Comparative Examples 1-7 and Example 1, it can be seen that the synergistic effect of other types of plasticizers and cold-resistant modifiers is poor. The increase in the number of carbon atoms of R in aconitic acid monoester will reduce the synergistic effect of aconitic acid monoester and the cold-resistant modifier, and reduce the compatibility of aconitic acid monoester with PVC and the plasticizing effect on the composite material.

[0147] The above is only the embodiment of the present application, and the protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.

Claims

1. A highly cold-resistant PVC composite material, characterized in that: The invention comprises, by weight, 100 parts of PVC resin, 1-10 parts of cold-resistant modifier, 5-90 parts of aconitic acid monoester, 0.5-10 parts of lubricant, and 3-20 parts of stabilizer. The T of the high cold-resistant PVC composite material is g Not more than 50℃; The structural formula of the aconitic acid single ester is as follows: Wherein R is an alkyl group having no more than 5 carbon atoms.

2. The highly cold-resistant PVC composite material according to claim 1, characterized in that: The acid value of the aconitic acid single ester is less than 0.15 mgKOH / g, the water content is less than 0.2%, and the purity is greater than 97%.

3. The highly cold-resistant PVC composite material according to claim 1, characterized in that: The PVC resin has a degree of polymerization of 650-1800, a polydispersity index of 3-5, and a K value of 55-77; Preferably, the polydispersity index of the PVC resin is 3.5-4.

5.

4. The highly cold-resistant PVC composite material according to claim 1, characterized in that: The lubricant is 2-4 parts; The lubricant is at least one of oxidized polyethylene wax, glyceryl stearate, ethylene bisstearamide synthetic wax, paraffin wax and polyethylene wax, preferably ethylene bisstearamide synthetic wax.

5. The highly cold-resistant PVC composite material according to claim 1, characterized in that: The stabilizer is 4-7 parts; The stabilizer is at least one of a heat stabilizer and a light stabilizer; Preferably, the weight ratio of the heat stabilizer to the light stabilizer is 2-10:0.5-4, preferably 3-5:1-2.

6. The highly cold-resistant PVC composite material according to claim 5, characterized in that: The heat stabilizer is selected from calcium stearate and zinc stearate in a weight ratio of 0.1-5:

1.

7. The highly cold-resistant PVC composite material according to claim 5, characterized in that: The light stabilizer is at least one of benzophenone, benzotriazole or triazine; The benzophenones include at least one of UV-9, UV-531, UV-356, and UV-284; The benzotriazoles include at least one of UV-327, UV-P, UV-320, UV-328, UV-350, UV-326, and UV-234.

8. The highly cold-resistant PVC composite material according to claim 1, characterized in that: The cold-resistant modifier is at least one of chlorinated polyethylene and ethylene-vinyl acetate copolymer; Preferably, the chlorine content in the chlorinated polyethylene is not less than 25%, and the VA content in the ethylene-vinyl acetate copolymer is 5-40%.

9. The method for preparing the highly cold-resistant PVC composite material according to any one of claims 1 to 8, characterized in that: The steps include: S1: mixing the aconitic acid single ester, PVC resin, stabilizer and lubricant to obtain a premix; S2: adding the premix to a high-speed mixer, mixing at 30-80° C. for 10-60 min, and then adding the premix to a two-roll mill, mixing at 130-190° C. for 5-20 min to obtain a mixed material; S3: placing the mixed material in a flat vulcanizing machine and hot pressing at 140-190° C. and 10-15 MPa for 5-15 min.

10. Application of the highly cold-resistant PVC composite material according to any one of claims 1 to 8, characterized in that: These include PVC plastic film used in greenhouses in winter, refrigerator sealing strips, snow boot soles, skis and blood storage bags.

Citation Information

Patent Citations

  • Aconitate polyvinyl chloride plasticizer, and preparation method and application thereof

    CN113817223A

  • Preparation method of bio-based degradable plasticizer

    CN114315576A

  • Composition containing tributyl aconitate and application thereof

    CN114773748A

  • Aconitate-based plasticizer composition and resin composition including the same

    US20240199846A1

Cited By

  • Electric car cable sheath material and preparation method thereof

    CN120025640A

  • A trolley cable jacket material and method of making the same

    CN120025640B

  • Bio-based trans-aconitate, preparation method therefor and use thereof

    EP4715056A1

  • Bio-based trans-aconitate, preparation method therefor and use thereof

    WO2024235233A1