Polyvinyl chloride (PVC) base material with fire resistance and cable manufactured by using base material
By using a specific fire-resistant PVC substrate, the problem of traditional PVC cables producing a large amount of smoke and drips in fire is solved, and the effect of less smoke and drips is achieved, improving the safety of the fire site.
Patent Information
- Application Number
- CN202411022514.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional PVC cables produce a large amount of thick smoke and drips in fires, causing the fire to spread. The traditional flame retardant method uses halogen compounds to produce harmful gases and harm escapees.
Fire-resistant PVC substrate consisting of PVC resin, recycling cable, epoxy soybean oil, ceramic powder, calcium and zinc stabilizer, ammonium octamolybdate, antioxidant and plasticizer, through specific mixing and treatment methods Prepare cables to avoid the use of halogen compounds and reduce the production of smoke during combustion.
The effect of less smoke and less dripping when the cable is burned in fire situations is achieved, which improves fire resistance, and avoids the production of harmful gases caused by halogen compounds, improving the safety of the fire site.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the field of PVC, and in particular, to a fire-resistant PVC substrate for manufacturing cables, and more particularly, to a fire-resistant PVC substrate and a cable manufactured using the substrate, wherein the cable has good fire resistance and can achieve the effects of less smoke and less dripping in a burning state. Background Art
[0002] Conventional non-environmentally friendly ordinary PVC materials have no flame retardant properties and will burn quickly when encountering flames. In order to make PVC materials have good flame retardant properties, a large amount of halogen compounds (antimony compounds, hydroxides, etc.) are added to the materials in the general process. Although the flame retardant effect is improved, a large amount of halogen harmful gases will be produced in the fire. Most of the victims at the fire scene are actually killed by the thick smoke and toxic substances in the thick smoke. Studies have shown that HC50 concentration / PPM3800 gas concentration can cause fatal coma of escapees; at the same time, the material will produce a large amount of burning drippings during the combustion process, causing the spread of the fire and expanding the fire situation.
[0003] Although the use of the above-mentioned halogen compounds has been avoided in some technologies, the problem of cable materials producing a large amount of thick smoke under high-temperature combustion still exists, especially for cables with PVC as the main material. The results of the IEC 61034-1 / ASTM E662 smoke density test are generally between 30-40, which is far below the low smoke standard. Therefore, how to reduce the smoke generation under combustion conditions or slow down the speed of smoke generation has become a new research and development topic. Summary of the invention
[0004] The present invention aims to overcome the above-mentioned defects and provide a fire-resistant PVC substrate. The cable prepared by using the material has the effect of less smoke in a burning situation compared with the traditional PVC cable.
[0005] The present invention provides a fire-resistant PVC substrate, characterized in that it is made of the following components:
[0006] 100 parts of PVC resin, 1-30 parts of recycled cable, 1-10 parts of epoxy soybean oil, 10-60 parts of ceramic powder, 1-12 parts of calcium zinc stabilizer, 5-25 parts of ammonium octamolybdate, 1-5 parts of antioxidant, and 10-70 parts of plasticizer.
[0007] Among them, the recycled cable is an environmentally friendly cable recycled material in which no halogen compounds are added.
[0008] Furthermore, the present invention provides a fire-resistant PVC substrate, characterized in that:
[0009] The mass ratio of the above PVC resin to the recycled cable is 10:0.5-1.5.
[0010] Furthermore, the present invention provides a fire-resistant PVC substrate, characterized in that:
[0011] The PVC resin used for preparing the environmentally friendly polyvinyl chloride material is selected to have a K greater than 70 and an average degree of polymerization greater than 1200.
[0012] Furthermore, the present invention provides a fire-resistant PVC substrate, characterized in that:
[0013] 100 parts of PVC resin, 5-15 parts of recycled cables, 5-8 parts of epoxy soybean oil, 30-50 parts of ceramic micropowder, 5-8 parts of calcium zinc stabilizer, 9-15 parts of ammonium octamolybdate, 1-2 parts of antioxidant, and 30-60 parts of plasticizer.
[0014] Furthermore, the present invention provides a fire-resistant PVC substrate, characterized in that: its specific preparation method is:
[0015] The other components except ceramic powder and antioxidant are mixed at a temperature of 120°C-130°C for 25-30 minutes, and then ceramic powder and antioxidant are added and mixed for 60-90 seconds to obtain a uniform mixture. The mixture is extruded and granulated, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
[0016] Furthermore, the present invention provides a fire-resistant PVC substrate, characterized in that:
[0017] Preheat the recycled cable to 130-150°C, mix it with 100 parts of PVC resin, cool it to 120-130°C, add other components except ceramic powder and antioxidant, and keep mixing at 120-130°C for 25-30 minutes.
[0018] Furthermore, the present invention provides a fire-resistant PVC substrate, characterized in that:
[0019] 1-5 parts of graphene may also be added.
[0020] Furthermore, the present invention provides a fire-resistant PVC substrate, characterized in that:
[0021] 100 parts of PVC resin, 5-15 parts of recycled cables, 1-3 parts of graphene, 3-5 parts of epoxy soybean oil, 20-40 parts of ceramic micropowder, 2-5 parts of calcium zinc stabilizer, 5-8 parts of ammonium octamolybdate, 1-2 parts of antioxidant, and 20-35 parts of plasticizer.
[0022] Furthermore, the present invention provides a fire-resistant PVC substrate, characterized in that: its specific preparation method is:
[0023] The other components except ceramic powder and antioxidant are mixed at a temperature of 120°C-130°C for 25-30 minutes, and then ceramic powder and antioxidant are added and mixed for 60-90 seconds to obtain a uniform mixture. The mixture is extruded and granulated, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
[0024] Furthermore, the present invention provides a fire-resistant PVC substrate, characterized in that:
[0025] The recycled cables, PVC resin and graphene are irradiated under infrared for more than 10 minutes, and other components except ceramic powder and antioxidant are mixed in, and the mixture is kept at 120℃-130℃ for 25-30 minutes. DETAILED DESCRIPTION
[0026] The present invention can be implemented in many ways and can have various embodiments, but this is not intended to limit the present invention to a specific implementation mode, but should be understood to include all changes, equivalents and even substitutes that fall within the concept and technical scope of the present invention.
[0027] Example 1
[0028] The present embodiment provides a fire-resistant PVC substrate. 5-15 parts of recycled cables are preheated to 130-150°C, mixed with 100 parts of PVC resin, cooled to 120°C-130°C, and then mixed with 5-8 parts of epoxy soybean oil, 5-8 parts of calcium zinc stabilizer, 9-15 parts of ammonium octamolybdate, and 30-60 parts of plasticizer. The mixture is mixed at a temperature of 120°C-130°C for 25-30 minutes, and then 30-50 parts of ceramic micropowder and 1-2 parts of antioxidant are added and the mixture is mixed for 60-90 seconds to obtain a uniform mixture. The mixture is extruded and granulated, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
[0029] The preferred solution is as follows:
[0030] Example 1-1. Fire-resistant PVC substrate 1#
[0031] Preheat 5 parts of recycled cables to 130-150°C, mix with 100 parts of PVC resin, cool to 120-130°C, add 8 parts of epoxy soybean oil, 6 parts of calcium zinc stabilizer, 11 parts of ammonium octamolybdate, and 45 parts of plasticizer, mix at 120-130°C for 25-30 minutes, add 40 parts of ceramic micropowder and 1 part of antioxidant and continue mixing for 60-90S to obtain a uniform mixture, extrude the mixture into granules, and dry the obtained plastic to obtain a fire-resistant PVC substrate.
[0032] Example 1-2. Fire-resistant PVC substrate 2#
[0033] Preheat 10 parts of recycled cables to 130-150°C, mix with 100 parts of PVC resin, cool to 120-130°C, add 8 parts of epoxy soybean oil, 6 parts of calcium zinc stabilizer, 11 parts of ammonium octamolybdate, and 45 parts of plasticizer, mix at 120-130°C for 25-30 minutes, add 40 parts of ceramic micropowder and 1 part of antioxidant and continue mixing for 60-90S to obtain a uniform mixture, extrude the mixture into granules, and dry the obtained plastic to obtain a fire-resistant PVC substrate.
[0034] Example 1-3. Fire-resistant PVC substrate 3#
[0035] Preheat 15 parts of recycled cables to 130-150°C, mix with 100 parts of PVC resin, cool to 120-130°C, add 8 parts of epoxy soybean oil, 6 parts of calcium zinc stabilizer, 11 parts of ammonium octamolybdate, and 45 parts of plasticizer, mix at 120-130°C for 25-30 minutes, add 40 parts of ceramic micropowder and 1 part of antioxidant and continue mixing for 60-90S to obtain a uniform mixture, extrude the mixture into granules, and dry the obtained plastic to obtain a fire-resistant PVC substrate.
[0036] Example 1-4. Fire-resistant PVC substrate 4#
[0037] Preheat 20 parts of recycled cables to 130-150°C, mix with 100 parts of PVC resin, cool to 120-130°C, add 8 parts of epoxy soybean oil, 6 parts of calcium zinc stabilizer, 11 parts of ammonium octamolybdate, and 45 parts of plasticizer, mix at 120-130°C for 25-30 minutes, add 40 parts of ceramic micropowder and 1 part of antioxidant and continue mixing for 60-90S to obtain a uniform mixture, extrude the mixture into granules, and dry the obtained plastic to obtain a fire-resistant PVC substrate.
[0038] Example 1-5. Fire-resistant PVC substrate 5#
[0039] Preheat 30 parts of recycled cables to 130-150°C, mix with 100 parts of PVC resin, cool to 120-130°C, add 8 parts of epoxy soybean oil, 6 parts of calcium zinc stabilizer, 11 parts of ammonium octamolybdate and 45 parts of plasticizer, mix at 120-130°C for 25-30 minutes, add 40 parts of ceramic micropowder and 1 part of antioxidant and continue mixing for 60-90S to obtain a uniform mixture, extrude the mixture into granules, and dry the obtained plastic to obtain a fire-resistant PVC substrate.
[0040] After the IEC 61034-1 / ASTM E662 smoke density test (five repeated tests were performed for each group), the results are as follows:
[0041] serial number Light transmittance 1# 43~49% 2# 45~50% 3# 42~45% 4# 38~43% 5# 35~45%
[0042] Example 1-6. Fire-resistant PVC substrate 6#
[0043] Preheat 15 parts of recycled cables to 130-150°C, mix with 100 parts of PVC resin, cool to 120-130°C, add 5 parts of epoxy soybean oil, 6 parts of calcium zinc stabilizer, 11 parts of ammonium octamolybdate, and 45 parts of plasticizer, mix at 120-130°C for 25-30 minutes, add 40 parts of ceramic micropowder and 1 part of antioxidant and continue mixing for 60-90S to obtain a uniform mixture, extrude the mixture into granules, and dry the obtained plastic to obtain a fire-resistant PVC substrate.
[0044] Example 1-7. Fire-resistant PVC substrate 7#
[0045] Preheat 15 parts of recycled cables to 130-150°C, mix with 100 parts of PVC resin, cool to 120-130°C, add 5 parts of epoxy soybean oil, 8 parts of calcium zinc stabilizer, 11 parts of ammonium octamolybdate, and 45 parts of plasticizer, mix at 120-130°C for 25-30 minutes, add 40 parts of ceramic micropowder and 1 part of antioxidant and continue mixing for 60-90S to obtain a uniform mixture, extrude the mixture into granules, and dry the obtained plastic to obtain a fire-resistant PVC substrate.
[0046] Example 1-8. Fire-resistant PVC substrate 8#
[0047] Preheat 15 parts of recycled cables to 130-150°C, mix with 100 parts of PVC resin, cool to 120-130°C, add 5 parts of epoxy soybean oil, 6 parts of calcium zinc stabilizer, 15 parts of ammonium octamolybdate, and 45 parts of plasticizer, mix at 120-130°C for 25-30 minutes, add 40 parts of ceramic micropowder and 1 part of antioxidant and continue mixing for 60-90S to obtain a uniform mixture, extrude the mixture into granules, and dry the obtained plastic to obtain a fire-resistant PVC substrate.
[0048] Example 1-9. Fire-resistant PVC substrate 9#
[0049] Preheat 15 parts of recycled cables to 130-150°C, mix with 100 parts of PVC resin, cool to 120-130°C, add 5 parts of epoxy soybean oil, 6 parts of calcium zinc stabilizer, 11 parts of ammonium octamolybdate, and 30 parts of plasticizer, mix at 120-130°C for 25-30 minutes, add 40 parts of ceramic micropowder and 1 part of antioxidant and continue mixing for 60-90S to obtain a uniform mixture, extrude the mixture into granules, and dry the obtained plastic to obtain a fire-resistant PVC substrate.
[0050] Example 1-10. Fire-resistant PVC substrate 10#
[0051] Preheat 15 parts of recycled cables to 130-150°C, mix with 100 parts of PVC resin, cool to 120-130°C, add 5 parts of epoxy soybean oil, 6 parts of calcium zinc stabilizer, 11 parts of ammonium octamolybdate, and 60 parts of plasticizer, mix at 120-130°C for 25-30 minutes, add 40 parts of ceramic micropowder and 1 part of antioxidant and continue mixing for 60-90S to obtain a uniform mixture, extrude the mixture into granules, and dry the obtained plastic to obtain a fire-resistant PVC substrate.
[0052] Example 1-11. Fire-resistant PVC substrate 11#
[0053] Preheat 15 parts of recycled cables to 130-150°C, mix with 100 parts of PVC resin, cool to 120-130°C, add 5 parts of epoxy soybean oil, 6 parts of calcium zinc stabilizer, 11 parts of ammonium octamolybdate, and 30 parts of plasticizer, mix at 120-130°C for 25-30 minutes, add 30 parts of ceramic micropowder and 1 part of antioxidant and continue mixing for 60-90S to obtain a uniform mixture, extrude the mixture into granules, and dry the obtained plastic to obtain a fire-resistant PVC substrate.
[0054] Example 1-12. Fire-resistant PVC substrate 12#
[0055] Preheat 15 parts of recycled cables to 130-150°C, mix with 100 parts of PVC resin, cool to 120-130°C, add 5 parts of epoxy soybean oil, 6 parts of calcium zinc stabilizer, 11 parts of ammonium octamolybdate, and 30 parts of plasticizer, mix at 120-130°C for 25-30 minutes, add 50 parts of ceramic micropowder and 1 part of antioxidant and continue mixing for 60-90S to obtain a uniform mixture, extrude the mixture into granules, and dry the obtained plastic to obtain a fire-resistant PVC substrate.
[0056] Example 1-13. Fire-resistant PVC substrate 13#
[0057] 15 parts of recycled cables, 100 parts of PVC resin, 5 parts of epoxy soybean oil, 6 parts of calcium zinc stabilizer, 11 parts of ammonium octamolybdate, and 30 parts of plasticizer are mixed at a temperature of 120°C-130°C for 25-30 minutes, and then 50 parts of ceramic micropowder and 1 part of antioxidant are added and mixed for 60-90 seconds to obtain a uniform mixture. The mixture is extruded and granulated, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
[0058] After the IEC 61034-1 / ASTM E662 smoke density test (five repeated tests were performed for each group), the results are as follows:
[0059]
[0060]
[0061] Example 2
[0062] 5-15 parts of recycled cables, 100 parts of PVC resin and 1-3 parts of 100 parts of graphene are irradiated under infrared for more than 10 minutes, and 3-5 parts of epoxy soybean oil, 2-5 parts of calcium zinc stabilizer, 5-8 parts of ammonium octamolybdate and 20-35 parts of plasticizer are mixed in. After mixing at 120℃-130℃ for 25-30 minutes, 20-40 parts of ceramic micropowder and 1-2 parts of antioxidant are added and mixing is continued for 60-90S to obtain a uniform mixture. The mixture is extruded and granulated, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
[0063] Example 2-1. PVC substrate 14#
[0064] 15 parts of recycled cables, 100 parts of PVC resin, 1 part of graphene, 3 parts of epoxy soybean oil; 5 parts of calcium zinc stabilizer, 6 parts of ammonium octamolybdate, and 25 parts of plasticizer are mixed at 120°C-130°C for 25-30 minutes, and then 30 parts of ceramic micropowder and 1 part of antioxidant are added and mixed for 60-90 seconds to obtain a uniform mixture. The mixture is extruded and granulated, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
[0065] Example 2-2. Fire-resistant PVC substrate 15#
[0066] 15 parts of recycled cables, 100 parts of PVC resin and 1 part of graphene are irradiated under infrared for more than 10 minutes, and then mixed with 3 parts of epoxy soybean oil, 5 parts of calcium zinc stabilizer, 6 parts of ammonium octamolybdate and 25 parts of plasticizer. After mixing at 120℃-130℃ for 25-30 minutes, 30 parts of ceramic micropowder and 1 part of antioxidant are added and mixing is continued for 60-90S to obtain a uniform mixture. The mixture is extruded and granulated, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
[0067] Example 2-3. Fire-resistant PVC substrate 16#
[0068] 10 parts of recycled cables, 100 parts of PVC resin and 1 part of graphene are irradiated under infrared for more than 10 minutes, and then mixed with 3 parts of epoxy soybean oil, 5 parts of calcium zinc stabilizer, 6 parts of ammonium octamolybdate and 25 parts of plasticizer. After mixing at 120℃-130℃ for 25-30 minutes, 30 parts of ceramic micropowder and 1 part of antioxidant are added and mixing is continued for 60-90S to obtain a uniform mixture. The mixture is extruded and granulated, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
[0069] Example 2-5. Fire-resistant PVC substrate 17#
[0070] Irradiate 5 parts of recycled cables, 100 parts of PVC resin and 1 part of graphene under infrared for more than 10 minutes, mix with 3 parts of epoxy soybean oil, 5 parts of calcium zinc stabilizer, 6 parts of ammonium octamolybdate and 25 parts of plasticizer, keep mixing at 120℃-130℃ for 25-30 minutes, then add 30 parts of ceramic micropowder and 1 part of antioxidant and continue mixing for 60-90S to obtain a uniform mixture, extrude the mixture into granules, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
[0071] Example 2-6. Fire-resistant PVC substrate 18#
[0072] Irradiate 25 parts of recycled cables, 100 parts of PVC resin and 1 part of graphene under infrared for more than 10 minutes, mix with 3 parts of epoxy soybean oil, 5 parts of calcium zinc stabilizer, 6 parts of ammonium octamolybdate and 25 parts of plasticizer, keep mixing at 120℃-130℃ for 25-30 minutes, then add 30 parts of ceramic micropowder and 1 part of antioxidant and continue mixing for 60-90S to obtain a uniform mixture, extrude the mixture into granules, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
[0073] Example 2-7. Fire-resistant PVC substrate 19#
[0074] 15 parts of recycled cables, 100 parts of PVC resin and 3 parts of graphene are irradiated under infrared for more than 10 minutes, and then mixed with 3 parts of epoxy soybean oil, 5 parts of calcium zinc stabilizer, 6 parts of ammonium octamolybdate and 25 parts of plasticizer. After mixing at 120℃-130℃ for 25-30 minutes, 30 parts of ceramic micropowder and 1 part of antioxidant are added and mixing is continued for 60-90S to obtain a uniform mixture. The mixture is extruded and granulated, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
[0075] Example 2-8. Fire-resistant PVC substrate 20#
[0076] 15 parts of recycled cables, 100 parts of PVC resin and 3 parts of graphene are irradiated under infrared for more than 10 minutes, and then mixed with 5 parts of epoxy soybean oil, 5 parts of calcium zinc stabilizer, 6 parts of ammonium octamolybdate and 25 parts of plasticizer. After mixing at 120℃-130℃ for 25-30 minutes, 30 parts of ceramic micropowder and 1 part of antioxidant are added and mixing is continued for 60-90S to obtain a uniform mixture. The mixture is extruded and granulated, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
[0077] Example 2-9. Fire-resistant PVC substrate 21#
[0078] 15 parts of recycled cables, 100 parts of PVC resin and 3 parts of graphene are irradiated under infrared for more than 10 minutes, and then mixed with 3 parts of epoxy soybean oil, 2 parts of calcium zinc stabilizer, 6 parts of ammonium octamolybdate and 25 parts of plasticizer. After mixing at 120℃-130℃ for 25-30 minutes, 30 parts of ceramic micropowder and 1 part of antioxidant are added and mixing is continued for 60-90S to obtain a uniform mixture. The mixture is extruded and granulated, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
[0079] Example 2-10. Fire-resistant PVC substrate 22#
[0080] 15 parts of recycled cables, 100 parts of PVC resin and 3 parts of graphene are irradiated under infrared for more than 10 minutes, and then mixed with 3 parts of epoxy soybean oil, 5 parts of calcium zinc stabilizer, 8 parts of ammonium octamolybdate and 25 parts of plasticizer. After mixing at 120℃-130℃ for 25-30 minutes, 30 parts of ceramic micropowder and 1 part of antioxidant are added and mixing is continued for 60-90S to obtain a uniform mixture. The mixture is extruded and granulated, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
[0081] Example 2-11. Fire-resistant PVC substrate 23#
[0082] 15 parts of recycled cables, 100 parts of PVC resin and 3 parts of graphene are irradiated under infrared for more than 10 minutes, and then mixed with 3 parts of epoxy soybean oil, 5 parts of calcium zinc stabilizer, 6 parts of ammonium octamolybdate and 35 parts of plasticizer. After mixing at 120℃-130℃ for 25-30 minutes, 30 parts of ceramic micropowder and 1 part of antioxidant are added and mixing is continued for 60-90S to obtain a uniform mixture. The mixture is extruded and granulated, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
[0083] Example 2-12. Fire-resistant PVC substrate 24#
[0084] 15 parts of recycled cables, 100 parts of PVC resin and 3 parts of graphene are irradiated under infrared for more than 10 minutes, and then mixed with 3 parts of epoxy soybean oil, 5 parts of calcium zinc stabilizer, 6 parts of ammonium octamolybdate and 25 parts of plasticizer. After mixing at 120℃-130℃ for 25-30 minutes, 40 parts of ceramic micropowder and 1 part of antioxidant are added and mixing is continued for 60-90S to obtain a uniform mixture. The mixture is extruded and granulated, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
[0085] After the IEC 61034-1 / ASTM E662 smoke density test (five repeated tests were performed for each group), the results are as follows:
[0086]
[0087]
[0088] The above cables were subjected to breakdown tests using the IEC 60331-1 method (10 parallel tests per group were performed to select the best result), and the results are as follows:
[0089]
[0090]
[0091] Although the above description is centered on the embodiment, it is only an example and does not limit the present invention. It is clear to those skilled in the art that various modifications and applications not illustrated above can be made within the scope of the essential characteristics of the present embodiment. For example, each component specifically shown in the embodiment can be implemented after being modified. Moreover, various differences related to such modifications and applications should be interpreted as being included in the scope of the present invention as defined in the attached claims.
Claims
1. A fire-resistant PVC substrate, characterized in that: Made of the following components: 100 parts of PVC resin, 1-30 parts of recycled cable, 1-10 parts of epoxy soybean oil, 10-60 parts of ceramic micropowder, 1-12 parts of calcium zinc stabilizer, 5-25 parts of ammonium octamolybdate, 1-5 parts of antioxidant, and 10-70 parts of plasticizer. Among them, the recycled cable is an environmentally friendly cable recycled material in which no halogen compounds are added.
2. The fire-resistant PVC substrate according to claim 1, characterized in that: The mass ratio of the PVC resin to the recycled cable is 10:0.5-1.
5.
3. The fire-resistant PVC substrate according to claim 1, characterized in that: The PVC resin used for preparing the environmentally friendly polyvinyl chloride material is selected to have a K greater than 70 and an average degree of polymerization greater than 1200.
4. The fire-resistant PVC substrate according to claim 1, characterized in that: The invention is made of the following components: 100 parts of PVC resin, 5-15 parts of recycled cables, 5-8 parts of epoxy soybean oil, 30-50 parts of ceramic micropowder, 5-8 parts of calcium zinc stabilizer, 9-15 parts of ammonium octamolybdate, 1-2 parts of antioxidant and 30-60 parts of plasticizer.
5. The fire-resistant PVC substrate according to claim 4, characterized in that: Its specific preparation method is: The other components except ceramic powder and antioxidant are mixed at a temperature of 120°C-130°C for 25-30 minutes, and then ceramic powder and antioxidant are added and mixed for 60-90 seconds to obtain a uniform mixture. The mixture is extruded and granulated, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
6. The fire-resistant PVC substrate according to claim 5, characterized in that: Preheat the recycled cable to 130-150°C, mix it with 100 parts of PVC resin, cool it to 120-130°C, add other components except ceramic powder and antioxidant, and keep mixing at 120-130°C for 25-30 minutes.
7. The fire-resistant PVC substrate according to claim 1, characterized in that: 1-5 parts of graphene may also be added.
8. The fire-resistant PVC substrate according to claim 7, characterized in that: Made of the following components: 100 parts of PVC resin, 5-15 parts of recycled cables, 1-3 parts of graphene, 3-5 parts of epoxy soybean oil, 20-40 parts of ceramic micropowder, 2-5 parts of calcium zinc stabilizer, 5-8 parts of ammonium octamolybdate, and 1-2 parts of antioxidant. Plasticizer 20-35 parts.
9. The fire-resistant PVC substrate according to claim 8, characterized in that: Its specific preparation method is: The other components except ceramic powder and antioxidant are mixed at a temperature of 120°C-130°C for 25-30 minutes, and then ceramic powder and antioxidant are added and mixed for 60-90 seconds to obtain a uniform mixture. The mixture is extruded and granulated, and the obtained plastic is dried to obtain a fire-resistant PVC substrate.
10. The fire-resistant PVC substrate according to claim 9, characterized in that: The recycled cables, PVC resin and graphene are irradiated under infrared for more than 10 minutes, and other components except ceramic micropowder and antioxidant are mixed in, and the mixture is kept at 120℃-130℃ for 25-30 minutes.