High-light-transmittance anti-injury super-tough resin and preparation process thereof

By introducing modifiers and wear-resistant agents into the resin material, combined with strict preparation technology, the problems of poor light transmittance and susceptibility to traditional resin materials are solved, and the ultra-strengthymage of high light transmission, scratch resistance and ultraviolet resistance are achieved. Resin material, suitable for high-precision optical devices.

CN118994868APending Publication Date: 2024-11-22JIANGSU XINDA FINE CHEM TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411072146.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional resin materials have poor light transmission, susceptibility and insufficient toughness in some application scenarios, making it difficult to meet performance requirements in modern industry and daily life.

Method used

Using a mixture of PC resin, polyether etherketone and polyimide as modifier, silica nanoparticles as wear resistance, UV-531 as anti-ultraviolet agent, and antioxidants and plasticizers are added to strictly Preparation processes such as drying, mixing, extrusion granulation, injection molding and heat treatment are prepared to produce high-light-transmitting and anti-trauma ultra-tough resin.

Benefits of technology

It achieves high light transmittance (over 99%) of resin lenses, significantly improved scratch resistance (pencil hardness reaches more than 6H) and good UV resistance, extending the service life of the product and improving safety.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-light-transmittance anti-injury super-tough resin and a preparation process of the high-light-transmittance anti-injury super-tough resin. The resin comprises polycarbonate resin, silicon dioxide nanoparticles, an anti-ultraviolet agent UV-531 and a mixture of a modifier polyether-ether-ketone and polyimide. By optimizing the resin formula and strictly controlling the manufacturing process, the light transmittance of the prepared resin lens reaches 99% or above, excellent optical performance is ensured, and the resin lens is suitable for high-precision optical devices. The silicon dioxide nanoparticles are introduced into the resin to serve as the wear-resistant agent, so that the surface hardness of the material is remarkably improved, the pencil hardness test reaches 6H or above, the scratch-proof performance of the lens is effectively improved, and the service life of the product is prolonged. Meanwhile, by adding a mixture of the modifier PC resin, the polyether-ether-ketone and the polyimide, the toughness of the material is improved, the lens is prevented from being broken when being impacted, and the safety and the reliability of the product are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of resin preparation, and more specifically to a highly light-transmitting, damage-proof, super-tough resin and a preparation process thereof. Background Art

[0002] In modern industry and daily life, resin materials are widely used in the manufacture of various products due to their excellent physical and chemical properties. However, with the development of science and technology and the continuous improvement of people's requirements for product performance, traditional resin materials have gradually exposed problems such as poor light transmittance, easy damage and insufficient toughness in certain application scenarios. In order to solve these problems, it is particularly necessary to develop a resin material with high light transmittance, anti-damage properties and super toughness. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the present invention provides a highly light-transmitting, damage-resistant, super-tough resin and a preparation process thereof. The specific scheme is as follows:

[0004] A highly light-transmitting, damage-resistant, ultra-tough resin comprises a mixture of PC resin, polyetheretherketone and polyimide as a modifier, an anti-ultraviolet agent, a wear-resistant agent and an auxiliary agent.

[0005] Furthermore, the addition amount of the modifier is 5% of the PC resin, and the ratio of polyetheretherketone to polyimide is 1:1.

[0006] Furthermore, the anti-wear agent is silicon dioxide nanoparticles, and the added amount is 1% of the PC resin.

[0007] Furthermore, the content of the anti-ultraviolet agent is 1%, and UV-531 is used as the anti-ultraviolet agent.

[0008] Furthermore, the additives include antioxidants and plasticizers; the added amount is 2% of the PC resin.

[0009] A preparation process of a highly light-transmitting, damage-resistant, ultra-tough resin, the preparation process comprising the following steps:

[0010] S1. Pretreatment of raw materials: Dry the selected PC resin at 120°C for 4 hours to ensure that the moisture content is less than 0.1%;

[0011] S2: Add the dried PC resin, 5% modifier, 1.0% UV inhibitor, 1.0% wear inhibitor and 2% additive into a high-speed mixer according to a preset ratio. The mixing time is 20 minutes to ensure that the additives are evenly distributed in the resin matrix.

[0012] S3: The mixed resin material is extruded and granulated through a twin-screw extruder, and the screw speed is 80 rpm to ensure that the material is evenly extruded and formed;

[0013] S4: Add the resin pellets into the injection molding machine, control the injection temperature at 250°C, the injection pressure at 100 MPa, and the injection time at 40 seconds to mold the product in the desired lens shape;

[0014] S5: heat treating the formed lens.

[0015] Furthermore, the heat treatment temperature in S5 is 110° C. and the time is 1.5 h.

[0016] Furthermore, in S3, the extrusion temperature of the twin-screw extruder is controlled to be 230°C.

[0017] Beneficial effects:

[0018] This patent involves a highly transparent, damage-resistant, ultra-tough resin and its preparation process, which has the following significant

[0019] Beneficial effects:

[0020] (1) By optimizing the resin formula and strictly controlling the manufacturing process, the light transmittance of the resin lens reaches more than 99%, ensuring excellent optical performance and suitable for high-precision optical devices. The introduction of silica nanoparticles into the resin as an anti-wear agent significantly improves the surface hardness of the material, with a pencil hardness test of more than 6H, effectively improving the anti-scratch performance of the lens and extending the service life of the product.

[0021] (2) Adding UV-531 anti-ultraviolet agent makes the resin have good anti-ultraviolet ability, avoiding material aging and performance degradation caused by long-term exposure to sunlight.

[0022] (3) By adding a modifier (a mixture of PC resin, polyetheretherketone and polyimide), the toughness of the material is improved, preventing the lens from breaking when impacted, thereby improving the safety and reliability of the product. DETAILED DESCRIPTION

[0023] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.

[0024] Embodiment 1:

[0025] A preparation process of a highly light-transmitting, damage-resistant, ultra-tough resin comprises the following steps:

[0026] (1) Pretreatment of raw materials:

[0027] 1000 g of PC resin was selected and dried at 120° C. for 4 hours to ensure that the moisture content was less than 0.1%.

[0028] (2) Mixing:

[0029] 1000g of dried PC resin, 50g of modifier (25g of polyetheretherketone and 25g of polyimide), 10g of UV-531 anti-ultraviolet agent, 10g of wear-resistant silica nanoparticles, and 20g of additives (antioxidant and plasticizer) were added into a high-speed mixer according to a preset ratio. The mixing time was 20 minutes to ensure that the additives were evenly distributed in the resin matrix.

[0030] (3) Extrusion granulation: The mixed resin material is extruded and granulated through a twin-screw extruder. The extrusion temperature is controlled at 230°C and the screw speed is 80 rpm to ensure that the material is evenly extruded and formed.

[0031] (4) Injection molding: Add the resin pellets into the injection molding machine; the injection molding temperature is controlled at 250°C, the injection molding pressure is 100 MPa, and the injection molding time is 40 seconds to mold the product into the desired lens shape.

[0032] (5) Heat treatment: The molded lens is heat treated at a temperature of 110°C for 1.5 hours.

[0033] Embodiment 2:

[0034] (1) Pretreatment of raw materials: 2000 g of PC resin was selected and dried at 120°C for 4 hours to ensure that the moisture content was less than 0.1%.

[0035] (2) Mixing:

[0036] 2000g of dried PC resin, 100g of modifier (50g of polyetheretherketone and 50g of polyimide), 20g of UV-531 anti-ultraviolet agent, 20g of wear-resistant silica nanoparticles, and 40g of additives (antioxidant and plasticizer) were added into a high-speed mixer according to a preset ratio. The mixing time was 20 minutes to ensure that the additives were evenly distributed in the resin matrix.

[0037] (3) Extrusion granulation:

[0038] The uniformly mixed resin material is extruded and granulated through a twin-screw extruder.

[0039] The extrusion temperature was controlled at 230 °C and the screw speed was 80 rpm to ensure uniform extrusion and molding of the material.

[0040] (4) Injection molding:

[0041] Add resin pellets into the injection molding machine.

[0042] The injection molding temperature is controlled at 250°C, the injection molding pressure is 100 MPa, and the injection molding time is 40 seconds to mold a product of the desired lens shape.

[0043] (5) Heat treatment:

[0044] The molded lens was heat treated at 110°C for 1.5 hours.

[0045] Embodiment 3:

[0046] (1) Pretreatment of raw materials:

[0047] 1500 g of PC resin was selected and dried at 120° C. for 4 hours to ensure that the moisture content was less than 0.1%.

[0048] (2) Mixing:

[0049] 1500g of dried PC resin, 75g of modifier (37.5g of polyetheretherketone and 37.5g of polyimide), 15g of UV-531 anti-ultraviolet agent, 15g of silica nanoparticles, and 30g of additives (antioxidant and plasticizer) were added into a high-speed mixer according to a preset ratio. The mixing time was 20 minutes to ensure that the additives were evenly distributed in the resin matrix.

[0050] (3) Extrusion granulation: The mixed resin material is extruded and granulated through a twin-screw extruder. The extrusion temperature is controlled at 230°C and the screw speed is 80 rpm to ensure that the material is evenly extruded and formed.

[0051] (4) Injection molding: Add the resin pellets into the injection molding machine. The injection molding temperature is controlled at 250°C, the injection molding pressure is 100 MPa, and the injection molding time is 40 seconds to mold the product into the desired lens shape.

[0052] (5) Heat treatment: The molded lens is heat treated at a temperature of 110°C for 1.5 hours.

[0053] The properties of the resin lenses finally obtained in Examples 1 to 3 were tested:

[0054] (1) Light transmittance test:

[0055] The light transmittance at each wavelength was measured using a spectrophotometer, and the average transmittance was calculated.

[0056] (2) Anti-scratch performance test:

[0057] Hardness test: Use a pencil hardness tester to test the surface hardness. The pencil hardness ranges from 6B to 9H.

[0058] Wear test: Under the specified load and friction times, use a wear tester to perform friction, and measure the change in light transmittance before and after friction.

[0059] The data is as follows:

[0060] Embodiment 1:

[0061] Light transmittance greater than 99%

[0062] Anti-scratch performance:

[0063] Hardness test: Pencil hardness reaches 6H

[0064] Wear test: After 500 frictions under 1000g load, the light transmittance decreases by less than 2%

[0065] Embodiment 2:

[0066] Light transmittance greater than 99%

[0067] Anti-scratch performance:

[0068] Hardness test: Pencil hardness reaches 7H

[0069] Wear test: After 500 frictions under a load of 1000g, the light transmittance decreases by less than 1.5%

[0070] Embodiment 3:

[0071] Light transmittance greater than 99%

[0072] Anti-scratch performance:

[0073] Hardness test: Pencil hardness reaches 6.5H

[0074] Wear test: After 500 frictions under a load of 1000g, the light transmittance decreases by less than 1.8%

[0075] The above data show that the modified PC resin lens significantly improves the anti-scratch performance while maintaining high light transmittance.

[0076] As a further improvement, the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A highly light-transmitting, damage-resistant, ultra-tough resin, characterized in that: The resin comprises a mixture of PC resin, polyetheretherketone and polyimide as a modifier, an anti-ultraviolet agent, an anti-wear agent and an auxiliary agent.

2. A highly light-transmitting, damage-resistant, super-tough resin according to claim 1, characterized in that: The amount of modifier added is 5% of PC resin, and the ratio of polyetheretherketone to polyimide is 1:

1.

3. A highly light-transmitting, damage-resistant, super-tough resin according to claim 1, characterized in that: The anti-wear agent is silicon dioxide nanoparticles, and the added amount is 1% of the PC resin.

4. The highly light-transmitting, damage-resistant, super-tough resin according to claim 1, characterized in that: The content of the anti-ultraviolet agent is 1%, and UV-531 is used as the anti-ultraviolet agent.

5. The highly light-transmitting, damage-resistant, super-tough resin according to claim 1, characterized in that: The additives include antioxidants and plasticizers; the added amount is 2% of the PC resin.

6. A process for preparing a highly light-transmitting, damage-resistant, super-tough resin, characterized in that: The preparation process comprises the following steps: S1. Pretreatment of raw materials: Dry the selected PC resin at 120°C for 4 hours to ensure that the moisture content is less than 0.1%; S2: Add the dried PC resin, 5% modifier, 1.0% UV inhibitor, 1.0% wear inhibitor and 2% additive into a high-speed mixer according to a preset ratio. The mixing time is 20 minutes to ensure that the additives are evenly distributed in the resin matrix. S3: The mixed resin material is extruded and granulated through a twin-screw extruder, and the screw speed is 80 rpm to ensure that the material is evenly extruded and formed; S4: Add the resin pellets into the injection molding machine, control the injection temperature at 250°C, the injection pressure at 100 MPa, and the injection time at 40 seconds to mold the product in the desired lens shape; S5: heat treating the formed lens.

7. The process for preparing a highly light-transmitting, damage-resistant, super-tough resin according to claim 6, characterized in that: The heat treatment temperature in S5 is 110°C and the time is 1.5 h.

8. The process for preparing a highly light-transmitting, damage-resistant, super-tough resin according to claim 6, characterized in that: In S3, the extrusion temperature of the twin-screw extruder is controlled to be 230°C.