Thermochromic coating material as well as preparation method and application thereof
By using raw materials such as oxalic acid dihydrate, potassium oxalate, cobalt carbonate, etc., the temperature change temperature range of 105 to 120°C and the significant color change are achieved, and the problem of insufficient color change temperature range in the prior art is solved, satisfying the problem of satisfying the problem of Thermal fault detection requirements of dry transformers, and have excellent performance and low cost characteristics.
Patent Information
- Application Number
- CN202411333212.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-22
AI Technical Summary
The color change temperature range of existing temperature-indicating coatings cannot meet the temperature detection requirements of thermal faults of dry transformers, and the color change effect is not obvious.
Two-component temperature-changing coating material prepared with raw materials such as oxalic acid dihydrate, potassium oxalate, cobalt carbonate and oxidizer. The color changes from dark gray to light purple, which significantly meets the thermal qualities of dry transformers. Defect temperature detection requirements, and have the characteristics of good adhesion performance, excellent electrical resistance and low production cost.
It provides suitable color change temperature range and significant color changes, which are easy to observe and meet the temperature detection requirements of thermal defects in dry transformers. It also has stable performance, excellent weather resistance, simple preparation technology and low production costs.
Smart Images

Figure CN118994960A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermochromic materials, and in particular relates to a thermochromic coating material and a preparation method and application thereof. Background Art
[0002] With the continuous acceleration of urbanization, dry-type transformers play an important role in urban distribution networks. Dry-type transformers have good safety, fire and explosion prevention, strong environmental adaptability, and convenient operation and maintenance. They are particularly suitable for densely populated urban areas and high-rise buildings. However, due to the limitation of overload capacity, their thermal conductivity still has a lot of room for improvement. The temperature rise of the windings during overload operation will further aggravate the insulation degradation process. Once the winding temperature exceeds the insulation tolerance temperature, it will seriously affect the operating life of the dry-type transformer. According to the infrared temperature measurement management standard "Q / YGD.2.06.13-2010", when the temperature of the dry-type transformer is higher than 120℃, the windings and cores of the dry-type transformer will have serious defects, causing transformer failure and affecting the normal operation of power equipment. Therefore, it is of great significance to carry out research on temperature detection of dry-type transformers, which can provide a reference for the diagnosis of thermal faults of dry-type transformers.
[0003] For example, CN115109450A discloses a large-range multi-color irreversible temperature indicating paint and a preparation method thereof. The temperature indicating paint includes the following components: bismuth yellow, neodymium trioxide, praseodymium oxide, sodium molybdate, cerium oxide, sodium fluorosilicate, molybdenum oxide, tungsten trioxide, ammonium tungstate, antimony pentoxide, antimony tungstate, lead chromate, barium chromate, strontium nitrate, nickel oxide, cobalt oxide, sodium zirconium silicate, lithium fluoride, selenium powder, aluminum silicate, aluminum hydroxide, aluminum trioxide, scarlet powder, toluidine purple red, fluorescent red, and permanent red. Although the temperature indicating paint has 9 color changes, the temperature measurement range is 200-1200°C.
[0004] For another example, CN111253861A discloses a high-temperature, multi-color, irreversible temperature-indicating coating for petrochemical equipment and a preparation method thereof. The raw materials of the high-temperature, multi-color, irreversible temperature-indicating coating for petrochemical equipment include the following components: 55-75% silicone resin, 8-20% ultramarine, 0.8-2% thickener, 6-15% filler, and 6-20% organic solvent; when the temperature of the irreversible temperature-indicating coating provided by the invention is between 250 and 300°C, the original color of the paint film becomes dull and dark; when the temperature is between 300 and 350°C, the paint film becomes bluish-gray; when the temperature is between 350 and 400°C, the paint film gradually turns gray; when the temperature is between 400 and 450°C, the paint film finally gradually turns grayish-white.
[0005] For another example, CN118147821A discloses a thermochromic nanofiber membrane, which includes an organic solvent, hard polyurethane particles and a nickel organometallic complex, wherein the metal compound is selected from nickel chloride, nickel bromide, cobalt chloride or cobalt bromide, and the fatty chain is selected from diethylamine hydrochloride, diethylamine hydrobromide, triethylamine hydrochloride or triethylamine hydrobromide, and the color transition temperature of the thermochromic nanofiber membrane is 70-72°C.
[0006] However, the color change temperature ranges of the temperature indicating coatings provided in the above three inventions cannot meet the temperature detection requirements for thermal faults of dry-type transformers.
[0007] Therefore, in response to the above technical problems, it is urgent to develop a thermochromic coating material whose color change temperature range meets the temperature detection requirements of thermal faults of dry-type transformers and has obvious color change effect. Summary of the invention
[0008] In view of the deficiencies in the prior art, the object of the present invention is to provide a thermochromic coating material and a preparation method and application thereof. The color change temperature range of the thermochromic coating material is 105-120°C, which meets the requirements for temperature detection of thermal faults in dry-type transformers, and the color change effect is obvious. At the same time, it also has the characteristics of stable performance, good adhesion performance, excellent hydrophobicity and electrical resistance, low production cost, simple and convenient preparation process, high yield of primary products, etc., which fully meets the requirements for temperature detection of thermal defects in dry-type transformers.
[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides a thermochromic coating material, wherein the thermochromic coating material comprises a thermochromic material and a base paint;
[0011] The raw materials of the thermochromic material include oxalic acid dihydrate, potassium oxalate, cobalt carbonate, an oxidant and a pH regulator.
[0012] The thermochromic coating material provided by the present invention is a two-component material, including a thermochromic material and a base paint. When used, the two are directly mixed and coated on the surface of a dry-type transformer, and then left to dry. The raw materials for preparing the thermochromic material include dihydrated oxalic acid, potassium oxalate, cobalt carbonate, an oxidant and a pH adjuster. The coating material obtained by mixing the thermochromic material obtained by matching the above raw materials with the base paint can change color between 105 and 120° C. The color change process is from dark gray to light purple. The color change effect is very obvious and easy to observe, that is, the color change temperature range meets the requirements for thermal defect temperature detection of dry-type transformers. In addition, the thermochromic coating material also has the characteristics of good adhesion performance, good electrical resistance, excellent weather resistance, simple and convenient preparation process, low production cost and high product yield. It will not affect the normal operation of the equipment when applied on the surface of the equipment, and is suitable for thermal defect temperature detection of dry-type transformers.
[0013] In the present invention, the "color change temperature range is 105-120°C" and "color change can occur between 105 and 120°C" both mean that when the temperature of the thermochromic material reaches 105°C, the color of the coating formed therein will change, and between 105 and 120°C, the color of the coating will gradually change with the increase of temperature; at the same time, the above color changes can be observed by naked eye.
[0014] The thermochromic material and base paint contained in the thermochromic coating material provided by the present invention need to be stored separately. The two are directly mixed before use and then coated on the surface of the dry-type transformer. When the dry-type transformer reaches the fault temperature, the temperature-indicating coating coated on the surface will change color, which can effectively reflect the abnormal heating phenomenon of the dry-type transformer under test.
[0015] Preferably, the mass ratio of the thermochromic material to the base paint is (1-5):10, for example, 1:10, 1.5:10, 2:10, 2.5:10, 3:10, 3.5:10, 4:10, 4.5:10 or 5:10, etc.
[0016] Preferably, the raw materials of the thermochromic material include the following components in parts by weight:
[0017]
[0018]
[0019] Wherein, the content of potassium oxalate can be 15 parts by weight, 20 parts by weight, 40 parts by weight, 60 parts by weight, 80 parts by weight, 100 parts by weight, 120 parts by weight, 140 parts by weight, 160 parts by weight, 180 parts by weight or 200 parts by weight, etc.
[0020] The content of the cobalt carbonate may be 50 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight or 100 parts by weight, etc.
[0021] The content of the oxidant may be 50 parts by weight, 55 parts by weight, 60 parts by weight, 65 parts by weight, 70 parts by weight, 75 parts by weight, 80 parts by weight, etc.
[0022] The content of the pH adjuster can be 40 parts by weight, 42 parts by weight, 44 parts by weight, 46 parts by weight, 48 parts by weight, 50 parts by weight, 52 parts by weight, 54 parts by weight, 56 parts by weight, 58 parts by weight or 60 parts by weight, etc.
[0023] Preferably, the oxidizing agent comprises lead dioxide.
[0024] Preferably, the pH adjuster comprises glacial acetic acid.
[0025] Preferably, the base paint comprises an anti-fouling flashover composite coating.
[0026] Preferably, the anti-pollution flashover composite coating is a colorless and transparent anti-pollution flashover composite coating. The colorless and transparent anti-pollution flashover composite coating has the characteristics of durability and in-situ forming, and also has excellent hydrophobicity and balanced hydrophobic migration, thereby ensuring that in severe weather (for example, in a moderate rain environment), a continuous water film will not be generated on the coating surface formed by the thermochromic coating material; in addition, the colorless and transparent anti-pollution flashover composite coating has excellent electrical insulation properties, good flame retardant properties, strong adhesion, acid and alkali resistance, UV resistance and good self-cleaning properties. At the same time, the colorless and transparent characteristics do not affect the color development of the thermochromic material, and can avoid the influence of the base paint color on the color change of the thermochromic material.
[0027] In a second aspect, the present invention provides a method for preparing the thermochromic coating material as described in the first aspect, the preparation method comprising providing a base paint and preparing the thermochromic material;
[0028] The preparation of the thermochromic material comprises the following steps:
[0029] (1) mixing oxalic acid dihydrate and potassium oxalate in water to obtain a mixed solution;
[0030] (2) adding cobalt carbonate to the mixed solution obtained in step (1) to carry out double decomposition reaction, then adding an oxidant to carry out oxidation reaction, then adding a pH adjuster to mix, letting stand, filtering by suction, and collecting the filtrate;
[0031] (3) adding anhydrous ethanol to the filtrate obtained in step (2) for crystallization, and filtering to obtain the thermochromic material.
[0032] The preparation method of the thermochromic material provided by the present invention comprises four steps: firstly, dissolving oxalic acid dihydrate (H2C2O4·2(H2O)) and potassium oxalate (K2C2O4) in water to obtain a mixed solution, which provides C2O4 for subsequent reactions; 2- and acidic environment; then add cobalt carbonate (CoCO3) to the above mixture for double decomposition reaction to generate cobalt oxalate (CoC2O4), and then add an oxidant for oxidation reaction to generate Co 2+ Oxidation to Co 3+ , and then adding a pH regulator to provide an acidic environment can promote the formation of a complex; finally, adding anhydrous ethanol can crystallize to obtain K3[Co(C2O4)3]·H2O, which is the thermochromic material.
[0033] Preferably, the mixing temperature in step (1) is 60-70°C, for example, 60°C, 62°C, 64°C, 66°C, 68°C or 70°C.
[0034] Preferably, the mixing time in step (1) is 20 to 40 minutes, for example, 20 minutes, 22 minutes, 25 minutes, 27 minutes, 30 minutes, 33 minutes, 35 minutes, 38 minutes or 40 minutes.
[0035] Preferably, the mixing in step (1) is carried out under stirring conditions at a rotation speed of 400 to 900 r / min (e.g., 400 r / min, 450 r / min, 500 r / min, 550 r / min, 600 r / min, 650 r / min, 700 r / min, 750 r / min, 800 r / min, 850 r / min or 900 r / min, etc.).
[0036] Preferably, the temperature of the metathesis reaction in step (2) is 60-70°C, for example, 60°C, 62°C, 64°C, 66°C, 68°C or 70°C.
[0037] Preferably, the time of the metathesis reaction in step (2) is 10 to 30 min, for example, 10 min, 12 min, 14 min, 16 min, 18 min, 20 min, 22 min, 24 min, 26 min, 28 min or 30 min.
[0038] Preferably, the temperature of the oxidation reaction in step (2) is 20-30°C, for example, 20°C, 22°C, 24°C, 26°C, 28°C or 30°C.
[0039] Preferably, the oxidation reaction time in step (2) is 10 to 30 min, for example, 10 min, 12 min, 15 min, 17 min, 20 min, 22 min, 25 min, 27 min or 30 min.
[0040] Preferably, the mixing temperature in step (2) is room temperature.
[0041] Preferably, the standing time in step (2) is 60 to 80 min, for example, 60 min, 62 min, 65 min, 67 min, 70 min, 72 min, 75 min, 77 min or 80 min.
[0042] Preferably, the filtration time in step (2) is 5 to 10 min, for example, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min.
[0043] Preferably, based on 50 parts by weight of the oxalic acid dihydrate, the amount of the anhydrous ethanol in step (3) is 100-150 parts by weight, for example, 100 parts by weight, 105 parts by weight, 110 parts by weight, 115 parts by weight, 120 parts by weight, 125 parts by weight, 130 parts by weight, 135 parts by weight, 140 parts by weight, 145 parts by weight or 150 parts by weight, etc.
[0044] Preferably, the crystallization time in step (3) is 20 to 40 min, for example, 20 min, 22 min, 25 min, 27 min, 30 min, 32 min, 35 min, 37 min or 40 min.
[0045] Preferably, step (3) further includes a drying step after the filtration.
[0046] Preferably, the drying temperature is 50-60°C, for example, 50°C, 52°C, 54°C, 56°C, 58°C or 60°C.
[0047] Preferably, the drying time is 24 to 48 hours, for example, 24 hours, 30 hours, 36 hours, 42 hours or 48 hours.
[0048] In a third aspect, the present invention provides a dry-type transformer, the surface of which is coated with the thermochromic coating material as described in the first aspect.
[0049] In a fourth aspect, the present invention provides an application of the dry-type transformer as described in the third aspect in a distribution network.
[0050] Compared with the prior art, the present invention has the following beneficial effects:
[0051] (1) The thermochromic coating material provided by the present invention includes a thermochromic material and a base paint. The raw materials of the thermochromic material include dihydrated oxalic acid, potassium oxalate, cobalt carbonate, an oxidant and a pH adjuster. The thermochromic material and the base paint of the above-mentioned specific raw materials are matched to make the obtained thermochromic coating material have a suitable color change temperature range (105-120°C), and when the temperature reaches 120°C, the color change is very obvious, which is easy to observe and meets the requirements for temperature detection of thermal defects of dry-type transformers.
[0052] (2) In addition, the thermochromic coating material provided by the present invention also has the characteristics of good adhesion performance, stable performance, good electrical resistance, excellent weather resistance, simple and convenient preparation process, low production cost and high product yield. It will not affect the normal operation of the equipment when coated on the surface of the equipment, and is suitable for the detection of thermal defects in dry-type transformers. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 Pictures of the coating formed by the thermochromic coating material provided in Example 1 at different temperatures;
[0054] Figure 2 This is an infrared spectrum of the coating formed by the thermochromic coating material provided in Example 1 before and after color change. DETAILED DESCRIPTION
[0055] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0056] Unless otherwise specified, the raw materials involved in the following specific embodiments are all conventional materials in the art and can be purchased from commercial products.
[0057] In particular, the colorless and transparent anti-pollution flashover composite coating used was purchased from Hebei Zhonglian Huayu Electric Power Technology Co., Ltd., with the brand name of RTV-Ⅱ.
[0058] Example 1
[0059] A thermochromic coating material, comprising a base paint and a thermochromic material in a mass ratio of 10:3;
[0060] The base paint is a colorless and transparent anti-fouling flashover composite paint, and the raw materials for preparing the thermochromic material include the following components in parts by weight:
[0061]
[0062] The preparation method of the thermochromic material comprises the following steps:
[0063] (1) Weighing oxalic acid dihydrate and potassium oxalate into a beaker, adding an appropriate amount of deionized water to completely dissolve the two, and then using a heat-collecting magnetic stirrer to heat the oil bath at 60° C., stirring at a speed of 400 r / min, and controlling the stirring time to 20 min to obtain a completely transparent mixed solution;
[0064] (2) Weigh cobalt carbonate and slowly add it to the mixed solution obtained in step (1), continue stirring and mixing at 60° C. and 400 r / min for 30 min, lower the heating temperature of the oil bath to room temperature, slowly add lead dioxide and react for 30 min, then add glacial acetic acid and mix, let stand at room temperature for 60 min, then filter and obtain a dark green filtrate;
[0065] (3) adding anhydrous ethanol to the filtrate obtained in step (2), crystallizing for 20 minutes, filtering to obtain a filter residue, and drying the filter residue in a constant temperature heating box at 50° C. for 24 hours to obtain a thermochromic coating material.
[0066] Example 2
[0067] A thermochromic coating material, comprising a base paint and a thermochromic material in a mass ratio of 10:4;
[0068] The base paint is a colorless and transparent anti-fouling flashover composite paint, and the raw materials for preparing the thermochromic material include the following components in parts by weight:
[0069]
[0070] The preparation of the thermochromic material is described in Example 1.
[0071] Example 3
[0072] A thermochromic coating material, comprising a base paint and a thermochromic material in a mass ratio of 10:2;
[0073] The base paint is a colorless and transparent anti-fouling flashover composite paint, and the raw materials for preparing the thermochromic material include the following components in parts by weight:
[0074]
[0075] The preparation of the thermochromic material is described in Example 1.
[0076] Example 4
[0077] A thermochromic coating material, comprising a base paint and a thermochromic material in a mass ratio of 10:4;
[0078] The base paint is a colorless and transparent anti-fouling flashover composite paint, and the raw materials for preparing the thermochromic material include the following components in parts by weight:
[0079]
[0080] The preparation of the thermochromic material is described in Example 1.
[0081] Example 5
[0082] A thermochromic coating material, comprising a base paint and a thermochromic material in a mass ratio of 10:2;
[0083] The base paint is a colorless and transparent anti-fouling flashover composite paint, and the raw materials for preparing the thermochromic material include the following components in parts by weight:
[0084]
[0085] The preparation of the thermochromic material is described in Example 1.
[0086] Example 6
[0087] A thermochromic coating material, which differs from Example 1 only in that it comprises a base paint and a thermochromic material in a mass ratio of 10:0.5, and other substances, amounts and preparation methods are the same as those in Example 1.
[0088] Example 7
[0089] A thermochromic coating material, which differs from Example 1 only in that it comprises a base paint and a thermochromic material in a mass ratio of 10:6, and other substances, amounts and preparation methods are the same as those in Example 1.
[0090] Comparative Example 1
[0091] A thermochromic coating material, which differs from Example 1 only in that no oxalic acid dihydrate is added to the raw materials for preparing the thermochromic material, and other substances, amounts and preparation methods are the same as those in Example 1.
[0092] Comparative Example 2
[0093] A coating material, which differs from Example 1 only in that it is only a base paint, and other substances, dosages and preparation methods are the same as those in Example 1.
[0094] Appearance Characterization:
[0095] (1) Visual observation: The thermochromic coating material provided in Example 1 was coated on an epoxy resin glass fiber board and dried at 25° C. for 24 h to form a coating. The color of the coating at room temperature, heated to 105° C., 110° C., and 120° C. was observed with the naked eye, and recorded with a Nikon D750 camera. Pictures of the thermochromic coating provided in Example 1 at different temperatures were obtained as shown in FIG. Figure 1 As shown;
[0096] from Figure 1 It can be seen that when the temperature of the coating formed by the thermochromic coating material provided in Example 1 reaches 105°C, the color of the coating formed will change, and between 105 and 120°C, the color of the coating will gradually change with the increase of temperature, from dark gray to light purple.
[0097] (2) Infrared spectrum: The coating formed by the thermochromic coating material provided in Example 1 was tested at room temperature and 120° C. using an infrared tester to obtain infrared spectra of the coating formed by the thermochromic coating material provided in Example 1 at different temperatures. Figure 2 As shown;
[0098] from Figure 2 It can be seen that when the temperature of the coating formed by the thermochromic coating material provided in Example 1 reaches 120° C., its light transmittance changes, which indirectly confirms that the color of the coating changes.
[0099] In addition, the colors of the coatings formed by the coating materials provided in other embodiments and comparative examples at different temperatures were recorded using a Nikon D750 camera, and the final results were statistically summarized in Table 1:
[0100] Table 1
[0101]
[0102] From the data in Table 1, we can see that:
[0103] Analysis of Example 1 shows that the coating discoloration temperature range is 105-120°C, the color changes from dark gray to light purple, the discoloration effect is obvious, and the discoloration is irreversible.
[0104] From the analysis of Example 1 and Examples 2 to 3, it can be seen that a reasonable increase in the amount of potassium oxalate has little effect on the color, and the coating can also undergo obvious color change within the temperature range of 105 to 120°C.
[0105] Analysis of Example 1 and Examples 4-5 shows that increasing the amount of cobalt carbonate will advance the color change temperature by about 5-10°C, and the colors at 110°C and 120°C are basically the same.
[0106] From the analysis of Example 1 and Examples 6 to 7, it can be seen that increasing the proportion of the thermochromic material will cause the color of the coating to darken both initially and after the color change, while reducing the proportion of the thermochromic material will cause the color of the coating to lighten both initially and after the color change, and the color change effect will be less obvious.
[0107] Analysis of Example 1 and Comparative Example 1 shows that if no oxalic acid dihydrate is added to the raw materials for preparing the thermochromic material, the coating will not have the ability to change color. The reason is that oxalic acid provides an acidic environment and oxalate ions for the preparation of the thermochromic material. When no oxalic acid dihydrate is added, C2O4 2- Insufficient content of K + and Co 2+ Excess, in the environment of acetic acid, excess Co 2+ It undergoes a redox reaction with lead dioxide to produce impurities such as lead acetate, potassium acetate, and cobalt acetate, resulting in an extremely low content of K3[Co(C2O4)3]·3H2O in the final product, which has no color-changing ability.
[0108] From the analysis of Example 1 and Comparative Example 2, it can be seen that without adding the thermochromic material, the coating will not have the ability to change color.
[0109] Performance Test:
[0110] (1) Adhesion: The test is conducted using a crosshatch knife in accordance with the GB / T 9286-2021 Crosshatch test for paints and varnishes.
[0111] (2) Weather resistance: The test was conducted in accordance with the standard GB / T 11026.1-2016 Heat resistance of electrical insulating materials Part 1: Aging procedures and evaluation of test results. The heat aging time was set to 168 h. A Nikon D750 camera was used to photograph the surface discoloration of the coating before and after heat aging, and the color difference ΔE of the coating before and after aging was extracted. The larger the color difference value, the more serious the aging degree.
[0112] (3) Voltage resistance: With reference to GB / T1408.1-2016 / IEC60243-1:2013 standard, a slow voltage rise test method was adopted with a voltage rise rate of 0.5 kV / s to obtain the surface flashover voltage of the coating.
[0113] (4) Thermal conductivity: Refer to GB / T32064-2015 and ISO22007-2:2008 standards and use DRE-III thermal conductivity tester to measure the thermal conductivity of the coating.
[0114] The coating materials provided in Examples 1 to 7 and Comparative Examples 1 to 2 were tested according to the above test method. The test results are shown in Table 2:
[0115] Table 2
[0116]
[0117] From the data in Table 2, we can see that:
[0118] Analysis of Example 1 shows that the adhesion performance of the coating is level 1, the color difference after high temperature aging for 168 hours is 1.417 NBS, the surface flashover voltage is 9.35 kV / cm, and the thermal conductivity is 0.47986 W / (m·K).
[0119] From the analysis of Example 1 and Examples 2 to 3, it can be seen that as the ratio of potassium oxalate is increased, the color difference of the coating becomes larger after high-temperature aging, that is, the weather resistance decreases slightly, and as the base paint content increases, the adhesion of the coating decreases significantly, and the surface flashover voltage and thermal conductivity both show a trend of first increasing and then decreasing, and both reach the maximum when the ratio is 10:3.
[0120] From the analysis of Example 1 and Examples 4 to 5, it can be seen that as the proportion of cobalt carbonate is increased, the color difference of the coating gradually increases after aging, the weather resistance gradually decreases, and the adhesion performance, surface flashover voltage and thermal conductivity are not much different from those of Examples 2 to 3, indicating that the color-changing material has little effect on the above-mentioned properties of the coating, and the proportion has a greater impact.
[0121] From the analysis of Example 1 and Examples 6 to 7, it can be seen that as the proportion of the thermochromic material is increased, the adhesion performance of the coating is further reduced and the weather resistance gradually deteriorates.
[0122] Analysis of Example 1 and Comparative Example 1 shows that if no oxalic acid dihydrate is added to the raw materials for preparing the thermochromic material, the coating will not have the ability to change color, and the color difference does not change much after high-temperature aging, indicating that the coating basically does not change color before and after aging. The other properties of the coating are not much different from those of Example 1, further indicating that the color-changing material has little effect on the coating's electrical resistance and thermal conductivity and other properties.
[0123] Analysis of Example 1 and Comparative Example 2 shows that without adding the thermochromic material, the coating will not have the ability to change color, the adhesion and thermal conductivity of the coating will reach the optimal level, and the surface discharge voltage will be slightly reduced.
[0124] The applicant declares that the present invention illustrates a thermochromic material and its preparation method and application through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A thermochromic coating material, characterized in that: The thermochromic coating material comprises a thermochromic material and a base paint; The raw materials of the thermochromic material include oxalic acid dihydrate, potassium oxalate, cobalt carbonate, an oxidant and a pH regulator.
2. The thermochromic coating material according to claim 1, characterized in that: The mass ratio of the thermochromic material to the base paint is (1-5):
10.
3. The thermochromic coating material according to claim 1 or 2, characterized in that: The raw materials of the thermochromic material include the following components in parts by weight: Preferably, the oxidant comprises lead dioxide; Preferably, the pH adjuster comprises glacial acetic acid.
4. The thermochromic coating material according to any one of claims 1 to 3, characterized in that: The base paint includes an anti-fouling flashover composite coating; Preferably, the anti-pollution flashover composite coating is a colorless and transparent anti-pollution flashover composite coating.
5. A method for preparing the thermochromic coating material according to any one of claims 1 to 4, characterized in that: The preparation method comprises providing a base paint and preparing a thermochromic material; The preparation of the thermochromic material comprises the following steps: (1) mixing oxalic acid dihydrate and potassium oxalate in water to obtain a mixed solution; (2) adding cobalt carbonate to the mixed solution obtained in step (1) to carry out double decomposition reaction, then adding an oxidant to carry out oxidation reaction, and finally adding a pH adjuster to mix, standing and filtering, and collecting the filtrate; (3) adding anhydrous ethanol to the filtrate obtained in step (2) for crystallization, and filtering to obtain the thermochromic material.
6. The preparation method according to claim 5, characterized in that: The mixing temperature in step (1) is 60-70° C. Preferably, the mixing time in step (1) is 20 to 40 minutes; Preferably, the mixing in step (1) is carried out under stirring conditions at a rotation speed of 400 to 900 r / min.
7. The preparation method according to claim 5 or 6, characterized in that: The temperature of the metathesis reaction in step (2) is 60-70° C. and the time is 10-30 min; Preferably, the temperature of the oxidation reaction in step (2) is 20 to 30° C. and the time is 10 to 30 min; Preferably, the mixing temperature in step (2) is room temperature; Preferably, the standing time in step (2) is 60 to 80 minutes; Preferably, the filtration time in step (2) is 5 to 10 minutes.
8. The preparation method according to any one of claims 5 to 7, characterized in that: Based on 50 parts by weight of the oxalic acid dihydrate, the amount of anhydrous ethanol in step (3) is 100 to 150 parts by weight; Preferably, the crystallization time in step (3) is 20 to 40 minutes; Preferably, step (3) further comprises a drying step after the filtration; Preferably, the drying temperature is 50-60°C; Preferably, the drying time is 24 to 48 hours.
9. A dry-type transformer, characterized in that: The surface of the dry-type transformer is coated with the thermochromic coating material according to any one of claims 1 to 4.
10. Use of the dry-type transformer according to claim 9 in a power distribution network.
Citation Information
Patent Citations
Reversible temperature indicating coating as well as preparation method and application thereof
CN116285693A
Reversible color-changing coating as well as preparation method and application thereof
CN116285694A