Silicon carbide polishing solution containing two-dimensional material
By introducing abrasives combined with α-alumina into the silicon carbide polishing liquid, the problems of low efficiency and scratches of silicon carbide polishing liquid during SiC surface treatment are solved, significantly improving the polishing quality and rate, and achieving more Efficient surface smoothing.
Patent Information
- Application Number
- CN202411129604.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
The existing silicon carbide polishing liquid is inefficient during processing and is prone to scratches, making it difficult to obtain a flat and scratch-free surface, especially because the abrasives of hard materials have poor stability during SiC surface treatment.
A two-dimensional material is introduced as abrasive in the silicon carbide polishing liquid, combined with α-alumina, and the polishing efficiency and surface quality are improved through the alternating action of chemical mechanical polishing.
By introducing two-dimensional materials, the polishing quality, polishing rate and surface smoothness are significantly improved, and the low efficiency and scratch problems of traditional polishing liquid during SiC surface treatment are overcome, and it has good application prospects.
Smart Images

Figure BDA0004997437490000031 
Figure BDA0004997437490000041 
Figure BDA0004997437490000051
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polishing liquids, and in particular relates to a silicon carbide polishing liquid containing two-dimensional materials. Background Art
[0002] SiC is the main third-generation semiconductor material and a high-temperature ceramic material with two significant characteristics: high hardness (Mohs hardness and chemical inertness). Chemical mechanical polishing technology is the only means to achieve global flatness in silicon carbide substrate processing. This process is specially designed to obtain a surface that is both flat and free of scratches and impurities. SiC material has high hardness, and the friction removal efficiency of ordinary hardness abrasives on SiC is low; moreover, the sharp edges of the abrasives are easily passivated by the hard SiC, the polishing efficiency decays rapidly over time, and the process stability is poor. At present, silicon carbide polishing liquid mainly uses superhard materials such as aluminum oxide or zirconium oxide as abrasives. The characteristics of this abrasive are fast removal rate, but it is particularly easy to cause scratches. Silicon carbide chemical mechanical polishing is a technology that combines chemical and mechanical actions. Its process is quite complicated and there are many influencing factors. At present, permanganate is mainly used as an oxidant to generate a relatively easy-to-remove soft layer under catalytic oxidation. Then, the soft layer is removed under the mechanical action of the abrasive in the polishing liquid and the polishing pad, so that the surface of the workpiece is exposed again, and then a chemical reaction is carried out. In this way, the surface of the workpiece is polished in the alternating chemical and mechanical processes. The polishing mechanism combining mechanical friction with conventional chemical corrosion encounters a serious bottleneck in the processing of hard and inert SiC, and it is urgent to innovate SiC polishing routes and explore basic research. Faced with the challenges of low SiC polishing efficiency and particularly easy scratches under superhard abrasives, scholars and industry practitioners at home and abroad have carried out extensive and in-depth basic research and exploration.
[0003] α-alumina is used as an abrasive, mainly due to its high hardness, to cut the oxide layer on the surface of silicon carbide, but this type of polishing liquid can easily cause scratches and excessive roughness on the surface. Therefore, it is necessary to find a new abrasive that can further reduce the roughness and further improve the efficiency of the subsequent fine polishing process. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a silicon carbide polishing liquid containing two-dimensional material. By introducing two-dimensional material into the abrasive, the polishing quality (including crystallization performance), polishing rate and polishing surface of the polishing liquid are also greatly improved, and it has good application prospects.
[0005] The present invention provides a silicon carbide polishing liquid containing a two-dimensional material, which comprises the following components by weight percentage:
[0006] Liquid carrier: 70%-95%;
[0007] Abrasive: 0.01%-10%;
[0008] Oxidant: 0.01%-5%;
[0009] pH adjuster: 0.01%-0.5%;
[0010] The abrasive includes α-aluminum oxide and a two-dimensional material or is only a two-dimensional material.
[0011] Preferably, the liquid carrier is water.
[0012] Preferably, the particle size range of the α-alumina is 80nm-2um, more preferably 100nm-0.5um, most preferably 150nm-0.3um.
[0013] Preferably, the two-dimensional material includes one or more of graphene oxide, boron nitride, molybdenum disulfide, tungsten disulfide, molybdenum diselenide, tungsten diselenide, and MXene materials; the particle size range of the two-dimensional material is 50nm-5um, more preferably 100nm-2um, and most preferably 0.3um-1um.
[0014] Preferably, the oxidant comprises one or more of chlorate, perchlorate, inorganic peroxide, nitrate, permanganate, ferrate, metal cation, sodium perborate, potassium perborate, chloric acid, chlorous acid, chloric acid, perchloric acid, bromic acid, perbromic acid, iodic acid, periodic acid, hypochlorite, chlorite, bromate, perbromate, and iodate.
[0015] Preferably, the pH adjuster includes one or more of an organic acid, an inorganic acid, an organic base, an inorganic base, a weak acid or a hydrolyzed salt of a weak base.
[0016] Preferably, the organic acid includes one or more of sulfonic acid, sulfinic acid, and thiocarboxylic acid.
[0017] Preferably, the inorganic acid includes one or more of hydrochloric acid, nitric acid, boric acid, sulfuric acid, carbonic acid, and phosphoric acid, more preferably phosphoric acid or nitric acid, and most preferably nitric acid.
[0018] Preferably, the organic base includes one or more of methylamine, dimethylamine and trimethylamine.
[0019] Preferably, the inorganic base includes one or more of sodium hydroxide, potassium hydroxide, barium hydroxide, calcium hydroxide, aluminum hydroxide, lithium hydroxide, magnesium hydroxide, zinc hydroxide, copper hydroxide, iron hydroxide, lead hydroxide, cobalt hydroxide, chromium hydroxide, zirconium hydroxide, nickel hydroxide, and ammonium hydroxide, more preferably potassium hydroxide.
[0020] Preferably, the hydrolyzed salt of the weak acid or weak base includes one or more of copper nitrate, copper chloride, copper sulfate, aluminum nitrate, aluminum sulfate, aluminum chloride, ferric nitrate, ferric sulfate, ferric chloride, zinc nitrate, zinc chloride, zinc sulfate, nickel nitrate, nickel sulfate, nickel chloride, calcium nitrate, calcium chloride, calcium sulfate, potassium silicate, sodium silicate, lithium silicate, sodium phosphate, potassium phosphate, sodium metaaluminate, potassium metaaluminate, sodium aluminate, potassium aluminate, sodium borate, potassium borate, sodium arsenate, potassium arsenate, sodium selenate, potassium selenate, sodium tellurate, and sodium tellurate.
[0021] Preferably, the polishing material targeted by the polishing liquid is an insulating silicon carbide wafer, a doped silicon carbide wafer (N-type silicon carbide or P-type silicon carbide) or a silicon carbide film. The crystal form of the silicon carbide wafer can be 3C-SiC, 4H-SiC, 6H-SiC, or other stable crystal forms.
[0022] Preferably, the polishing pad used in the polishing liquid is made of non-woven fabric or polyurethane.
[0023] Beneficial Effects
[0024] The present invention introduces two-dimensional materials into the abrasive, so that the polishing quality (including crystallization performance), polishing rate and polishing surface of the polishing liquid are greatly improved, and has good application prospects. DETAILED DESCRIPTION
[0025] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0026] Example 1
[0027] Alumina abrasives of different particle sizes are mixed with graphene oxide of different particle sizes, and oxidants and pH regulators of different concentrations are added, and stirred evenly for polishing.
[0028] 1:5wt%0.15umAl 2 O 3 +1wt%0.3um graphene oxide+3wt%KMnO 4 + 0.1wt%KOH;
[0029] 2: 5wt% 0.15umAl 2 O 3 +1wt% 0.5um graphene oxide +3wt% KMnO 4 + 0.1wt%KOH;
[0030] 3:5wt%0.15umAl 2 O 3 +1wt%1um graphene oxide+3wt%KMnO 4 + 0.1wt%KOH;
[0031] 4:5wt%0.15umAl 2 O 3 +1wt% 0.3um graphene oxide +3wt% KMnO 4 + 0.1wt%NaOH;
[0032] 5:5wt%0.3umAl 2 O 3 +1wt% 0.3um graphene oxide +3wt% KMnO 4 + 0.1wt%KOH;
[0033] 6: 5wt% 0.5umAl 2 O 3 +1wt% 0.3um graphene oxide +3wt% KMnO 4 + 0.1wt%KOH;
[0034] 7: 5wt% 0.15umAl 2 O 3 +3wt%KMnO 4 + 0.1wt%KOH;
[0035] 8: 5wt% 0.3um graphene oxide + 3wt% KMnO 4 + 0.1wt%KOH;
[0036] 9: 5wt% 0.5um graphene oxide + 3wt% KMnO 4 + 0.1wt%KOH;
[0037] 10: 5wt% 2um graphene oxide + 3wt% KMnO 4 + 0.1 wt% KOH.
[0038] Polishing experiment: This polishing experiment uses a CP-4 machine, and a 4-inch silicon carbide wafer (N-type SiC, Si surface) is attached to the polishing head through wax. The polishing parameters are set as follows: SUBA800 polishing pad; polishing pressure is 6psi; polishing pad speed is 100rpm; polishing sheet speed is 10-rpm; polishing liquid flow rate is 125mL / min for recycling; polishing time is 60min. After each polishing, the polishing pad is repaired for 5 minutes with a 4-inch diamond repair disk, and the polished sheet is ultrasonically cleaned in the cleaning liquid for 10 minutes and then blown dry with nitrogen. The results are listed in Table 1.
[0039] Table 1 Experimental results statistics
[0040]
[0041]
[0042] It can be seen from the data in Table 1 that under the condition of the same particle size of aluminum oxide, the introduction of graphene oxide improves the surface quality; the smaller the aluminum oxide, the higher the surface quality.
[0043] Example 2
[0044] Super-hard abrasive-alumina of different particle sizes and different contents are mixed with graphene oxide of different particle sizes, and different concentrations and types of oxidants and pH adjusters are added, and stirred evenly for polishing.
[0045] Polishing experiment: This polishing experiment uses a CP-4 machine, and a 4-inch silicon carbide wafer (N-type SiC, Si surface) is glued to the polishing head through wax. The polishing parameters are set as follows: SUBA800 polishing pad; polishing pressure is 6psi; polishing pad speed is 100rpm; polishing sheet speed is 90rpm; polishing liquid flow rate is 125mL / min for recycling; polishing time is 60min. After each polishing, the polishing pad is repaired for 5 minutes with a 4-inch diamond repair disk. The polished sheet is ultrasonically cleaned in the cleaning solution for 10 minutes and then blown dry with nitrogen. The results are listed in Table 2.
[0046] A.5wt%0.15umAl 2 O 3 +1wt%0.3um graphene oxide+3wt%KMnO 4 +0.1wt% calcium nitrate;
[0047] B.5wt%0.15umAl 2 O 3 +1wt%0.3um graphene oxide+3wt%KMnO 4 + 0.1wt% ferric nitrate;
[0048] C.5wt%0.15umAl 2 O 3 +1wt%0.3um graphene oxide+1wt%KMnO 4 + 0.1wt%KOH;
[0049] D.5wt%0.15umAl 2 O 3 +1wt% 0.3um graphene oxide +2wt% KMnO 4 + 0.1wt%KOH;
[0050] E.5wt% 0.3um graphene oxide + 3wt% KMnO 4 +0.1wt% calcium nitrate;
[0051] F.5wt% 0.3um graphene oxide + 3wt% KMnO 4 + 0.1wt% ferric nitrate;
[0052] G.5wt% 0.3um graphene oxide + 3wt% sodium perchlorate + 0.1wt% KOH;
[0053] H.5wt% 0.3um graphene oxide + 3wt% sodium hypochlorite + 0.1wt% KOH.
[0054] Table 2 Experimental results statistics
[0055]
[0056]
[0057] It can be seen from the data in Table 2 that after the introduction of graphene oxide, different pH adjusters will affect the surface quality. Iron nitrate is the best under acidic conditions, and KOH is the best under alkaline conditions. Potassium permanganate is the best oxidant. The higher the concentration of potassium permanganate, the faster the removal rate.
[0058] In summary, the polishing liquid of the present invention effectively overcomes various shortcomings in the prior art and has high industrial utilization value.
[0059] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A silicon carbide polishing liquid containing two-dimensional material, characterized in that: Calculated by weight percentage, it includes the following components: liquid phase carrier: 70%-95%; Abrasive: 0.01%-10%; Oxidant: 0.01%-5%; pH adjuster: 0.01%-0.5%; The abrasive includes α-aluminum oxide and a two-dimensional material or is only a two-dimensional material.
2. The silicon carbide polishing liquid containing two-dimensional material according to claim 1, characterized in that: The liquid carrier is water.
3. The silicon carbide polishing liquid containing two-dimensional material according to claim 1, characterized in that: The particle size of the α-alumina is in the range of 80nm-2um.
4. The silicon carbide polishing liquid containing two-dimensional material according to claim 1, characterized in that: The two-dimensional material includes one or more of graphene oxide, boron nitride, molybdenum disulfide, tungsten disulfide, molybdenum diselenide, tungsten diselenide, and MXene materials; the particle size range of the two-dimensional material is 50nm-5um.
5. The silicon carbide polishing liquid containing two-dimensional material according to claim 1, characterized in that: The oxidant includes one or more of chlorate, perchlorate, inorganic peroxide, nitrate, permanganate, ferrate, metal cation, sodium perborate, potassium perborate, chloric acid, chlorous acid, chloric acid, perchloric acid, bromic acid, perbromic acid, iodic acid, periodic acid, hypochlorite, chlorite, bromate, perbromate, and iodate.
6. The silicon carbide polishing liquid containing two-dimensional material according to claim 1, characterized in that: The pH regulator includes one or more of an organic acid, an inorganic acid, an organic base, an inorganic base, a weak acid or a hydrolyzed salt of a weak base.
7. The silicon carbide polishing liquid containing two-dimensional material according to claim 6, characterized in that: The organic acid includes one or more of sulfonic acid, sulfinic acid, and thiocarboxylic acid; the inorganic acid includes one or more of hydrochloric acid, nitric acid, boric acid, sulfuric acid, carbonic acid, and phosphoric acid; the organic base includes one or more of methylamine, dimethylamine, and trimethylamine; the inorganic base includes sodium hydroxide, potassium hydroxide, barium hydroxide, calcium hydroxide, aluminum hydroxide, lithium hydroxide, magnesium hydroxide, zinc hydroxide, copper hydroxide, iron hydroxide, lead hydroxide, cobalt hydroxide, chromium hydroxide, zirconium hydroxide, nickel hydroxide, and ammonium hydroxide. one or more of; the hydrolyzed salt of the weak acid or weak base includes one or more of copper nitrate, copper chloride, copper sulfate, aluminum nitrate, aluminum sulfate, aluminum chloride, ferric nitrate, ferric sulfate, ferric chloride, zinc nitrate, zinc chloride, zinc sulfate, nickel nitrate, nickel sulfate, nickel chloride, calcium nitrate, calcium chloride, calcium sulfate, potassium silicate, sodium silicate, lithium silicate, sodium phosphate, potassium phosphate, sodium metaaluminate, potassium metaaluminate, sodium aluminate, potassium aluminate, sodium borate, potassium borate, sodium arsenate, potassium arsenate, sodium selenate, potassium selenate, sodium tellurate, and sodium tellurate.
8. The silicon carbide polishing liquid containing two-dimensional material according to claim 1, characterized in that: The polishing material targeted by the polishing liquid is an insulating silicon carbide wafer, a doped silicon carbide wafer or a silicon carbide film.
9. The silicon carbide polishing liquid containing two-dimensional material according to claim 1, characterized in that: The polishing pad used in the polishing liquid is made of non-woven fabric or polyurethane.
Citation Information
Cited By
Silicon carbide substrate rough polishing composition as well as preparation method and application thereof
CN120966368A