Silane modified composite electrochromic material and preparation method thereof

The preparation method of silane-modified composite electrochromic materials solves the problems of instability and poor effect of existing electrochromic materials, and improves the stability and color change effect of the materials, thus extending their service life.

CN118995193APending Publication Date: 2024-11-22深圳豪威显示科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411091388.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing electrochromic materials suffer from instability and poor performance during preparation, especially the simple combination of organic and inorganic materials fails to fully utilize their respective advantages.

Method used

The preparation method of silane-modified composite electrochromic material involves mixing a silane coupling agent with an aqueous ethanol solution, adjusting the pH value, and then stirring and heating the mixture with tungsten trioxide, polyaniline, triphenylamine, crystal violet lactone, and other materials. The mixture is then washed with water and vacuum dried to form a tightly connected organic and inorganic material structure.

Benefits of technology

It improves the stability and color change effect of electrochromic materials, expands the color change range, and extends the performance and cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995193A_ABST
    Figure CN118995193A_ABST
Patent Text Reader

Abstract

The invention discloses a silane modified composite electrochromic material which comprises a silane coupling agent, an ethanol water solution, tungsten trioxide, polyaniline, triphenylamine, 3, 3-bis (4-dimethylaminophenyl)-6-dimethylaminophenyl peptide, a solvent and a catalyst. The preparation process of the silane modified composite electrochromic material is convenient and efficient, tight connection of organic and inorganic materials is guaranteed through silane modification, the use stability of the prepared electrochromic material is improved, the color change effect is improved, the color change range is wide, the use performance is improved, and the cycle service life is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrochromic materials, in particular to a silane-modified composite electrochromic material and a preparation method thereof. Background Art

[0002] Electrochromic materials refer to the phenomenon that the optical properties (reflectivity, transmittance, absorptivity, etc.) of materials undergo stable and reversible color changes under the action of an external electric field, which is manifested in the reversible changes of color and transparency. Materials with electrochromic properties are called electrochromic materials, but the preparation of existing electrochromic materials still has certain defects, such as:

[0003] The application number of CN201010232235.5 is “A method for preparing an organic-inorganic electrochromic film”. This method is just a simple combination of organic and inorganic materials and cannot give full play to their respective advantages. Therefore, it will lead to problems of instability and poor effect. Summary of the invention

[0004] The object of the present invention is to provide a silane-modified composite electrochromic material and a preparation method thereof, so as to solve the problem that the electrochromic material prepared by the existing method proposed in the above background technology is unstable and has poor effect.

[0005] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a silane-modified composite electrochromic material, comprising a silane coupling agent, an ethanol aqueous solution, tungsten trioxide, polyaniline, triphenylamine, 3,3-bis(4-dimethylaminophenyl)-6-dimethylaminophenyl peptide, a solvent and a catalyst.

[0006] As a preferred technical solution of the present invention, the silane coupling agent is one of vinyl triethoxy silane, vinyl trimethoxy silane and vinyl trisilane.

[0007] A method for preparing a silane-modified composite electrochromic material comprises the following steps:

[0008] Step 1: Stir and mix the silane coupling agent and the ethanol aqueous solution to prepare a modified liquid, and adjust the pH value;

[0009] Step 2: Mix tungsten trioxide, polyaniline, triphenylamine and crystal violet lactone, and then add solvent and catalyst and continue to stir and mix;

[0010] Step 3: Add the modified liquid to the mixture in step 2, and heat and stir to mix;

[0011] Step 4: Wash the mixture in step 3 repeatedly with water and filter;

[0012] Step 5: Heat and dry the mixture after washing and filtering in step 4 under vacuum to obtain a finished product.

[0013] As a preferred technical solution of the present invention, in step 1, the silane coupling agent accounts for 2-5% of the mass of the modified liquid.

[0014] As a preferred technical solution of the present invention, in the step 2, tungsten trioxide, polyaniline, triphenylamine, and crystal violet lactone are reacted at a stirring speed of 500 to 800 rpm for 10 to 15 minutes, then allowed to stand for 5 to 8 minutes, and after adding a solvent and a catalyst, the mixture is reacted at a stirring speed of 600 to 1000 rpm for 20 to 30 minutes.

[0015] As a preferred technical solution of the present invention, in the step three, after adding the modifying liquid, the reaction is carried out at a stirring speed of 1500-2000 rpm for 5-10 minutes and heated to 50-60°C, then the stirring speed is reduced to 800-1000 rpm and the reaction is carried out for 30-50 minutes, and then naturally cooled.

[0016] As a preferred technical solution of the present invention, in step 4, deionized water is used for washing 3 to 6 times.

[0017] As a preferred technical solution of the present invention, in step 5, the drying temperature is controlled to be 90-100° C. and the drying time is 3-5 hours.

[0018] Compared with the prior art, the beneficial effects of the present invention are: the preparation process of the silane-modified composite electrochromic material is convenient and efficient, and the close connection between organic and inorganic materials is ensured through silane modification, thereby improving the stability of the prepared electrochromic material, improving the color change effect, widening the color change range, and improving the performance and cycle life. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a graph showing the color change test results of the silane-modified composite electrochromic material of the present invention;

[0020] Figure 2 This is a graph showing the cycle test results of the silane-modified composite electrochromic material of the present invention. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Embodiment 1

[0023] The technical solution of the present invention: a silane-modified composite electrochromic material and a preparation method thereof, comprising an alkane coupling agent, an ethanol aqueous solution, tungsten trioxide, polyaniline, triphenylamine, 3,3-bis(4-dimethylaminophenyl)-6-dimethylaminophenyl peptide, a solvent and a catalyst;

[0024] The silane coupling agent is one of vinyl triethoxysilane, vinyl trimethoxysilane and vinyl trisilane;

[0025] A method for preparing a silane-modified composite electrochromic material comprises the following steps:

[0026] Step 1: Stir and mix the silane coupling agent and the ethanol aqueous solution to prepare a modified liquid, and adjust the pH value;

[0027] Step 2: Mix tungsten trioxide, polyaniline, triphenylamine and crystal violet lactone, and then add solvent and catalyst and continue to stir and mix;

[0028] Step 3: Add the modified liquid to the mixture in step 2, and heat and stir to mix;

[0029] Step 4: Wash the mixture in step 3 repeatedly with water and filter;

[0030] Step 5: Heat and dry the mixture after washing and filtering in step 4 under vacuum to obtain a finished product.

[0031] Wherein the silane coupling agent in step 1 accounts for 2% of the mass of the modified liquid;

[0032] In step 2, tungsten trioxide, polyaniline, triphenylamine, and crystal violet lactone are reacted at a stirring speed of 500 rpm for 15 minutes, then allowed to stand for 5 minutes, and then a solvent and a catalyst are added and reacted at a stirring speed of 600 rpm for 30 minutes;

[0033] In step 3, after adding the modified liquid, the mixture was stirred at 1500 rpm for 10 min and heated to 50° C., then the stirring speed was reduced to 800 rpm and the mixture was stirred for 50 min, and then cooled naturally;

[0034] In step 4, deionized water was used for washing 3 times;

[0035] In step 5, the drying temperature is controlled to be 90° C. and the drying time is controlled to be 5 h.

[0036] Embodiment 2

[0037] The technical solution of the present invention: a silane-modified composite electrochromic material and a preparation method thereof, comprising an alkane coupling agent, an ethanol aqueous solution, tungsten trioxide, polyaniline, triphenylamine, 3,3-bis(4-dimethylaminophenyl)-6-dimethylaminophenyl peptide, a solvent and a catalyst;

[0038] The silane coupling agent is one of vinyl triethoxysilane, vinyl trimethoxysilane and vinyl trisilane;

[0039] A method for preparing a silane-modified composite electrochromic material comprises the following steps:

[0040] Step 1: Stir and mix the silane coupling agent and the ethanol aqueous solution to prepare a modified liquid, and adjust the pH value;

[0041] Step 2: Mix tungsten trioxide, polyaniline, triphenylamine and crystal violet lactone, and then add solvent and catalyst and continue to stir and mix;

[0042] Step 3: Add the modified liquid to the mixture in step 2, and heat and stir to mix;

[0043] Step 4: Wash the mixture in step 3 repeatedly with water and filter;

[0044] Step 5: Heat and dry the mixture after washing and filtering in step 4 under vacuum to obtain a finished product.

[0045] Wherein the silane coupling agent in step 1 accounts for 2% of the mass of the modified liquid;

[0046] In step 2, tungsten trioxide, polyaniline, triphenylamine, and crystal violet lactone were reacted at a stirring speed of 600 rpm for 15 minutes, then allowed to stand for 5 minutes, and then solvent and catalyst were added and reacted at a stirring speed of 700 rpm for 28 minutes;

[0047] In step 3, after adding the modifying liquid, the mixture was stirred at 1600 rpm for 9 minutes and heated to 55° C., then the stirring speed was reduced to 800 rpm and the mixture was stirred for 45 minutes, and then cooled naturally;

[0048] In step 4, deionized water was used for washing 3 times;

[0049] In step 5, the drying temperature is controlled to be 90° C. and the drying time is controlled to be 5 h.

[0050] Embodiment 3

[0051] The technical solution of the present invention: a silane-modified composite electrochromic material and a preparation method thereof, comprising an alkane coupling agent, an ethanol aqueous solution, tungsten trioxide, polyaniline, triphenylamine, 3,3-bis(4-dimethylaminophenyl)-6-dimethylaminophenyl peptide, a solvent and a catalyst;

[0052] The silane coupling agent is one of vinyl triethoxysilane, vinyl trimethoxysilane and vinyl trisilane;

[0053] A method for preparing a silane-modified composite electrochromic material comprises the following steps:

[0054] Step 1: Stir and mix the silane coupling agent and the ethanol aqueous solution to prepare a modified liquid, and adjust the pH value;

[0055] Step 2: Mix tungsten trioxide, polyaniline, triphenylamine and crystal violet lactone, and then add solvent and catalyst and continue to stir and mix;

[0056] Step 3: Add the modified liquid to the mixture in step 2, and heat and stir to mix;

[0057] Step 4: Wash the mixture in step 3 repeatedly with water and filter;

[0058] Step 5: Heat and dry the mixture after washing and filtering in step 4 under vacuum to obtain a finished product.

[0059] The silane coupling agent in step 1 accounts for 3% of the mass of the modified liquid;

[0060] In step 2, tungsten trioxide, polyaniline, triphenylamine, and crystal violet lactone were reacted at a stirring speed of 600 rpm for 13 minutes, then allowed to stand for 6 minutes, and then solvent and catalyst were added and reacted at a stirring speed of 700 rpm for 26 minutes;

[0061] In step 3, after adding the modifying liquid, the mixture was stirred at 1700 rpm for 8 min and heated to 55° C., then the stirring speed was reduced to 900 rpm and the mixture was stirred for 42 min, followed by natural cooling;

[0062] In step 4, deionized water was used for washing 4 times;

[0063] In step 5, the drying temperature is controlled to be 95° C. and the drying time is 4 h.

[0064] Embodiment 4

[0065] The technical solution of the present invention: a silane-modified composite electrochromic material and a preparation method thereof, comprising an alkane coupling agent, an ethanol aqueous solution, tungsten trioxide, polyaniline, triphenylamine, 3,3-bis(4-dimethylaminophenyl)-6-dimethylaminophenyl peptide, a solvent and a catalyst;

[0066] The silane coupling agent is one of vinyl triethoxysilane, vinyl trimethoxysilane and vinyl trisilane;

[0067] A method for preparing a silane-modified composite electrochromic material comprises the following steps:

[0068] Step 1: Stir and mix the silane coupling agent and the ethanol aqueous solution to prepare a modified liquid, and adjust the pH value;

[0069] Step 2: Mix tungsten trioxide, polyaniline, triphenylamine and crystal violet lactone, and then add solvent and catalyst and continue to stir and mix;

[0070] Step 3: Add the modified liquid to the mixture in step 2, and heat and stir to mix;

[0071] Step 4: Wash the mixture in step 3 repeatedly with water and filter;

[0072] Step 5: Heat and dry the mixture after washing and filtering in step 4 under vacuum to obtain a finished product.

[0073] Wherein the silane coupling agent in step 1 accounts for 4% of the mass of the modified liquid;

[0074] In step 2, tungsten trioxide, polyaniline, triphenylamine, and crystal violet lactone were reacted at a stirring speed of 700 rpm for 12 minutes, then allowed to stand for 7 minutes, and then solvent and catalyst were added and reacted at a stirring speed of 800 rpm for 25 minutes;

[0075] In step 3, after adding the modifying liquid, the mixture was stirred at 1800 rpm for 6 min and heated to 60° C., then the stirring speed was reduced to 1000 rpm and the mixture was reacted for 35 min, and then cooled naturally;

[0076] In step 4, deionized water was used for washing 5 times;

[0077] In step 5, the drying temperature is controlled to be 95° C. and the drying time is 4 h.

[0078] Embodiment 5

[0079] The technical solution of the present invention: a silane-modified composite electrochromic material and a preparation method thereof, comprising an alkane coupling agent, an ethanol aqueous solution, tungsten trioxide, polyaniline, triphenylamine, 3,3-bis(4-dimethylaminophenyl)-6-dimethylaminophenyl peptide, a solvent and a catalyst;

[0080] The silane coupling agent is one of vinyl triethoxysilane, vinyl trimethoxysilane and vinyl trisilane;

[0081] A method for preparing a silane-modified composite electrochromic material comprises the following steps:

[0082] Step 1: Stir and mix the silane coupling agent and the ethanol aqueous solution to prepare a modified liquid, and adjust the pH value;

[0083] Step 2: Mix tungsten trioxide, polyaniline, triphenylamine and crystal violet lactone, and then add solvent and catalyst and continue to stir and mix;

[0084] Step 3: Add the modified liquid to the mixture in step 2, and heat and stir to mix;

[0085] Step 4: Wash the mixture in step 3 repeatedly with water and filter;

[0086] Step 5: Heat and dry the mixture after washing and filtering in step 4 under vacuum to obtain a finished product.

[0087] Wherein the silane coupling agent in step 1 accounts for 5% of the mass of the modified liquid;

[0088] In step 2, tungsten trioxide, polyaniline, triphenylamine, and crystal violet lactone are reacted at a stirring speed of 800 rpm for 12 minutes, then allowed to stand for 8 minutes, and then solvent and catalyst are added and reacted at a stirring speed of 1000 rpm for 20 minutes;

[0089] In step 3, after adding the modifying liquid, the mixture was stirred at 2000 rpm for 6 min and heated to 58° C., then the stirring speed was reduced to 1000 rpm and the mixture was stirred for 30 min, and then cooled naturally;

[0090] In step 4, deionized water was used for washing 5 times;

[0091] In step 5, the drying temperature is controlled to be 100° C. and the drying time is 3.5 h.

[0092] Embodiment 6

[0093] The technical solution of the present invention: a silane-modified composite electrochromic material and a preparation method thereof, comprising an alkane coupling agent, an ethanol aqueous solution, tungsten trioxide, polyaniline, triphenylamine, 3,3-bis(4-dimethylaminophenyl)-6-dimethylaminophenyl peptide, a solvent and a catalyst;

[0094] The silane coupling agent is one of vinyl triethoxysilane, vinyl trimethoxysilane and vinyl trisilane;

[0095] A method for preparing a silane-modified composite electrochromic material comprises the following steps:

[0096] Step 1: Stir and mix the silane coupling agent and the ethanol aqueous solution to prepare a modified liquid, and adjust the pH value;

[0097] Step 2: Mix tungsten trioxide, polyaniline, triphenylamine and crystal violet lactone, and then add solvent and catalyst and continue to stir and mix;

[0098] Step 3: Add the modified liquid to the mixture in step 2, and heat and stir to mix;

[0099] Step 4: Wash the mixture in step 3 repeatedly with water and filter;

[0100] Step 5: Heat and dry the mixture after washing and filtering in step 4 under vacuum to obtain a finished product.

[0101] Wherein the silane coupling agent in step 1 accounts for 5% of the mass of the modified liquid;

[0102] In step 2, tungsten trioxide, polyaniline, triphenylamine, and crystal violet lactone are reacted at a stirring speed of 800 rpm for 10 minutes, then allowed to stand for 8 minutes, and then a solvent and a catalyst are added and reacted at a stirring speed of 1000 rpm for 20 minutes;

[0103] In step 3, after adding the modifying liquid, the mixture was stirred at 2000 rpm for 5 min and heated to 60° C., then the stirring speed was reduced to 1000 rpm and the mixture was stirred for 30 min, and then cooled naturally;

[0104] In step 4, deionized water was used for washing 6 times;

[0105] Wherein in step 5, the drying temperature is controlled to be 100°C and the drying time is 3h;

[0106] Comparative Example 1

[0107] This solution is the same as Example 6 except that tungsten trioxide is not added.

[0108] Comparative Example 2

[0109] This solution is the same as Example 6 except that polyaniline is not added.

[0110] Comparative Example 3

[0111] This scheme is the same as Example 6 except that triphenylamine is not added.

[0112] Performance Testing

[0113] The silane-modified composite electrochromic materials prepared in the above examples and comparative examples were placed in a hydrochloric acid solution, and voltages of 1V, 2V, 3V, 4V, and 5V were applied in sequence to observe the color changes. Figure 1 As shown, it can be clearly seen that the color changes of the silane-modified composite electrochromic material prepared in the embodiment are diverse, and the color change of the silane-modified composite electrochromic material prepared in the comparative example is relatively simple. Therefore, it can be known that tungsten trioxide, polyaniline and triphenylamine affect the color change effect;

[0114] The silane-modified composite electrochromic materials prepared in the above-mentioned embodiments and comparative examples were used to make color-changing glass, and voltages of 1V, 2V, 3V, 4V, and 5V were applied respectively to detect the time interval of color change and the number of cycles. Figure 2As shown, in the embodiment, the light-changing time interval is short and the service life is longer, so it can be known that tungsten trioxide, polyaniline and triphenylamine affect the color-changing time interval and service life.

[0115] The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.

[0116] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A silane-modified composite electrochromic material, characterized in that: The invention comprises a silane coupling agent, an ethanol aqueous solution, tungsten trioxide, polyaniline, triphenylamine, 3,3-bis(4-dimethylaminophenyl)-6-dimethylaminophenyl peptide, a solvent and a catalyst.

2. The silane-modified composite electrochromic material according to claim 1, characterized in that: The silane coupling agent is one of vinyl triethoxysilane, vinyl trimethoxysilane and vinyl trisilane.

3. The method for preparing a silane-modified composite electrochromic material according to claim 1, characterized in that: The following steps are involved: Step 1: Stir and mix the silane coupling agent and the ethanol aqueous solution to prepare a modified liquid, and adjust the pH value; Step 2: Mix tungsten trioxide, polyaniline, triphenylamine and crystal violet lactone, and then add solvent and catalyst and continue to stir and mix; Step 3: Add the modified liquid to the mixture in step 2, and heat and stir to mix; Step 4: Wash the mixture in step 3 repeatedly with water and filter; Step 5: Heat and dry the mixture after washing and filtering in step 4 under vacuum to obtain a finished product.

4. The method for preparing a silane-modified composite electrochromic material according to claim 3, characterized in that: In the step 1, the silane coupling agent accounts for 2-5% of the mass of the modified liquid.

5. The method for preparing a silane-modified composite electrochromic material according to claim 3, characterized in that: In the step 2, tungsten trioxide, polyaniline, triphenylamine and crystal violet lactone are reacted at a stirring speed of 500 to 800 rpm for 10 to 15 minutes, then allowed to stand for 5 to 8 minutes, and then a solvent and a catalyst are added and reacted at a stirring speed of 600 to 1000 rpm for 20 to 30 minutes.

6. The method for preparing a silane-modified composite electrochromic material according to claim 3, characterized in that: In the step 3, after adding the modifying liquid, the mixture is reacted for 5 to 10 minutes at a stirring speed of 1500 to 2000 rpm and heated to 50 to 60° C., then the stirring speed is reduced to 800 to 1000 rpm and reacted for 30 to 50 minutes, and then cooled naturally.

7. The method for preparing a silane-modified composite electrochromic material according to claim 3, characterized in that: In the step 4, deionized water is used for washing 3 to 6 times.

8. The method for preparing a silane-modified composite electrochromic material according to claim 3, characterized in that: In step 5, the drying temperature is controlled to be 90-100° C. and the drying time is 3-5 hours.