Fluorescent material and preparation process thereof

By adopting core-shell structures in fluorescent materials and using doped mesoporous silica microspheres and polymer shells, the problem of poor aging resistance of fluorescent materials is solved, and high aging resistance and precipitation resistance are achieved while maintaining the High light transmittance and luminous effect.

CN118995198APending Publication Date: 2024-11-22HUAZHONG XINSHENG (TANGSHAN) FLUORESCENT MATERIAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411193637.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The poor aging resistance of existing fluorescent materials affects their performance in fluorescent lamps and LED applications, and pretreatment methods will affect the luminous effect of the phosphor.

Method used

Fluorescent material with core-shell structure, the core is mesoporous silica microspheres doped with phosphor, the inner shell is polyvinyl butyral, the outer shell is polymethyl methacrylate, through hexamethyldisilazane Modified mesoporous silica microspheres reduce surface adsorption and improve the aging resistance and precipitation resistance of fluorescent materials.

Benefits of technology

It improves the aging resistance and precipitation resistance of fluorescent materials, maintains high light transmittance, does not affect the luminous effect of the phosphor, and significantly improves the stability and service life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of fluorescent materials, and provides a fluorescent material and a preparation process thereof. The fluorescent material is of a core-shell structure, a core in the core-shell structure is mesoporous silica microspheres doped with fluorescent powder, a shell in the core-shell structure comprises an inner shell and an outer shell, the inner shell is polyvinyl butyral, and the outer shell is polymethyl methacrylate. According to the technical scheme, the problem of poor aging resistance of the fluorescent material in the prior art is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fluorescent materials, and in particular to a fluorescent material and a preparation process thereof. Background Art

[0002] Fluorescent materials are materials that can emit light of a specific wavelength after absorbing light of a specific wavelength. They are mainly composed of a matrix, an activator, and a flux that promotes matrix crystallization and improves luminous efficiency. According to the chemical composition of the matrix, fluorescent materials can be divided into sulfide fluorescent materials, silicate fluorescent materials, tungstate fluorescent materials, oxide fluorescent materials, and fluoride fluorescent materials. Due to their superior performance, fluorescent materials are widely used in various fields, such as fluorescent lamps, LEDs, medical treatment, chemistry, etc.

[0003] Fluorescent lamps and LEDs are two important areas of application of fluorescent materials. Compared with traditional incandescent lamps, fluorescent lamps have the advantages of energy saving and low cost. In addition, as a new type of lighting tool, LED has the advantages of energy saving, environmental protection, and long life. However, both fluorescent lamps and LEDs will generate heat during the application process, which affects the performance of fluorescent materials. Therefore, improving the aging resistance of silver light materials is a research hotspot.

[0004] Application No. 202111027382.3 discloses an aging-resistant and anti-precipitation fluorescent material. The fluorescent powder is treated with gas-phase silica, an amino-containing alkaline solution, porous silica microspheres and a silane coupling agent, and then mixed with fluorescent glue to prepare an aging-resistant and anti-precipitation fluorescent material. However, the fluorescent powder is pre-treated with opaque materials, which will affect the fluorescent effect of the fluorescent powder to a certain extent, and its aging resistance needs to be further improved. Summary of the invention

[0005] The present invention provides a fluorescent material and a preparation process thereof, which solves the problem of poor aging resistance of the fluorescent material in the related art.

[0006] The technical solution of the present invention is as follows: A fluorescent material is a core-shell structure, wherein the core of the core-shell structure is a mesoporous silica microsphere doped with fluorescent powder, and the shell of the core-shell structure comprises an inner shell and an outer shell, wherein the inner shell is polyvinyl butyral and the outer shell is polymethyl methacrylate.

[0007] As a further technical solution, the mass ratio of the raw material of the core to the raw material of the shell is 30~35:1~5.

[0008] As a further technical solution, the mesoporous silica microspheres are hexamethyldisilazane-modified mesoporous silica.

[0009] The present invention limits the mesoporous silica microspheres to hexamethyldisilazane-modified mesoporous silica. After the mesoporous silica is modified with hexamethyldisilazane, the hydroxyl groups on the surface will be blocked, which greatly reduces the surface adsorption. When further doped with fluorescent powder, the fluorescent powder will be adsorbed in the pores of the mesoporous silica, thereby further improving the aging resistance and precipitation resistance of the fluorescent material.

[0010] As a further technical solution, the raw materials of the core include phosphor and mesoporous silica microspheres in a mass ratio of 30:3-4.

[0011] The present invention limits the raw materials of the core to phosphor and mesoporous silica microspheres in a mass ratio of 30:3-4, thereby further improving the aging resistance and precipitation resistance of the fluorescent material.

[0012] As a further technical solution, the phosphor may be any type of phosphor, preferably one or both of yttrium aluminum garnet phosphor and γ-phase alumina.

[0013] As a further technical solution, the mass ratio of the raw material of the core to the raw material of the shell is 30~35:3.

[0014] The present invention limits the mass ratio of the core raw material to the shell raw material to 30-35:3, thereby further improving the aging resistance and precipitation resistance of the fluorescent material.

[0015] As a further technical solution, the mass of the polyvinyl butyral is greater than or equal to the mass of polymethyl methacrylate.

[0016] The invention makes the quality of polyvinyl butyral greater than or equal to that of polymethyl methacrylate, thereby further improving the aging resistance and precipitation resistance of the fluorescent material.

[0017] As a further technical solution, the mass ratio of the polymethyl methacrylate to polyvinyl butyral is 1:2.

[0018] The invention limits the mass ratio of polymethyl methacrylate to polyvinyl butyral to 1:2, thereby further improving the aging resistance and precipitation resistance of the fluorescent material.

[0019] The present invention also proposes a preparation process of a fluorescent material, comprising the following steps: S1, mixing the phosphor, mesoporous silica microspheres and solvent uniformly, filtering, washing and drying to obtain pretreated phosphor; S2, mixing the pretreated phosphor, polyvinyl butyral and solvent evenly, filtering and drying to obtain a phosphor with an inner shell; S3, mixing the inner shell-encapsulated fluorescent powder, polymethyl methacrylate and solvent evenly, filtering and drying to obtain a fluorescent material.

[0020] As a further technical solution, the solvents in S1 and S2 are both alcohol solutions, preferably ethanol.

[0021] As a further technical solution, the solvent in S3 can be any solvent that can dissolve polymethyl methacrylate, preferably N,N-dimethylformamide.

[0022] The working principle and beneficial effects of the present invention are: The present invention provides a fluorescent material, which is a core-shell structure. The core in the core-shell structure is a mesoporous silica microsphere doped with fluorescent powder. The shell in the core-shell structure includes an inner shell and an outer shell. The inner shell is polyvinyl butyral and the outer shell is polymethyl methacrylate. A polymer material with high light transmittance is used as the outer shell, which will not affect the fluorescent effect of the fluorescent powder. In addition, the mesoporous silica microspheres in the core structure and the shell structure provide the fluorescent material with good aging resistance and precipitation resistance. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] The parameters of the raw materials in the following examples and comparative examples are as follows: The particle size of mesoporous silica microspheres was 90 μm and was purchased from Beijing Zhongke Keyou Technology Co., Ltd.; The phosphor is γ-phase aluminum oxide with a particle size of 20nm and a content of 99.99%; Polymethyl methacrylate is PMMA IR-D70; Polyvinyl butyral is PVB B60H; The preparation method of fluorescent glue is as follows: Component A of Dow Corning OE-6351 was mixed with 1 / 2 of the mass of component B, and after stirring at 1000 rpm for 20 minutes, the remaining 1 / 2 of the mass of component B was added and stirred for 100 minutes to obtain fluorescent glue. The mass ratio of component A to component B was 1:1.

[0025] Example 1 S1, 30 g of phosphor, 1 g of mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, dissolving 0.4 g of polyvinyl butyral in 100 mL of ethanol, adding the above-mentioned pretreated phosphor and mixing evenly, filtering, and drying to obtain a phosphor with an inner shell; S3. Dissolve 0.6 g of polymethyl methacrylate in 100 mL of DMF, add the inner shell fluorescent powder and mix well, filter and dry to obtain a fluorescent material.

[0026] Example 2 S0, after mixing 300 mL of petroleum ether with a boiling range of 60-90°C and 25 mL of hexamethyldisilazane, add 100 g of mesoporous silica microspheres, reflux at 70°C for 15 h, transfer to a Soxhlet extractor, extract with acetone for 12 h, and dry to obtain modified mesoporous silica microspheres; S1, mixing 30 g of phosphor, 1 g of modified mesoporous silica microspheres and 450 mL of ethanol, ultrasonically treating at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtering, washing with ethanol, and drying to obtain a pretreated phosphor; S2, dissolving 0.4 g of polyvinyl butyral in 100 mL of ethanol, adding the above-mentioned pretreated phosphor and mixing evenly, filtering, and drying to obtain a phosphor with an inner shell; S3. Dissolve 0.6 g of polymethyl methacrylate in 100 mL of DMF, add the inner shell fluorescent powder and mix well, filter and dry to obtain a fluorescent material.

[0027] Example 3 S1. Mix 30 g of phosphor, 1 g of mesoporous silica microspheres, 25 mL of hexamethyldisilazane and 450 mL of ethanol, ultrasonicate for 30 min at a power of 300 W and a frequency of 40 kHz until uniform, filter, wash with ethanol, and dry to obtain a pretreated phosphor; S2, dissolving 0.4 g of polyvinyl butyral in 100 mL of ethanol, adding the above-mentioned pretreated phosphor and mixing evenly, filtering, and drying to obtain a phosphor with an inner shell; S3. Dissolve 0.6 g of polymethyl methacrylate in 100 mL of DMF, add the inner shell fluorescent powder and mix well, filter and dry to obtain a fluorescent material.

[0028] Example 4 S0, after mixing 300 mL of petroleum ether with a boiling range of 60-90°C and 25 mL of hexamethyldisilazane, add 100 g of mesoporous silica microspheres, reflux at 70°C for 15 h, transfer to a Soxhlet extractor, extract with acetone for 12 h, and dry to obtain modified mesoporous silica microspheres; S1, mixing 30 g of phosphor, 3 g of modified mesoporous silica microspheres and 450 mL of ethanol, ultrasonicating at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtering, washing with ethanol, and drying to obtain a pretreated phosphor; S2, dissolving 0.4 g of polyvinyl butyral in 100 mL of ethanol, adding the above-mentioned pretreated phosphor and mixing evenly, filtering, and drying to obtain a phosphor with an inner shell; S3. Dissolve 0.6 g of polymethyl methacrylate in 100 mL of DMF, add the inner shell fluorescent powder and mix well, filter and dry to obtain a fluorescent material.

[0029] Example 5 S0, after mixing 300 mL of petroleum ether with a boiling range of 60-90°C and 25 mL of hexamethyldisilazane, add 100 g of mesoporous silica microspheres, reflux at 70°C for 15 h, transfer to a Soxhlet extractor, extract with acetone for 12 h, and dry to obtain modified mesoporous silica microspheres; S1, 30 g of phosphor, 4 g of modified mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, dissolving 0.4 g of polyvinyl butyral in 100 mL of ethanol, adding the above-mentioned pretreated phosphor and mixing evenly, filtering, and drying to obtain a phosphor with an inner shell; S3. Dissolve 0.6 g of polymethyl methacrylate in 100 mL of DMF, add the inner shell fluorescent powder and mix well, filter and dry to obtain a fluorescent material.

[0030] Example 6 S0, after mixing 300 mL of petroleum ether with a boiling range of 60-90°C and 25 mL of hexamethyldisilazane, add 100 g of mesoporous silica microspheres, reflux at 70°C for 15 h, transfer to a Soxhlet extractor, extract with acetone for 12 h, and dry to obtain modified mesoporous silica microspheres; S1, mixing 30 g of phosphor, 5 g of modified mesoporous silica microspheres and 450 mL of ethanol, ultrasonicating at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtering, washing with ethanol, and drying to obtain a pretreated phosphor; S2, dissolving 0.4 g of polyvinyl butyral in 100 mL of ethanol, adding the above-mentioned pretreated phosphor and mixing evenly, filtering, and drying to obtain a phosphor with an inner shell; S3. Dissolve 0.6 g of polymethyl methacrylate in 100 mL of DMF, add the inner shell fluorescent powder and mix well, filter and dry to obtain a fluorescent material.

[0031] Example 7 S0, after mixing 300 mL of petroleum ether with a boiling range of 60-90°C and 25 mL of hexamethyldisilazane, add 100 g of mesoporous silica microspheres, reflux at 70°C for 15 h, transfer to a Soxhlet extractor, extract with acetone for 12 h, and dry to obtain modified mesoporous silica microspheres; S1, 30 g of phosphor, 4 g of modified mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, dissolving 1.2 g of polyvinyl butyral in 100 mL of ethanol, adding the above-mentioned pretreated phosphor and mixing evenly, filtering, and drying to obtain a phosphor with an inner shell; S3. Dissolve 1.8 g of polymethyl methacrylate in 100 mL of DMF, add the inner shell fluorescent powder and mix well, filter and dry to obtain a fluorescent material.

[0032] Example 8 S0, after mixing 300 mL of petroleum ether with a boiling range of 60-90°C and 25 mL of hexamethyldisilazane, add 100 g of mesoporous silica microspheres, reflux at 70°C for 15 h, transfer to a Soxhlet extractor, extract with acetone for 12 h, and dry to obtain modified mesoporous silica microspheres; S1, 30 g of phosphor, 4 g of modified mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, dissolving 2 g of polyvinyl butyral in 100 mL of ethanol, adding the above-mentioned pretreated phosphor and mixing evenly, filtering, and drying to obtain a phosphor with an inner shell; S3. After dissolving 3 g of polymethyl methacrylate in 100 mL of DMF, add the inner shell-encapsulated fluorescent powder and mix well, filter, and dry to obtain a fluorescent material.

[0033] Example 9 S0, after mixing 300 mL of petroleum ether with a boiling range of 60-90°C and 25 mL of hexamethyldisilazane, add 100 g of mesoporous silica microspheres, reflux at 70°C for 15 h, transfer to a Soxhlet extractor, extract with acetone for 12 h, and dry to obtain modified mesoporous silica microspheres; S1, 30 g of phosphor, 4 g of modified mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, dissolving 1.5 g of polyvinyl butyral in 100 mL of ethanol, adding the above-mentioned pretreated phosphor and mixing evenly, filtering, and drying to obtain a phosphor with an inner shell; S3. Dissolve 1.5 g of polymethyl methacrylate in 100 mL of DMF, add the inner shell phosphor and mix well, filter and dry to obtain a fluorescent material.

[0034] Example 10 S0, after mixing 300 mL of petroleum ether with a boiling range of 60-90°C and 25 mL of hexamethyldisilazane, add 100 g of mesoporous silica microspheres, reflux at 70°C for 15 h, transfer to a Soxhlet extractor, extract with acetone for 12 h, and dry to obtain modified mesoporous silica microspheres; S1, 30 g of phosphor, 4 g of modified mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, dissolving 2 g of polyvinyl butyral in 100 mL of ethanol, adding the above-mentioned pretreated phosphor and mixing evenly, filtering, and drying to obtain a phosphor with an inner shell; S3. Dissolve 1 g of polymethyl methacrylate in 100 mL of DMF, add the inner shell phosphor and mix well, filter and dry to obtain a fluorescent material.

[0035] Embodiment 11 S0, after mixing 300 mL of petroleum ether with a boiling range of 60-90°C and 25 mL of hexamethyldisilazane, add 100 g of mesoporous silica microspheres, reflux at 70°C for 15 h, transfer to a Soxhlet extractor, extract with acetone for 12 h, and dry to obtain modified mesoporous silica microspheres; S1, 30 g of phosphor, 4 g of modified mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, dissolving 2.3 g of polyvinyl butyral in 100 mL of ethanol, adding the above-mentioned pretreated phosphor and mixing evenly, filtering, and drying to obtain a phosphor with an inner shell; S3. Dissolve 0.7 g of polymethyl methacrylate in 100 mL of DMF, add the inner shell fluorescent powder and mix well, filter and dry to obtain a fluorescent material.

[0036] Comparative Example 1 S1, 30 g of phosphor, 1 g of mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a pretreated phosphor; S2, dissolving 0.6 g of polymethyl methacrylate in 100 mL of DMF, adding the above-mentioned pretreated phosphor and mixing evenly, filtering, and drying to obtain a phosphor with an inner shell; S3. Dissolve 0.4 g of polyvinyl butyral in 100 mL of ethanol, add the inner shell fluorescent powder and mix well, filter, and dry to obtain a fluorescent material.

[0037] Comparative Example 2 30 g of phosphor, 1 g of mesoporous silica microspheres and 450 mL of ethanol were mixed, ultrasonicated at a power of 300 W and a frequency of 40 kHz for 30 min until uniform, filtered, washed with ethanol, and dried to obtain a fluorescent material.

[0038] The fluorescent materials obtained in Examples 1 to 11 and Comparative Examples 1 to 2 were respectively mixed with fluorescent glue at a mass ratio of 0.7:1, and stirred at 1000 rpm for 30 min. The aging resistance test was performed with reference to the method in GB / T 2689.3-1981 "Simple linear unbiased estimation method for life tests and accelerated life tests (for Weibull distribution)". The aging resistance was evaluated by the percentage of the 2000 h luminous flux to the initial luminous flux; and the sedimentation velocity was calculated by the following formula to evaluate the anti-sedimentation property; V g =[d 2 ×(ρ 2 -ρ 1 )]÷18η×G; Where: V g is the sedimentation velocity, d is the particle diameter, ρ 2 is the particle density, ρ 1 is the fluid density, η is the fluid viscosity, and G is the gravitational acceleration; The results are recorded in Table 1.

[0039] Table 1 Aging resistance and precipitation resistance of fluorescent materials

[0040] It can be seen from Table 1 that the fluorescent material obtained by the present invention has good aging resistance and precipitation resistance.

[0041] Compared with Comparative Examples 1-2, the fluorescent material in Examples 1-11 is a core-shell structure, the core is mesoporous silica microspheres doped with phosphor, the inner shell is polyvinyl butyral, and the outer shell is polymethyl methacrylate. The percentage of 2000h luminous flux of the fluorescent material obtained in Examples 1-11 to the initial luminous flux is higher than that of Comparative Examples 1-2, and the sedimentation rate is lower than that of Comparative Examples 1-2, indicating that the core is mesoporous silica microspheres doped with phosphor, the inner shell is polyvinyl butyral, and the outer shell is polymethyl methacrylate, which can improve the aging resistance and precipitation resistance of the fluorescent material.

[0042] The percentage of 2000h luminous flux of the fluorescent materials obtained in Examples 2 and 4 to 11 to the initial luminous flux is higher than that in Examples 1 and 3, and the sedimentation rate is lower than that in Examples 1 and 3, indicating that the mesoporous silica microspheres are mesoporous silica modified by hexamethyldisilazane, which can further improve the aging resistance and precipitation resistance of the fluorescent material.

[0043] The percentage of the 2000h luminous flux of the fluorescent material obtained in Examples 4~5 to the initial luminous flux is higher than that in Examples 2 and 6, and the sedimentation rate is lower than that in Examples 2 and 6, indicating that the raw materials of the core are phosphor and mesoporous silica microspheres in a mass ratio of 30:3~4, which can further improve the aging resistance and precipitation resistance of the fluorescent material.

[0044] The percentage of the 2000h luminous flux of the fluorescent material obtained in Example 7 to the initial luminous flux is higher than that in Example 5 and Example 8, and the sedimentation rate is lower than that in Example 5 and Example 8, indicating that the mass ratio of the core raw material to the shell raw material is 30~35:3, which can further improve the aging resistance and precipitation resistance of the fluorescent material.

[0045] The percentage of the 2000h luminous flux of the fluorescent materials obtained in Examples 9 to 11 to the initial luminous flux is higher than that in Example 7, and the sedimentation rate is lower than that in Example 7, indicating that the quality of polyvinyl butyral is ≥ the quality of polymethyl methacrylate, which can further improve the aging resistance and precipitation resistance of the fluorescent material.

[0046] The percentage of the 2000h luminous flux of the fluorescent material obtained in Example 10 to the initial luminous flux is higher than that in Example 9 and Example 11, and the sedimentation rate is lower than that in Example 9 and Example 11, indicating that the mass ratio of polymethyl methacrylate and polyvinyl butyral is 1:2, which can further improve the aging resistance and precipitation resistance of the fluorescent material.

[0047] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A fluorescent material, characterized in that: The core of the core-shell structure is a mesoporous silica microsphere doped with fluorescent powder, and the shell of the core-shell structure includes an inner shell and an outer shell, wherein the inner shell is polyvinyl butyral and the outer shell is polymethyl methacrylate.

2. A fluorescent material according to claim 1, characterized in that: The mass ratio of the raw material of the core to the raw material of the shell is 30-35:1-5.

3. A fluorescent material according to claim 2, characterized in that: The raw materials of the core include phosphor and mesoporous silica microspheres in a mass ratio of 30:3-4.

4. A fluorescent material according to claim 3, characterized in that: The mass ratio of the raw material of the core to the raw material of the shell is 30-35:

3.

5. A fluorescent material according to claim 1, characterized in that: The particle size of the mesoporous silica microspheres is 90 μm.

6. A fluorescent material according to claim 1, characterized in that: The mass of the polyvinyl butyral is greater than or equal to the mass of the polymethyl methacrylate.

7. A fluorescent material according to claim 6, characterized in that: The mass ratio of the polymethyl methacrylate to the polyvinyl butyral is 1:

2.

8. The fluorescent material according to claim 1, characterized in that: The mesoporous silica microspheres are hexamethyldisilazane-modified mesoporous silica.

9. A fluorescent material according to claim 5, characterized in that: The phosphor is γ-phase aluminum oxide, with a particle size of 20 nm and a content of 99.99%.

10. A process for preparing a fluorescent material according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1, mixing the phosphor, mesoporous silica microspheres and solvent uniformly, filtering, washing and drying to obtain pretreated phosphor; S2, mixing the pretreated phosphor, polyvinyl butyral and solvent evenly, filtering and drying to obtain a phosphor with an inner shell; S3, mixing the inner shell-encapsulated fluorescent powder, polymethyl methacrylate and solvent evenly, filtering and drying to obtain a fluorescent material.

Citation Information

Patent Citations

  • Anti-aging anti-settling fluorescent material as well as preparation method and application thereof