Indium phosphide core-shell quantum dot and luminous efficiency improving method thereof
The preparation of indium phosphide core-shell quantum dots through hexafluorophosphate etching and one-pot method solves the problem of removing the surface oxide layer of indium phosphide quantum dots, improves luminescence efficiency and reduces process risks, and achieves environmentally friendly and high performance Quantum dot preparation.
Patent Information
- Application Number
- CN202411041920.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, when preparing indium phosphide quantum dots, it is difficult to effectively remove the surface oxide layer, resulting in low luminescence efficiency and harsh process conditions, posing safety hazards and high cost problems.
Hexafluorophosphate is used to etch the indium phosphide nanocrystal surface under mild conditions, and the one-pot method is used to prepare indium phosphide core-shell quantum dots, which avoids the risk of secondary oxidation and over-etching and improves the photoluminescence efficiency.
It significantly improves the photoluminescence efficiency of indium phosphide core-shell quantum dots, achieves better luminescence performance, and avoids the use of heavy metals, making it suitable for environmentally friendly applications.
Smart Images

Figure CN118995215A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of quantum dots, and in particular to an indium phosphide core-shell quantum dot and a method for improving the luminous efficiency thereof. Background Art
[0002] As a zero-dimensional fluorescent nanomaterial with quantum confinement effect and size effect, colloidal quantum dots (QDs) have attracted extensive attention from academia and industry. At present, the research on representative quantum dot luminescence systems mainly focuses on cadmium-based (CdSe, CdS, CdTe, etc.), indium-based (InP), lead-based (APbX3), zinc-based (ZnSe), copper-based (CuInS2) and perovskite quantum dots (CsPbX3, X = Cl, Br and / or I). Although cadmium-based quantum dots and new perovskite quantum dots have achieved excellent optical properties, the potential harm of heavy metal cadmium and lead to the environment and organisms limits their application scenarios. Indium phosphide (InP) quantum dots are regarded as the most promising alternative materials due to their large Bohr exciton radius (9.6 nm), narrow bulk band gap (1.34 eV), wide emission spectrum control range (blue light to near infrared), low exciton emission threshold, and non-toxic and environmentally friendly. They are expected to be used in lighting, display and biomedical imaging.
[0003] Due to the strong covalent nature of the In-P bond, it is still challenging to obtain InP quantum dots with optical properties (fluorescence quantum yield, luminescence intensity, color purity, etc.) comparable to cadmium-based quantum dots and perovskite quantum dots. In early studies, when preparing indium phosphide quantum dots, the surface ligands directly combined with InP nanocrystals, and the luminescence of the resulting quantum dots was very weak, and the emission spectrum was wide and asymmetric. As the research continued to deepen, researchers discovered that quantum dots have surface effects, that is, large specific surface area and a high proportion of surface atoms. The protective effect of organic ligands on InP nanocrystals is limited, and the negative trivalent phosphorus on the surface is easily oxidized by oxidizing sources in the environment to form an oxide layer and oxidation defects. The distribution of oxidation defect energy levels is wide, which broadens the emission spectrum of InP quantum dots. The effective electron mass of InP is only 0.076. m 0( m 0 is the mass of free electrons), and the binding ability to excitons is weak. After the excitons dissociate, the delocalized electrons diffuse to the surface of InP nanocrystals, and then are captured by surface defects and deactivated by non-radiative transitions, resulting in fluorescence quenching. In order to confine excitons in InP nanocrystals, a technical route of constructing a type I band structure at the core-shell interface by coating with an inorganic shell layer was developed, and good results were achieved.
[0004] In the core-shell structure of InP quantum dots, common shell materials are zinc sulfide (ZnS), zinc selenide (ZnSe), zinc sulfide selenide alloy (ZnSex S 1-x ) etc. Compared with organic ligands, inorganic shells can achieve better protection effects. Since the oxide layer on the surface of InP nanocrystals will hinder the epitaxial growth of the shell and affect the luminescence efficiency, how to solve the adverse effects of the oxide layer has become a research hotspot.
[0005] The commonly used solution in the industry is to use silicon-based phosphine (for example, tris(trimethylsilyl)phosphine, i.e. TMSP, etc.) to synthesize InP cores, and then add hydrofluoric acid to etch the surface of InP nanocrystals to remove the surface oxide layer. Although this approach has improved the luminescence performance of indium phosphide quantum dots, it has serious drawbacks and hidden dangers: (1) InP is very sensitive to hydrofluoric acid. Even if the concentration of hydrofluoric acid is adjusted to a lower level, over-etching is very likely to occur. Once hydrofluoric acid is added, the etching process is difficult to stop, and shortening the etching time is of little significance. Therefore, it is very difficult to control the progress of the etching reaction. (2) Currently, most methods using silicon-based phosphine have harsh reaction conditions and generally require a reaction temperature above 260°C. Silicon-based phosphine is highly sensitive to water and oxygen. The reaction process using silicon-based phosphine needs to be completed in an inert atmosphere. Therefore, it is necessary to operate in a glove box in the laboratory. (3) When using the "two-pot method" to prepare indium phosphide core-shell quantum dots (i.e., purifying the synthesized indium phosphide core and then coating it with a shell), the InP core etched by hydrofluoric acid will still face the risk of secondary oxidation before the shell is coated. (4) Hydrofluoric acid is a fuming corrosive liquid. If it is accidentally leaked, it will cause serious damage to the environment and human body. (5) Silicon-based phosphine is expensive, and the cost of preparing InP quantum dots is high.
[0006] Based on this, developing a solution that can effectively etch away the oxide layer on the surface of InP nanocrystals with mild and controllable etching reaction conditions is of great significance to promoting the development of such quantum dots, and is also a technical problem that urgently needs to be solved. Summary of the invention
[0007] The present invention provides an indium phosphide core-shell quantum dot and a method for improving its luminous efficiency. The etching method provided by the present invention has relatively mild reaction conditions, and the progress and degree of the etching reaction are more controllable. The preparation method of indium phosphide core-shell quantum dots provided by the present invention adopts a "one-pot method" to avoid the problem of secondary oxidation faced by the InP core during the purification process before the shell coating. Compared with conventional indium phosphide quantum dots of the same type with a core-shell structure, the indium phosphide quantum dots prepared by this method have significantly improved photoluminescence efficiency and exhibit more excellent luminescent performance. The indium phosphide core etching method and the indium phosphide core-shell quantum dot preparation method provided by the present invention are specifically achieved through the following technologies.
[0008] The first aspect of the present invention provides an etching method for an indium phosphide core of an indium phosphide core-shell quantum dot, comprising mixing an indium source, a phosphorus source and a zinc halide to prepare an indium phosphide nanocrystalline core; dissolving hexafluorophosphate in an organic solvent and adding the solvent to the indium phosphide nanocrystalline core for etching.
[0009] Furthermore, the molar ratio of the hexafluorophosphate to the indium source is 1:(1-5).
[0010] Indium phosphide nanocrystals are extremely oxygen-affinity, and the defect sites formed by oxidation will capture excitons and cause luminescence quenching. In order to minimize the oxidation defects on the surface of indium phosphide nanocrystals, the present invention adopts a "one-pot method" to complete the synthesis and modification of indium phosphide nanocrystals and the preparation of indium phosphide core-shell quantum dots in the same reaction vessel. First, indium source and zinc halide are added to the container and mixed evenly, a protective gas atmosphere is created, the temperature is raised to the reaction temperature, and finally a phosphorus source is added to react to complete the synthesis of indium phosphide nanocrystals; then a certain amount of hexafluorophosphate is introduced to complete the etching.
[0011] There is a trace amount of water in the above reaction system of the present invention, for example, when the protective gas (such as argon gas, etc.) is evacuated and filled, the trace amount of water vapor in the protective gas is not completely removed, and the trace amount of water in the commercially available reagent products. Hexafluorophosphate is very sensitive to water and reacts to generate hydrogen fluoride gas when it encounters trace water. Under the action of hydrogen fluoride, the oxides and defect sites on the surface of the indium phosphide nanocrystals will be etched away, thereby achieving an improvement in the photoluminescence efficiency.
[0012] It should be noted that hexafluorophosphates include, but are not limited to, alkali metal salts such as lithium hexafluorophosphate (LiPF6), sodium hexafluorophosphate (NaPF6), potassium hexafluorophosphate (KPF6), and other salts that can react with trace amounts of water to generate hydrogen fluoride. These hexafluorophosphates with the same function all fall within the scope of protection of the present invention.
[0013] In some embodiments of the present invention, the hexafluorophosphate may generally be lithium hexafluorophosphate (LiPF6).
[0014] Furthermore, the etching reaction conditions are 180-240° C. for 5-60 min.
[0015] Furthermore, the reaction conditions for preparing the indium phosphide nanocrystal core are 160-220° C. for 5-40 min.
[0016] It is well known in the art that indium phosphide nanocrystal cores are prepared under a protective atmosphere, the purpose of which is to isolate oxygen without affecting the main reaction. Therefore, any protective atmosphere that meets the above purpose belongs to the protection scope of the present invention.
[0017] Optionally, the preparation method of the indium phosphide nanocrystal core is: weigh an indium source and a zinc halide, dissolve the two in a three-necked flask containing 5 mL of oleylamine, repeat the vacuum and argon filling operation three times to create an inert atmosphere, and then heat it to a predetermined temperature and add a phosphorus source to react to prepare an indium phosphide nanocrystal core.
[0018] Furthermore, the molar ratio of the indium halide source, the phosphorus source and the zinc halide is 1:(3-5):(4-6).
[0019] Optionally, the molar ratio of the indium halide source, the phosphorus source and the zinc halide is 1:4:5.
[0020] Furthermore, the indium halide source is at least one of indium trichloride, indium tribromide, and indium triiodide.
[0021] Further, the phosphorus source is at least one aminophosphine; Furthermore, the phosphorus source is tri(dimethylamino)phosphine and / or tri(diethylamino)phosphine.
[0022] Furthermore, the zinc halide is at least one of zinc chloride, zinc bromide and zinc iodide.
[0023] A second aspect of the present invention provides a method for preparing indium phosphide core-shell quantum dots, comprising the following steps: etching the indium phosphide nanocrystal core using the above-mentioned indium phosphide core etching method; A sulfur source and a selenium source are added to the reaction system, and the temperature is raised to the shell coating temperature to perform inner shell coating; The sulfur source, selenium source and zinc source are added, the temperature is raised to the shell coating temperature for shell coating, and purification is performed to obtain indium phosphide core-shell quantum dots.
[0024] The removal of oxide species on the surface of indium phosphide nanocrystals is conducive to the epitaxial growth of the shell layer. After the hexafluorophosphate has acted for a period of time, only the sulfur source and selenium source are added to the reaction container, and the temperature is raised to react with the original zinc halide in the system to complete the coating of the inner shell layer. Finally, the sulfur source, selenium source and zinc source are added, and after sufficient reaction, the hexafluorophosphate-etched indium phosphide core-shell quantum dots are obtained. Compared with the core-shell quantum dots that have not been etched, the hexafluorophosphate-etched quantum dots have fewer defect sites at the core-shell interface and show better luminescence performance.
[0025] Furthermore, when a sulfur source and a selenium source are added to the reaction system for inner shell coating, the temperature is raised to 240-320° C. and the reaction is carried out for 20-120 min.
[0026] Furthermore, after adding the sulfur source, selenium source and zinc source, the temperature is raised to 180-320° C. and the reaction is carried out for 120-240 min.
[0027] Optionally, the sulfur source is at least one of sulfur powder, octyl mercaptan, and 1-dodecyl mercaptan.
[0028] Optionally, the selenium source is selenium powder and / or selenium oxide.
[0029] Optionally, the zinc source is at least one of zinc oleate, zinc stearate, zinc laurate, anhydrous zinc acetate, and zinc acetate dihydrate.
[0030] The third aspect of the present invention provides an indium phosphide core-shell quantum dot, which is prepared by etching the indium phosphide core using the above method; or prepared by the above method for preparing indium phosphide core-shell quantum dots.
[0031] A fourth aspect of the present invention provides an application of indium phosphide core-shell quantum dots in the optoelectronic field.
[0032] It is easy to know that based on the characteristics of the indium phosphide core-shell quantum dots of the present invention, they can have very wide applications in the optoelectronic field.
[0033] Specifically, the above-mentioned uses include but are not limited to using indium phosphide core-shell quantum dots to prepare light-emitting devices, fluorescent probes or fluorescent detectors, etc.
[0034] Compared with the prior art, the present invention is beneficial in that: 1. The present invention provides an etching method for indium phosphide cores. By introducing hexafluorophosphate, the oxide species and defects on the surface of indium phosphide are effectively removed, thereby improving the luminous efficiency of the indium phosphide cores. In addition, the etching conditions of this method are mild, the process is controllable, the etching effect is good, and the problem of over-etching will not occur.
[0035] 2. The present invention provides a method of using an etched indium phosphide core, using a "one-pot method" to further coat the surface of the indium phosphide core with a sulfur source, a selenium source and a zinc source to form a shell structure of ZnSeS and ZnS, thereby preparing an indium phosphide core-shell quantum dot. The indium phosphide core-shell quantum dots prepared by the present invention have significantly improved luminous efficiency, effectively inhibited the adverse effects of oxides and defect sites on the surface of the indium phosphide core, and avoided the risk of secondary oxidation of the indium phosphide core during the "two-pot method" purification process.
[0036] 3. The indium phosphide core-shell quantum dots prepared by the present invention have the advantages of excellent luminescence performance, no heavy metal elements, and environmental friendliness, and are suitable for promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The UV-visible absorption spectrum and steady-state fluorescence spectrum of the indium phosphide core etched with 0.1 mmol lithium hexafluorophosphate prepared in Example 1.
[0038] Figure 2This is the calculated fluorescence quantum yield spectrum of the 0.1 mmol lithium hexafluorophosphate-etched indium phosphide core prepared in Example 1.
[0039] Figure 3 The UV-visible absorption spectrum and steady-state fluorescence spectrum of the indium phosphide core etched with 0.3 mmol lithium hexafluorophosphate prepared in Example 2.
[0040] Figure 4 This is the calculated fluorescence quantum yield spectrum of the 0.3 mmol lithium hexafluorophosphate-etched indium phosphide core prepared in Example 2.
[0041] Figure 5 The UV-visible absorption spectrum and steady-state fluorescence spectrum of the indium phosphide core etched with 0.5 mmol lithium hexafluorophosphate prepared in Example 3.
[0042] Figure 6 This is the calculated fluorescence quantum yield spectrum of the 0.5 mmol lithium hexafluorophosphate-etched indium phosphide core prepared in Example 3.
[0043] Figure 7 The UV-visible absorption spectrum and steady-state fluorescence spectrum of the indium phosphide core prepared in Comparative Example 1.
[0044] Figure 8 This is the calculated fluorescence quantum yield spectrum of the indium phosphide core prepared in Comparative Example 1.
[0045] Fig. 9 It is a comparison chart of the steady-state fluorescence spectra and fluorescence quantum yields of the indium phosphide cores prepared in Example 3 and Comparative Example 1.
[0046] Fig.10 These are optical photographs of n-octane solutions of indium phosphide cores prepared in Comparative Example 1 and Examples 1-3 under natural light, and optical photographs under 365 nm ultraviolet light.
[0047] Fig.11 The figure is a comparison of the UV-visible absorption spectra of the indium phosphide cores prepared in Example 3 and Comparative Example 1 after being diluted by the same multiple.
[0048] Fig.12 It is the XPS fine spectrum of P(2p) of the indium phosphide core prepared in Comparative Example 1 and Example 3.
[0049] Fig.13 It is the transient fluorescence spectrum of the indium phosphide core prepared in comparative example 1 and example 3.
[0050] Fig.14 The UV-visible absorption spectrum and steady-state fluorescence spectrum of 0.1 mmol lithium hexafluorophosphate-etched indium phosphide core-shell quantum dots prepared in Example 4 are shown.
[0051] Fig.15 This is the calculated fluorescence quantum yield spectrum of 0.1 mmol lithium hexafluorophosphate-etched indium phosphide core-shell quantum dots prepared in Example 4.
[0052] Fig.16 The UV-visible absorption spectrum and steady-state fluorescence spectrum of 0.3 mmol lithium hexafluorophosphate-etched indium phosphide core-shell quantum dots prepared in Example 5 are shown.
[0053] Fig.17 This is the calculated fluorescence quantum yield spectrum of 0.3 mmol lithium hexafluorophosphate-etched indium phosphide core-shell quantum dots prepared in Example 5.
[0054] Fig.18 The UV-visible absorption spectrum and steady-state fluorescence spectrum of 0.5 mmol lithium hexafluorophosphate-etched indium phosphide core-shell quantum dots prepared in Example 6 are shown.
[0055] Fig.19 This is the calculated fluorescence quantum yield spectrum of 0.5 mmol lithium hexafluorophosphate-etched indium phosphide core-shell quantum dots prepared in Example 6.
[0056] Fig. 20 The UV-visible absorption spectrum and steady-state fluorescence spectrum of the indium phosphide core-shell quantum dots prepared in Comparative Example 2 are shown.
[0057] Fig.21 This is the calculated spectrum of the fluorescence quantum yield of the indium phosphide core-shell quantum dots prepared in Comparative Example 2.
[0058] Fig. 22 These are optical photographs of n-octane solutions of indium phosphide core-shell quantum dots prepared in Comparative Example 2 and Examples 4-6 under natural light, and optical photographs under 365 nm ultraviolet light.
[0059] Fig.23 The transient fluorescence spectra of indium phosphide core-shell quantum dots prepared in comparative example 2 and example 6 are shown.
[0060] Fig.24 The transmission electron micrographs of indium phosphide core-shell quantum dots prepared in Examples 4-6 and Comparative Example 2 are shown respectively. DETAILED DESCRIPTION
[0061] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0062] In some implementation cases of the present invention, a method for etching an indium phosphide core of an indium phosphide core-shell quantum dot is provided, wherein an indium source, a phosphorus source and a zinc halide are mixed to prepare an indium phosphide nanocrystalline core; hexafluorophosphate is dissolved in an organic solvent and added to the indium phosphide nanocrystalline core to complete the etching reaction.
[0063] Optionally, the molar ratio of the hexafluorophosphate to the indium source is 1:(1-5).
[0064] Optionally, the etching reaction condition is 180-240° C. for 5-60 min.
[0065] It should be noted that the hexafluorophosphate used in the present invention includes, but is not limited to, alkali metal salts such as lithium hexafluorophosphate (LiPF6), sodium hexafluorophosphate (NaPF6), potassium hexafluorophosphate (KPF6), and other hexafluorophosphates that can react with trace amounts of water to generate hydrogen fluoride. These hexafluorophosphates with the same effect all fall within the scope of protection of the present invention.
[0066] In some embodiments of the present invention, the hexafluorophosphate may generally be lithium hexafluorophosphate (LiPF6).
[0067] In some embodiments of the present invention, in the method for preparing the indium phosphide nanocrystal core, the molar ratio of the indium source, the phosphorus source and the zinc halide is 1:(3-5):(4-6).
[0068] Optionally, the molar ratio of the indium source, the phosphorus source and the zinc halide is 1:4:5.
[0069] In some embodiments of the present invention, the reaction conditions for preparing the indium phosphide nanocrystal core are 160-220° C. for 5-40 min.
[0070] In some specific implementation cases of the present invention, the preparation method of indium phosphide nanocrystal core is specifically as follows: weigh an indium source and a zinc halide, dissolve the two in a three-necked flask containing 5 mL of oleylamine, repeat the vacuum pumping and filling with argon (to create a protective atmosphere) operation three times to create an inert atmosphere, and then heat to a predetermined temperature and add a phosphorus source to react to prepare an indium phosphide nanocrystal core.
[0071] The indium phosphide nanocrystal core preparation process of the present invention is completed under a protective atmosphere, the purpose of which is to isolate oxygen without affecting the main reaction. Therefore, except for argon, any protective atmosphere that meets the above purpose belongs to the protection scope of the present invention.
[0072] Furthermore, the indium halide source is at least one of indium trichloride, indium tribromide, and indium triiodide.
[0073] Further, the phosphorus source is at least one aminophosphine; Furthermore, the phosphorus source is tri(dimethylamino)phosphine and / or tri(diethylamino)phosphine.
[0074] Furthermore, the zinc halide is at least one of zinc chloride, zinc bromide and zinc iodide.
[0075] In some implementation cases of the present invention, the preparation method of indium phosphide core-shell quantum dots provided is completed in the same container, and includes the following steps: Using the above-mentioned indium phosphide core etching method, preparing indium phosphide nanocrystalline cores and etching them; A sulfur source and a selenium source are added to the reaction system, and the temperature is raised to the shell coating temperature to perform inner shell coating; Adding the sulfur source, selenium source and zinc source, controlling the temperature to continue the reaction and complete the shell coating; Purification was performed to obtain indium phosphide core-shell quantum dots.
[0076] In order to minimize the oxidation defects on the surface of indium phosphide nanocrystals, the present invention adopts a "one-pot method" when preparing indium phosphide quantum dots, that is, the entire process from the synthesis and etching of indium phosphide nanocrystal cores to the final preparation of indium phosphide core-shell quantum dots is completed in the same reaction vessel. This effectively avoids the probability of indium phosphide nanocrystal cores being oxidized during the transfer process of different reaction vessels.
[0077] Furthermore, when a sulfur source and a selenium source are added to the reaction system for inner shell coating, the reaction conditions for the inner shell coating are 240-320° C. for 20-120 min.
[0078] Furthermore, the reaction conditions after adding the sulfur source, selenium source and zinc source are 180-320° C. and 120-240 min.
[0079] Furthermore, the sulfur source is at least one of sulfur powder, octyl mercaptan, and 1-dodecyl mercaptan.
[0080] Furthermore, the selenium source is selenium powder and / or selenium oxide.
[0081] Furthermore, the zinc source is at least one of zinc oleate, zinc stearate, zinc laurate, anhydrous zinc acetate, and zinc acetate dihydrate.
[0082] Example 1
[0083] The etching method of indium phosphide core provided in this embodiment comprises the following specific steps: (1) Accurately weigh 110 mg of indium trichloride and 340 mg of zinc chloride and dissolve them in a three-necked flask containing 5 mL of oleylamine; repeat the vacuum and argon filling operation three times to create an inert atmosphere (protective atmosphere).
[0084] The temperature was raised to 180°C, and a mixed solution of 0.40 mL of tri(dimethylamino)phosphine (phosphorus source) and 0.60 mL of tri-n-octylphosphine was injected. The mixture was reacted at 180°C for 30 min to obtain a reaction system containing indium phosphide cores.
[0085] (2) Add 1 mL of 0.1 M lithium hexafluorophosphate oleylamine solution (prepared by dissolving 15 mg lithium hexafluorophosphate in 1 mL oleylamine) to the reaction system, and react at 180°C for 30 min, then cool to room temperature; That is, the molar ratio of lithium hexafluorophosphate to indium trichloride is 1:5.
[0086] (3) The mixture in the reaction container was mixed with anhydrous ethanol at a volume ratio of 1:5, and the precipitate was collected by high-speed centrifugation (10,000 r / min, 5 min); Add 10 mL of n-octane, dissolve the precipitate by shaking, centrifuge at high speed (10000 r / min, 5 min), and take out the supernatant; mix the supernatant with anhydrous ethanol at a volume ratio of 1:5, and centrifuge at high speed (10000 r / min, 5 min) to obtain 0.1 mmol of indium phosphide core etched by lithium hexafluorophosphate.
[0087] Example 2
[0088] The specific steps of the indium phosphide core etching method provided in this embodiment are basically the same as those in Example 1, except that the preparation method of the lithium hexafluorophosphate oleylamine solution in step (2) is: 45 mg lithium hexafluorophosphate (0.3 mmol) is dissolved in 1 mL oleylamine. That is, the molar ratio of lithium hexafluorophosphate to indium trichloride is 3:5. Example 3
[0089] The specific steps of the indium phosphide core etching method provided in this embodiment are basically the same as those in Example 1, except that the preparation method of the lithium hexafluorophosphate oleylamine solution in step (2) is: 75 mg lithium hexafluorophosphate (0.5 mmol) is dissolved in 1 mL oleylamine. That is, the molar ratio of lithium hexafluorophosphate to indium trichloride is 1:1. Example 4: The method of Example 1 is used to etch the indium phosphide core and prepare indium phosphide core-shell quantum dots.
[0090] The preparation method of indium phosphide core-shell quantum dots provided in this embodiment is as follows: Step 1: The same as step (1) of Example 1. Accurately weigh 110 mg of indium trichloride and 340 mg of zinc chloride, and dissolve them in a three-necked flask containing 5 mL of oleylamine; repeat the vacuum and argon filling operation three times to create an inert atmosphere (protective atmosphere).
[0091] The temperature was raised to 180°C, and a mixed solution of 0.40 mL of tri(dimethylamino)phosphine (phosphorus source) and 0.60 mL of tri-n-octylphosphine was injected. The mixture was reacted at 180°C for 30 min to obtain a reaction system containing indium phosphide cores.
[0092] Step 2: Similar to step (2) of Example 1. 1 mL of 0.1 M lithium hexafluorophosphate oleylamine solution (prepared by dissolving 15 mg lithium hexafluorophosphate in 1 mL oleylamine) was added to the reaction system, and the mixture was reacted at 180°C for 10 min. That is, the molar ratio of lithium hexafluorophosphate to indium trichloride is 1:5.
[0093] Step 3: Quickly inject the prepared sulfur source (64 mg of sulfur powder dissolved in 1 mL of tri-n-octylphosphine) and selenium source (126 mg of selenium powder dissolved in 1.6 mL of tri-n-octylphosphine) into the three-necked flask at the same time; heat to 280°C and react at a constant temperature for 60 min.
[0094] Step 4: Simultaneously inject the pre-prepared sulfur source (128 mg of sulfur powder dissolved in 2 mL of tri-n-octylphosphine), selenium source (79 mg of selenium powder dissolved in 1 mL of tri-n-octylphosphine) and zinc source (1265 mg of zinc stearate dissolved in 4 mL of 1-octadecene), and heat to 290°C for 60 min.
[0095] Step 5: Inject the previously prepared sulfur source (192 mg of sulfur powder dissolved in 3 mL of tri-n-octylphosphine), selenium source (32 mg of selenium powder dissolved in 0.4 mL of tri-n-octylphosphine) and zinc source (1265 mg of zinc stearate dissolved in 4 mL of 1-octadecene) simultaneously again, raise the temperature to 300°C and react at a constant temperature for 60 min.
[0096] Step 6: After the reaction, the temperature of the reaction system was quickly lowered to 230°C, 2 mL of octanethiol was injected and the reaction was kept at a constant temperature for 60 min; the temperature of the reaction system was further lowered to 190°C, a mixed solution containing 460 mg of zinc acetate dihydrate and 2 mL of oleic acid was injected and the reaction was kept at a constant temperature for 30 min to complete the shell coating.
[0097] Step 7: Remove the heat source and cool the reaction system to room temperature by using an ice-water bath; mix the mixture in the reaction container with anhydrous ethanol at a volume ratio of 1:3, and collect the precipitate by high-speed centrifugation (10,000 r / min, 5 min); Add 10 mL of n-octane, dissolve the precipitate fully by shaking, and remove the supernatant after high-speed centrifugation (10,000 r / min, 5 min); The supernatant was mixed with anhydrous ethanol in a volume ratio of 1:3 and centrifuged at high speed (10000 r / min, 5 min) to obtain 0.1 mmol lithium hexafluorophosphate-etched indium phosphide core-shell quantum dots. Example 5: The method of Example 2 is used to etch the indium phosphide core and prepare indium phosphide core-shell quantum dots.
[0098] The preparation method of indium phosphide core-shell quantum dots provided in this embodiment is basically the same as that of embodiment 4, except that: the etching of the indium phosphide core is carried out in the manner of embodiment 2, that is, the amount of lithium hexafluorophosphate added in step 2 is adjusted to 45 mg (45 mg lithium hexafluorophosphate is dissolved in 1 mL oleylamine), and the molar ratio of lithium hexafluorophosphate to indium trichloride is 3:5; other steps and conditions remain unchanged. Example 6: The method of Example 3 is used to etch the indium phosphide core and prepare indium phosphide core-shell quantum dots.
[0099] The preparation method of indium phosphide core-shell quantum dots provided in this embodiment is basically the same as that of embodiment 4, except that: the etching of the indium phosphide core is carried out in the manner of embodiment 3, that is, the amount of lithium hexafluorophosphate added in step 2 is adjusted to 75 mg (75 mg of lithium hexafluorophosphate is dissolved in 1 mL of oleylamine), and the molar ratio of lithium hexafluorophosphate to indium trichloride is 1:1; other steps and conditions remain unchanged. Comparative Example 1: Preparation of indium phosphide cores without lithium hexafluorophosphate etching.
[0100] The preparation method of the indium phosphide core of this comparative example is based on Example 1, except that the etching process of adding lithium hexafluorophosphate in step (2) is deleted, and the other steps and conditions remain unchanged. The specific steps are: (1) Accurately weigh 110 mg of indium trichloride and 340 mg of zinc chloride and dissolve them in a three-necked flask containing 5 mL of oleylamine; repeat the vacuum and argon filling operation three times to create an inert atmosphere (protective atmosphere).
[0101] The temperature was raised to 180°C, and a mixed solution of 0.40 mL of tri(dimethylamino)phosphine (phosphorus source) and 0.60 mL of tri-n-octylphosphine was injected. The mixture was reacted at 180°C for 30 min to obtain a reaction system containing indium phosphide cores, and then cooled to room temperature. (2) The mixture in the reaction container was mixed with anhydrous ethanol at a volume ratio of 1:5, and the precipitate was collected by high-speed centrifugation (10,000 r / min, 5 min); Add 10 mL of n-octane, dissolve the precipitate fully by shaking, centrifuge at high speed (10000 r / min, 5 min), and take out the supernatant; mix the supernatant with anhydrous ethanol at a volume ratio of 1:5, and centrifuge at high speed (10000 r / min, 5 min) to obtain the indium phosphide core that has not been etched by lithium hexafluorophosphate. Comparative Example 2: Using indium phosphide cores that have not been etched with lithium hexafluorophosphate, corresponding indium phosphide core-shell quantum dots were prepared.
[0102] Step 1: The same as step (1) of Example 1. Accurately weigh 110 mg of indium trichloride and 340 mg of zinc chloride, and dissolve them in a three-necked flask containing 5 mL of oleylamine; repeat the vacuum and argon filling operation three times to create an inert atmosphere (protective atmosphere).
[0103] The temperature was raised to 180°C, and a mixed solution of 0.40 mL of tri(dimethylamino)phosphine (phosphorus source) and 0.60 mL of tri-n-octylphosphine was injected. The mixture was reacted at 180°C for 30 min to obtain a reaction system containing indium phosphide cores.
[0104] Step 2: Cool the reaction system to room temperature; quickly inject the prepared sulfur source (64 mg of sulfur powder dissolved in 1 mL of tri-n-octylphosphine) and selenium source (126 mg of selenium powder dissolved in 1.6 mL of tri-n-octylphosphine) into the three-necked flask at the same time; heat to 280°C and react at a constant temperature for 60 min.
[0105] Step 3: Simultaneously inject the pre-prepared sulfur source (128 mg of sulfur powder dissolved in 2 mL of tri-n-octylphosphine), selenium source (79 mg of selenium powder dissolved in 1 mL of tri-n-octylphosphine) and zinc source (1265 mg of zinc stearate dissolved in 4 mL of 1-octadecene), and heat to 290°C for 60 min.
[0106] Step 4: Add the previously prepared sulfur source (192 mg of sulfur powder dissolved in 3 mL of tri-n-octylphosphine), selenium source (32 mg of selenium powder dissolved in 0.4 mL of tri-n-octylphosphine) and zinc source (1265 mg of zinc stearate dissolved in 4 mL of 1-octadecene) at the same time, raise the temperature to 300°C and react for 60 min.
[0107] Step 5: After the reaction, the temperature of the reaction system was quickly lowered to 230°C, 2 mL of octanethiol was injected and the reaction was kept at a constant temperature for 60 min; the temperature of the reaction system was further lowered to 190°C, a mixed solution containing 460 mg of zinc acetate dihydrate and 2 mL of oleic acid was injected and the reaction was kept at a constant temperature for 30 min to complete the coating of the shell layer; Step 6: Remove the heat source and cool the reaction system to room temperature by using an ice-water bath; mix the mixture in the reaction container with anhydrous ethanol at a volume ratio of 1:3, and collect the precipitate by high-speed centrifugation (10,000 r / min, 5 min); Add 10 mL of n-octane, dissolve the precipitate fully by shaking, and remove the supernatant after high-speed centrifugation (10,000 r / min, 5 min); The supernatant was mixed with anhydrous ethanol in a volume ratio of 1:3 and centrifuged at high speed (10000 r / min, 5 min) to obtain indium phosphide core-shell quantum dots that were not etched by lithium hexafluorophosphate.
[0108] Experimental example: Characterization and performance testing of indium phosphide core and indium phosphide core-shell quantum dots The indium phosphide cores prepared in Examples 1-3 and Comparative Example 1, and the indium phosphide core-shell quantum dots prepared in Examples 4-6 and Comparative Example 2 were characterized, and the obtained UV-visible absorption spectra, steady-state fluorescence spectra, fluorescence quantum yield calculation spectra, transient fluorescence spectra, X-ray photoelectron spectra, transmission electron microscopy images, etc. were shown in Figure 2. Figure 1-24 The key data related to the optical performance are shown in Table 1, and the fitting results of the transient fluorescence spectrum are shown in Table 2.
[0109] 1. Characterization and analysis of the indium phosphide cores prepared in Examples 1-3 and Comparative Example 1.
[0110] like Figure 7 , 8 As shown in Figures 10 and 11, the characterization results of Comparative Example 1 show that the emission peak of the InP core without LiPF6 etching is located at 599 nm, and it hardly emits light under ultraviolet light, and the photoluminescence quantum yield is less than 1%. The InP core exhibits obvious defect state luminescence near 700 nm. The presence of defect state energy levels near the conduction band and the valence band broadens its emission spectrum, and the half-peak width exceeds 70 nm.
[0111] like Figure 1-6 As shown, the luminescence performance of the InP core after etching with LiPF6 in Examples 1-3 is improved. When the amount of LiPF6 added is 0.1 mmol, 0.3 mmol and 0.5 mmol, the emission peaks of the obtained InP core are located at 609nm, 606 nm and 609 nm, respectively, and the photoluminescence quantum yields are 6%, 14% and 22%, respectively. The steady-state fluorescence spectrum shows that the steady-state fluorescence spectrum of the InP core modified with LiPF6 is narrowed (the half-peak width is about 60nm), and the defect state luminescence near 700nm is suppressed.
[0112] like Fig. 9 As shown, by comparing the emission spectra and quantum yields of the 0.5 mmol LiPF6-modified InP core prepared in Example 3 and the unmodified InP core prepared in Comparative Example 1 under the same light source excitation, the positive effect of LiPF6 modification on improving the luminescence performance of the InP core is further revealed.
[0113] like Fig.10As shown, under the irradiation of ultraviolet light, the luminescence of the InP core prepared in Comparative Example 1 and Implementations 1-3 gradually increases, which is consistent with the change trend of the measured quantum yield.
[0114] Since colloidal quantum dots exhibit an intrinsic absorption coefficient close to that of bulk materials at short wavelengths, the molar amount of quantum dots in the measured solution can be calculated by measuring the absorbance at a specific wavelength. For the InP cores obtained after purification in Example 3 and Comparative Example 1, 1 / 300 of the total amount of samples were taken and dissolved in 3 mL of n-octane to test the UV-visible absorption spectrum. The results are as follows: Fig.11 As shown. It can be seen that the absorbance of the InP core modified with 0.5 mmol LiPF6 at 413 nm is 0.27, which is significantly lower than that of the InP core not modified with LiPF6 (0.42). This shows that the molar amount of the InP core prepared in Example 3 is less than that of the InP core prepared in Comparative Example 1, and the introduction of LiPF6 has an etching effect on the InP core.
[0115] Fig.12 By comparing the X-ray photoelectron (XPS) spectra of the InP core prepared in Example 3 and Comparative Example 1, it is fully proved that the introduction of LiPF6 effectively removes the phosphine oxide (InPO x ).
[0116] In order to further understand the decay process of the excited state of the material, transient fluorescence spectroscopy tests were performed on the InP cores prepared in Example 3 and Comparative Example 1. The results are as follows: Fig.13 The measured transient fluorescence spectra all conform to the double exponential decay kinetics, and the fast decay process ( τ 1) and slow decay process ( τ 2) are respectively related to the band edge recombination of excitons and the recombination involving defect states. According to the fitting results in Table 2 below, for the InP cores prepared in Example 3 and Comparative Example 1, the proportion of band edge recombination is 61.4% and 51.2%, respectively, and the proportion of defect states participating in recombination is 38.6% and 21.5%, respectively. It can be seen that after LiPF6 modification, the defect states of the InP core are effectively passivated / eliminated, the proportion of band edge recombination increases, and the proportion of defect state luminescence decreases.
[0117] 2. Characterization and analysis of the indium phosphide core-shell quantum dots prepared in Examples 4-6 and Comparative Example 2.
[0118] By coating ZnSeS and ZnS shells under the same conditions, Examples 4-6 and Comparative Example 2 explored the effect of LiPF6 on the luminescence properties of indium phosphide core-shell quantum dots.
[0119] Fig. 20 and 21It shows that the emission peak of the InP core-shell quantum dots prepared in Comparative Example 2 without LiPF6 modification is located at 614nm, and the photoluminescence quantum yield is 62%.
[0120] like Figure 14-19 As shown, after the InP core is etched by introducing LiPF6, the luminescence performance of the core-shell quantum dots prepared in Examples 4-6 is significantly improved. When the amount of LiPF6 introduced is 0.1 mmol, 0.3 mmol and 0.5 mmol, the emission peaks of the obtained core-shell quantum dots are located at 616 nm, 618 nm and 621 nm, respectively, and the photoluminescence quantum yields are 76%, 84% and 85%, respectively. As the amount of LiPF6 introduced increases, the luminescence efficiency of the obtained quantum dots gradually increases, accompanied by a gradual red shift in the emission spectrum.
[0121] Fig. 22 Optical photographs of n-octane solutions of InP core-shell quantum dots prepared in Comparative Example 2 and Examples 4-6 under natural light and 365 nm ultraviolet light are intuitively shown.
[0122] By comparing the transient fluorescence spectra of the core-shell quantum dots obtained in Example 6 with those in Comparative Example 2 ( Fig.23 ) and the fitting results (Table 2) show that the proportion of band edge recombination in the former reaches 89.0%, which is significantly higher than the 78.5% in the latter. The transient fluorescence spectrum results strongly prove the passivation ability of LiPF6 on the surface defects of InP core and the improvement of the luminescence efficiency of InP core and InP core-shell quantum dots.
[0123] Using ultra-thin carbon film as a carrier, the morphology of the InP core-shell quantum dots prepared in Examples 4-6 and Comparative Example 2 was characterized by a transmission electron microscope (JEM-2100Plus). Fig.24 The morphologies of the above four core-shell quantum dots are similar, all close to triangular pyramids.
[0124] Table 1 Optical properties of InP core and core-shell quantum dots
[0125] Table 2 Fitting results of transient fluorescence spectra of indium phosphide core and core-shell quantum dots
[0126] The above specific embodiments describe the implementation of the present invention in detail, but the present invention is not limited to the specific details in the above embodiments. Within the scope of the claims and technical concept of the present invention, the technical solution of the present invention can be modified and changed in many simple ways, and these simple modifications all belong to the protection scope of the present invention.
Claims
1. A method for etching an indium phosphide core of an indium phosphide core-shell quantum dot, characterized in that: An indium source, a phosphorus source and a zinc halide are mixed to prepare an indium phosphide nanocrystal core; hexafluorophosphate is dissolved in an organic solvent and added to the indium phosphide nanocrystal core for etching.
2. The etching method of indium phosphide core of indium phosphide core-shell quantum dots according to claim 1, characterized in that: The molar ratio of the hexafluorophosphate to the indium element in the indium source used to prepare the indium phosphide nanocrystal core is 1:(1-5).
3. The etching method of indium phosphide core of indium phosphide core-shell quantum dots according to claim 1, characterized in that: The etching reaction conditions are 180-240° C. for 5-60 min.
4. The etching method of indium phosphide core of indium phosphide core-shell quantum dots according to claim 1, characterized in that: The molar ratio of the indium source, the phosphorus source and the zinc halide is 1:(3-5):(4-6).
5. The etching method of indium phosphide core of indium phosphide core-shell quantum dots according to claim 1, characterized in that: The reaction conditions for preparing the indium phosphide nanocrystal core are 160-220° C. for 5-40 min.
6. The method for etching the indium phosphide core of the indium phosphide core-shell quantum dots according to claim 1, characterized in that: The indium source is at least one of indium trichloride, indium tribromide and indium triiodide; the phosphorus source is at least one aminophosphine; and the zinc halide is at least one of zinc chloride, zinc bromide and zinc iodide.
7. A method for preparing indium phosphide core-shell quantum dots, characterized in that: The following steps are involved: Etching the indium phosphide nanocrystal core using the indium phosphide core etching method of indium phosphide core-shell quantum dots according to any one of claims 1 to 6; A sulfur source and a selenium source are added to the reaction system, and the temperature is raised to perform inner shell coating; Sulfur source, selenium source and zinc source are added, and the temperature is controlled to continue the reaction to complete the shell coating; Purification was performed to obtain indium phosphide core-shell quantum dots.
8. The method for preparing indium phosphide core-shell quantum dots according to claim 7, characterized in that: The reaction conditions for the inner shell coating are 240-320° C. for 20-120 min; and the reaction conditions after adding the sulfur source, selenium source and zinc source are 180-320° C. for 120-240 min.
9. An indium phosphide core-shell quantum dot, characterized in that: The method is used to etch the indium phosphide core according to any one of claims 1 to 6; or the method is used to prepare the indium phosphide core according to claim 7.