Method for using aluminum electrolysis waste carbon in fuming furnace
By treating aluminum electrolytic waste carbon as a reducing agent for the smoke furnace, the problems of incomplete treatment of aluminum electrolytic waste carbon and shortage of coal are solved, efficient utilization of resources and environmental sustainability are achieved, and smoke is reduced Energy consumption and carbon emissions of furnaces.
Patent Information
- Application Number
- CN202410998310.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, aluminum electrolytic waste carbon treatment process cannot be completely recycled or widely used, and there is a shortage of reducing agents such as coal in the fume furnace, resulting in waste of resources and environmental pollution.
By vacuum distillation, wet leaching or flotation on aluminum electrolytic waste carbon, composite reducing agents are made or secondary waste carbon is used alone as the reducing agent for the fume furnace, and the smelting parameters are adjusted to reduce the reduction temperature and volatility. reduce the amount of coal, and control the amount of fluorine element to avoid the formation of dangerous solid waste residue.
It realizes the efficient utilization of aluminum electrolytic waste carbon, reduces coal consumption, reduces energy consumption and carbon emissions of fume furnaces, and avoids the generation of new hazardous solid waste, and has good industrial application prospects.
Smart Images

Figure CN118996124A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fuming furnace technology, and in particular relates to a method for using aluminum electrolysis waste carbon in a fuming furnace. Background Art
[0002] China is a major producer of electrolytic aluminum. In 2023, China's total electrolytic aluminum production reached 41.594 million tons. Due to the selective oxidation and mechanical loss of the carbon anodes and cathodes used in aluminum electrolysis during the electrolysis process, some carbon components fall into the electrolyte, increasing the electrolyte resistance and reducing the current efficiency. The fallen carbon electrodes are regularly salvaged from the electrolytic cell by production personnel during the production process and form carbon slag after cooling. Carbon slag was identified as a national hazardous waste in 2016. my country's electrolytic aluminum industry produces more than 300,000 tons of carbon slag each year, which contains important valuable resources such as carbon, cryolite and calcium fluoride. Waste cathode carbon blocks from electrolytic aluminum are solid wastes generated during the dismantling of aluminum electrolytic cells. They contain a large amount of fluoride and cyanide. The fluoride content is generally 20%-40%, and the cyanide content is about 100g / t. They are clearly listed as hazardous wastes in the "National List of Hazardous Wastes" and are numbered 321-023-HW48. If these hazardous wastes are not used or disposed of in a timely manner, a large amount of fluoride salts, cyanide and other toxic substances in the waste cathode carbon blocks will gradually transfer to the atmosphere, soil and groundwater through wind, sun and rain, seriously affecting the health and survival of animals, plants and humans. Waste cathode carbon blocks from electrolytic aluminum contain useful minerals C, NaF, cryolite and CaF2, and the purity of the mineral C reaches a high level. After treatment, it can be prepared into a carbonaceous reducing agent.
[0003] As a traditional fossil fuel, coal has long occupied an important position in the global energy structure. It is widely used in power generation, metal smelting production, cement manufacturing and as an industrial energy source. However, with the increasingly severe global climate change problem, as well as the challenges of environmental pollution and sustainable development, the control of coal energy has become an important issue in global energy policy. In order to cope with environmental and climate issues, many countries and regions have implemented a series of policies, regulations and measures to strengthen the control of coal energy. These measures include restricting the construction of new coal-fired power plants, raising emission standards, imposing carbon taxes, and providing renewable energy subsidies. Coal is consumed in large quantities every year as a reducing agent for lead smelting, and coal energy control also has a certain impact on the fuming furnace industry. Summary of the invention
[0004] In order to solve the problems existing in the prior art that the secondary carbonaceous waste slag obtained by the aluminum electrolysis waste carbon treatment process cannot be completely recovered or utilized in large quantities, and that reducing agents such as coal in fuming furnaces are in short supply, the purpose of the present invention is to provide a method for using aluminum electrolysis waste carbon in a fuming furnace. The present application uses secondary waste carbon from aluminum electrolysis waste carbon treated by vacuum distillation, wet leaching or flotation to prepare a composite reducing agent with traditional reducing agents such as coal and coke, or uses secondary waste carbon alone as a reducing agent, or uses aluminum electrolysis waste carbon without any treatment as a reducing agent for fuming furnace production. According to the secondary waste carbon with different treatment degrees, the important smelting parameters such as the primary air dosage, secondary air dosage, oxygen concentration, reduction temperature, slag-making agent and reduction time of the fuming furnace production are adjusted, and the fluoride mixed in the aluminum electrolysis waste carbon is converted into calcium fluoride, which can improve the fluidity and surface tension of the slag, reduce the reduction smelting temperature of the fuming furnace, and increase the volatilization rate of the material in the fuming furnace. At the same time, by controlling the amount of fluorine introduced, the generation of dangerous solid waste slag is avoided. Moreover, by using the secondary waste carbon treated in various ways as a fuming furnace reducing agent, the amount of the original reducing agent coal can be reduced, thereby realizing the green energy saving and carbon reduction of the lead smelting reduction furnace.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A method for using waste carbon from aluminum electrolysis in a fuming furnace, the method comprising the following steps:
[0007] (1) Pre-treating the aluminum electrolysis waste carbon and removing the volatile matter by high-temperature vacuum distillation to obtain secondary waste carbon;
[0008] (2) preparing a composite reducing agent by mixing the secondary waste carbon obtained in step (1) with a reducing agent such as granular carbon, coal, coke, etc. at a mass ratio of 1:100-100:1;
[0009] (3) Adding the composite reducing agent obtained in step (2) into a fuming furnace to perform a reduction operation.
[0010] Furthermore, the aluminum electrolysis waste carbon in step (1) can also be pretreated by high-temperature non-vacuum distillation, ultra-high temperature vacuum treatment, wet flotation or mechanical crushing and physical separation.
[0011] Furthermore, the aluminum electrolysis waste carbon in step (1) is aluminum electrolysis waste carbon that has not been pretreated in any way.
[0012] Furthermore, the composite reducing agent in step (2) also includes distilled anode carbon slag or waste cathode carbon blocks.
[0013] Furthermore, in step (2), the composite reducing agent is in any of powder, granular or block form.
[0014] Furthermore, the fuming furnace in step (3) is any one of a side-blown furnace, a top-blown furnace, a vacuum tube furnace or a bottom-blown furnace.
[0015] Furthermore, in step (3), the melt reduction temperature in the fuming furnace is 100-1800°C; the primary air consumption and secondary air consumption of the lead smelting reduction furnace are both 0-10000Nm 3 / h; the primary air oxygen concentration and the secondary air oxygen concentration of the lead smelting reduction furnace are both 20%-100%, and the reduction time of the lead smelting reduction furnace is 1-1000min; the slag-forming agent in the lead smelting reduction furnace includes any one or more of lime, limestone, quartz, iron ore, fluorite or dolomite.
[0016] Furthermore, the chemical reaction occurring in the fuming furnace in step (3) is as follows:
[0017] PbO+C=Pb+CO;
[0018] PbO+CO=Pb+CO2;
[0019] ZnO+C=Zn+CO;
[0020] ZnO+CO=Zn+CO2.
[0021] Furthermore, the chemical reaction occurring in the fuming furnace in step (3) also includes the following reaction:
[0022] 2AlF3+3CaO=Al2O3+3CaF2;
[0023] 2Na3AlF6+6CaO+3SiO2=Al2O3+6CaF2+3Na2SiO3;
[0024] 2NaF+CaO+SiO2=CaF2+Na2SiO3;
[0025] 4NaCN+9O2+2SiO2=2Na2SiO3+4NO2+4CO2;
[0026] 2NaCN+4O2+SiO2=Na2SiO3+N2O3+2CO2.
[0027] Compared with the prior art, the present invention has the following positive and beneficial effects:
[0028] The present invention provides a method for using waste carbon from aluminum electrolysis in a fuming furnace. Through this method, the present invention can not only efficiently and greenly utilize a large amount of hazardous solid wastes such as anode carbon slag and waste cathode carbon blocks generated in the aluminum electrolysis production process, but also can replace the coal consumption of the fuming furnace process system with energy. At the same time, the method of the present invention not only consumes the hazardous solid waste and waste carbon generated by aluminum electrolysis, but also achieves energy saving and carbon reduction in the production of the fuming furnace, and does not generate new hazardous solid waste. The entire process has a good industrial application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a process flow chart of a method for using waste carbon from aluminum electrolysis in a fuming furnace in the present invention;
[0030] Figure 2 is a phase analysis diagram of tailings after reduction in Example 1 of the present invention;
[0031] Figure 3 is a phase analysis diagram of tailings after reduction in Example 2 of the present invention;
[0032] Figure 4 This is a phase analysis diagram of the tailings after reduction in Example 5 of the present invention. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is further described below in conjunction with the embodiments, but is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.
[0034] Example 1
[0035] A method for using waste carbon from aluminum electrolysis in a fuming furnace, the specific process flow chart of the method is as follows: Figure 1 As shown, the specific steps include:
[0036] (1) crushing the waste carbon from aluminum electrolysis (waste cathode carbon blocks) to a particle size of 1-3 cm, vacuum distilling at 1100° C. and 30 Pa for 2 h to obtain secondary waste carbon, which is then ground to less than 200 mesh;
[0037] (2) mixing the spent cathode carbon blocks ground in step (1) with high zinc slag from a fuming furnace in a mass ratio of 100:20, adding 2% of the total mass of the high zinc slag as a slagging agent, and then preparing into pellets;
[0038] (3) The pellets prepared in step (2) are placed in a crucible, and then the crucible is placed in a vacuum tube furnace for smelting at a smelting temperature of 1350°C, a smelting time of 2h, and a primary air consumption of 2000Nm 3 / h, secondary air consumption 1000Nm3 / h, the oxygen concentration of the wind is 21%. After smelting reduction, it is found that the phase analysis diagram of high zinc slag after reduction is as follows Figure 2 As shown, from Figure 2 It can be seen that the main phases of the tailings after reduction are calcium ferrite, calcium orthosilicate and olivine, and there is no obvious zinc-containing phase, which shows that the reduction effect of the high-tech slag is good and meets the experimental expectations; according to the residual zinc content in the high-zinc slag of the fuming furnace, the reduction rate of zinc in the high-zinc slag of the fuming furnace is calculated to be 80.52%; the chemical reactions occurring in the vacuum tube furnace are as follows:
[0039] PbO+C=Pb+CO;
[0040] PbO+CO=Pb+CO2;
[0041] ZnO+C=Zn+CO;
[0042] ZnO+CO=Zn+CO2;
[0043] 2AlF3+3CaO=Al2O3+3CaF2;
[0044] 2Na3AlF6+6CaO+3SiO2=Al2O3+6CaF2+3Na2SiO3;
[0045] 2NaF+CaO+SiO2=CaF2+Na2SiO3;
[0046] 4NaCN+9O2+2SiO2=2Na2SiO3+4NO2+4CO2;
[0047] 2NaCN+4O2+SiO2=Na2SiO3+N2O3+2CO2.
[0048] Example 2
[0049] A method for using waste carbon from aluminum electrolysis in a fuming furnace, comprising the following steps:
[0050] (1) crushing the waste carbon from aluminum electrolysis (waste cathode carbon blocks) into a particle size of 1-3 cm, vacuum distilling at 1100° C. and 30 Pa for 2 h to obtain secondary waste carbon, and grinding it to less than 200 mesh;
[0051] (2) mixing the waste cathode carbon block ground in step (1) with the granular carbon powder in a mass ratio of 1:1 to prepare a composite reducing agent;
[0052] (3) the composite reducing agent prepared in step (2) is mixed evenly with the high zinc slag used in the fuming furnace in a mass ratio of 100:10, and 2% of the total mass of the high zinc slag is added as a slagging agent, and then prepared into pellets;
[0053] (4) The pellets prepared in step (3) are placed in a crucible, and then the crucible is placed in a vacuum tube furnace for smelting at a smelting temperature of 1250°C, a smelting time of 2h, and a primary air consumption of 2000Nm 3 / h, secondary air consumption 1000Nm 3 / h, the oxygen concentration of the wind is 21%. After smelting reduction, it is found that the phase analysis diagram of high zinc slag after reduction is as follows Figure 3 As shown, from Figure 3 It can be seen that the main phases of the tailings after reduction are calcium zinc silicate, calcium iron olivine and silicon dioxide, and the diffraction peaks of the calcium zinc silicate phase are obvious, which indicates that the reduction effect of the high-tech slag is poor, and a large amount of zinc is still not reduced; according to the residual zinc content in the high-zinc slag of the fuming furnace, the reduction rate of zinc in the high-zinc slag of the fuming furnace is calculated to be 75.34%; the chemical reactions occurring in the vacuum tube furnace are as follows:
[0054] PbO+C=Pb+CO;
[0055] PbO+CO=Pb+CO2;
[0056] ZnO+C=Zn+CO;
[0057] ZnO+CO=Zn+CO2;
[0058] 2AlF3+3CaO=Al2O3+3CaF2;
[0059] 2Na3AlF6+6CaO+3SiO2=Al2O3+6CaF2+3Na2SiO3;
[0060] 2NaF+CaO+SiO2=CaF2+Na2SiO3;
[0061] 4NaCN+9O2+2SiO2=2Na2SiO3+4NO2+4CO2;
[0062] 2NaCN+4O2+SiO2=Na2SiO3+N2O3+2CO2.
[0063] Example 3
[0064] A method for using waste carbon from aluminum electrolysis in a fuming furnace, comprising the following steps:
[0065] (1) crushing the waste carbon from aluminum electrolysis (waste cathode carbon blocks) to a particle size of 1-3 cm, vacuum distilling at 1100° C. and 30 Pa for 2 h to obtain secondary waste carbon, which is then ground to less than 200 mesh;
[0066] (2) mixing the waste cathode carbon block ground in step (1) with the granular carbon powder in a mass ratio of 2:1 to prepare a composite reducing agent;
[0067] (3) the composite reducing agent prepared in step (2) is mixed evenly with the high zinc slag used in the fuming furnace in a mass ratio of 100:20, and 2% of the total mass of the high zinc slag is added as a slagging agent, and then prepared into pellets;
[0068] (4) The pellets prepared in step (3) are placed in a crucible, and then the crucible is placed in a vacuum tube furnace for smelting at a smelting temperature of 1350°C, a smelting time of 2h, and a primary air consumption of 2000Nm 3 / h, secondary air consumption 1000Nm 3 / h, the oxygen concentration of the wind is 21%. After smelting reduction, it was found that the reduction rate of zinc in the high zinc slag of the fuming furnace was 81.59% based on the residual zinc content in the high zinc slag of the fuming furnace; the chemical reactions occurring in the vacuum tube furnace are as follows:
[0069] PbO+C=Pb+CO;
[0070] PbO+CO=Pb+CO2;
[0071] ZnO+C=Zn+CO;
[0072] ZnO+CO=Zn+CO2;
[0073] 2AlF3+3CaO=Al2O3+3CaF2;
[0074] 2Na3AlF6+6CaO+3SiO2=Al2O3+6CaF2+3Na2SiO3;
[0075] 2NaF+CaO+SiO2=CaF2+Na2SiO3;
[0076] 4NaCN+9O2+2SiO2=2Na2SiO3+4NO2+4CO2;
[0077] 2NaCN+4O2+SiO2=Na2SiO3+N2O3+2CO2.
[0078] Example 4
[0079] A method for using waste carbon from aluminum electrolysis in a fuming furnace, comprising the following steps:
[0080] (1) crushing the waste carbon from aluminum electrolysis (waste cathode carbon blocks) to a particle size of 1-3 cm, vacuum distilling at 1100° C. and 30 Pa for 2 h to obtain secondary waste carbon, which is then ground to less than 200 mesh;
[0081] (2) mixing the waste cathode carbon block ground in step (1) with the granular carbon powder in a mass ratio of 1:2 to prepare a composite reducing agent;
[0082] (3) the composite reducing agent prepared in step (2) is mixed evenly with the high zinc slag used in the fuming furnace in a mass ratio of 100:20, and 2% of the total mass of the high zinc slag is added as a slagging agent, and then prepared into pellets;
[0083] (4) The pellets prepared in step (3) are placed in a crucible, and then the crucible is placed in a vacuum tube furnace for smelting at a smelting temperature of 1350°C, a smelting time of 2h, and a primary air consumption of 2000Nm 3 / h, secondary air consumption 1000Nm 3 / h, the oxygen concentration of the wind is 21%. After smelting reduction, it was found that the reduction rate of zinc in the high zinc slag of the fuming furnace was 87.65% based on the residual zinc content in the high zinc slag of the fuming furnace; the chemical reactions occurring in the vacuum tube furnace are as follows:
[0084] PbO+C=Pb+CO;
[0085] PbO+CO=Pb+CO2;
[0086] ZnO+C=Zn+CO;
[0087] ZnO+CO=Zn+CO2;
[0088] 2AlF3+3CaO=Al2O3+3CaF2;
[0089] 2Na3AlF6+6CaO+3SiO2=Al2O3+6CaF2+3Na2SiO3;
[0090] 2NaF+CaO+SiO2=CaF2+Na2SiO3;
[0091] 4NaCN+9O2+2SiO2=2Na2SiO3+4NO2+4CO2;
[0092] 2NaCN+4O2+SiO2=Na2SiO3+N2O3+2CO2.
[0093] Example 5
[0094] A method for using waste carbon from aluminum electrolysis in a fuming furnace, comprising the following steps:
[0095] (1) crushing the waste carbon from aluminum electrolysis (waste cathode carbon blocks) to a particle size of 1-3 cm, vacuum distilling at 1100° C. and 30 Pa for 2 h to obtain secondary waste carbon, which is then ground to less than 200 mesh;
[0096] (2) mixing the waste cathode carbon block ground in step (1) with the granular carbon powder in a mass ratio of 1:5 to prepare a composite reducing agent;
[0097] (3) the composite reducing agent prepared in step (2) is mixed evenly with the high zinc slag used in the fuming furnace in a mass ratio of 100:30, and 2% of the total mass of the high zinc slag is added as a slagging agent, and then prepared into pellets;
[0098] (4) The pellets prepared in step (3) are placed in a crucible, and then the crucible is placed in a vacuum tube furnace for smelting at a smelting temperature of 1350°C, a smelting time of 2h, and a primary air consumption of 2000Nm 3 / h, secondary air consumption 1000Nm 3 / h, the oxygen concentration of the wind is 21%. After smelting reduction, it is found that the phase analysis diagram of high zinc slag after reduction is as follows Figure 4 As shown, from Figure 4 It can be seen that the main phases of the tailings after reduction are calcium ferrite and olivine, and there is no obvious zinc-containing phase, which shows that the reduction effect of the high-tech slag is good and meets the experimental expectations; according to the residual zinc content in the high-zinc slag of the fuming furnace, the reduction rate of zinc in the high-zinc slag of the fuming furnace is calculated to be 90.26%; the chemical reactions occurring in the vacuum tube furnace are as follows:
[0099] PbO+C=Pb+CO;
[0100] PbO+CO=Pb+CO2;
[0101] ZnO+C=Zn+CO;
[0102] ZnO+CO=Zn+CO2;
[0103] 2AlF3+3CaO=Al2O3+3CaF2;
[0104] 2Na3AlF6+6CaO+3SiO2=Al2O3+6CaF2+3Na2SiO3;
[0105] 2NaF+CaO+SiO2=CaF2+Na2SiO3;
[0106] 4NaCN+9O2+2SiO2=2Na2SiO3+4NO2+4CO2;
[0107] 2NaCN+4O2+SiO2=Na2SiO3+N2O3+2CO2.
[0108] Obviously, the above embodiments are only examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from them are still within the protection scope of the invention.
Claims
1. A method for using waste carbon from aluminum electrolysis in a fuming furnace, It is characterized in that The method comprises the following steps: (1) Pre-treating the aluminum electrolysis waste carbon and removing the volatile matter by high-temperature vacuum distillation to obtain secondary waste carbon; (2) preparing a composite reducing agent by mixing the secondary waste carbon obtained in step (1) with granular carbon, coal and coke in a mass ratio of 1:100-100:1; (3) Adding the composite reducing agent obtained in step (2) into a fuming furnace to perform a reduction operation.
2. The method of using waste carbon from aluminum electrolysis in a fuming furnace according to claim 1, It is characterized in that The aluminum electrolysis waste carbon in step (1) can also be pretreated by high-temperature non-vacuum distillation, ultra-high temperature vacuum treatment, wet flotation or mechanical crushing and physical separation.
3. The method of using waste carbon from aluminum electrolysis in a fuming furnace according to claim 1, It is characterized in that The aluminum electrolysis waste carbon in the step (1) is aluminum electrolysis waste carbon that has not been pretreated in any way.
4. The method of using waste carbon from aluminum electrolysis in a fuming furnace according to claim 1, It is characterized in that The composite reducing agent in step (2) also includes anode carbon slag or waste cathode carbon blocks after distillation.
5. The method of using waste carbon from aluminum electrolysis in a fuming furnace according to claim 1, It is characterized in that In the step (2), the composite reducing agent is in the form of powder, granules or blocks.
6. The method of using waste carbon from aluminum electrolysis in a fuming furnace according to claim 1, It is characterized in that The fuming furnace in step (3) is any one of a side-blown furnace, a top-blown furnace, a vacuum tube furnace or a bottom-blown furnace.
7. The method of using waste carbon from aluminum electrolysis in a fuming furnace according to claim 1, It is characterized in that In the step (3), the melt reduction temperature in the fuming furnace is 100-1800°C; the primary air consumption and secondary air consumption of the lead smelting reduction furnace are both 0-10000Nm 3 / h; the primary air oxygen concentration and the secondary air oxygen concentration of the lead smelting reduction furnace are both 20%-100%, and the reduction time of the lead smelting reduction furnace is 1-1000min; the slag-forming agent in the lead smelting reduction furnace includes any one of lime, limestone, quartz, iron ore, fluorite or dolomite.
8. The method of using waste carbon from aluminum electrolysis in a fuming furnace according to claim 1, It is characterized in that The chemical reaction occurring in the fuming furnace in step (3) is as follows: PbO+C=Pb+CO; PbO+CO=Pb+CO 2 ; ZnO+C=Zn+CO; ZnO+CO=Zn+CO 2 。 9. The method of using waste carbon from aluminum electrolysis in a fuming furnace according to claim 1, It is characterized in that The chemical reaction occurring in the fuming furnace in step (3) also includes the following reaction: <h2 style=";text-align:left;direction:ltr">2AlF<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> +3CaO=Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> +3CaF<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> ; <h2 style=";text-align:left;direction:ltr">2Na<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> AlF<h2 style=";text-align:left;direction:ltr"> 6 <h2 style=";text-align:left;direction:ltr"> +6CaO+3SiO<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> (Al)<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> +6CaF<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> +3Na<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> SiO<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> ; 2NaF+CaO+SiO 2 =CaF 2 +And 2 Not. 3 ; <h2 style=";text-align:left;direction:ltr">4NaCN+9O<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> +2SiO<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> <2Na<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> SiO<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> +4NO<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> +4CO<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> ; 2NaCN+4O 2 +SiO 2 =Na 2 SiO 3 +N 2 About 3 +2CO 2 。