Zinc leaching residue treatment method and application thereof
By mixing zinc leach slag, copper powder and sulfuric acid for galvanic corrosion reaction at room temperature, the high energy consumption problem of zinc leach slag under high temperature and high acid leaching conditions is solved, and efficient leaching and resource recovery of zinc leach slag is achieved, which improves the efficiency of zinc leach slag Cleanliness and implementability of the process.
Patent Information
- Application Number
- CN202310573524.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, the high temperature and high acid leaching conditions of zinc leaching slag lead to high energy consumption, and zinc ferrite is difficult to effectively leaching, resulting in low zinc loss and resource recovery efficiency.
The zinc leaching slag, copper powder and sulfuric acid are mixed at room temperature, and the decomposition of iron oxides is accelerated through the galvanic corrosion reaction, and the metal zinc is released, reducing the energy consumption of the zinc leaching process, and obtaining high metals through solid-liquid separation and settlement separation Grade leachate.
It realizes efficient room temperature leaching of zinc slag, significantly reduces process energy consumption, improves process cleanliness and implementability, and improves zinc recycling efficiency and resource utilization.
Smart Images

Figure CN118996145A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of solid waste treatment, and specifically relates to a treatment method for zinc leaching slag and application thereof. Background Art
[0002] Zinc leaching slag is the largest zinc-containing hazardous waste in the zinc smelting production process, and its recycling and treatment is of great significance to environmental protection and resource utilization.
[0003] The most difficult component to handle in zinc leaching residue is iron oxides represented by zinc ferrite, which are rich in zinc, copper, cadmium, indium and other elements and are key phases for resource recovery. However, iron oxides are difficult to be leached by conventional acid, and the improvement of their leaching rate depends on high temperature, high acid and long time leaching conditions, which results in high energy consumption of acid leaching technology.
[0004] Iron is an associated element of zinc sulfide concentrate, the raw material of zinc smelting. When the zinc concentrate is roasted, it will inevitably form an insoluble zinc ferrite phase with part of zinc, resulting in zinc being mixed with other insoluble components such as lead sulfate and silicate into the zinc leaching residue as an insoluble component during the acid leaching of zinc roasted sand. It is estimated that about 20% of the total zinc production is lost in the zinc leaching residue in the form of zinc ferrite, which has great recovery value.
[0005] However, due to the difficult leaching characteristics of zinc ferrite, it is difficult to achieve efficient leaching of iron oxides by conventional acid leaching.
[0006] At present, the methods for treating zinc leaching residue include hot acid leaching-iron precipitation method, which realizes leaching of zinc leaching residue through higher acid concentration (>50g / L), higher temperature (>90℃), and longer reaction time (>4 hours) to obtain lead-silver slag and iron slag; however, since the zinc ferrite phase is very stable, the zinc ferrite phase is usually mixed in the lead-silver slag, resulting in unnecessary zinc loss. Summary of the invention
[0007] In order to solve the technical problem of zinc loss in the zinc leaching slag recovery process in the above-mentioned prior art, the present invention provides a method for treating zinc leaching slag, comprising the steps of:
[0008] S1. Mix zinc leaching residue, copper powder and sulfuric acid and react for 6 to 24 hours to obtain a mixed solution;
[0009] The phases in the zinc leaching residue include zinc ferrite and lead sulfate, the molar ratio of the copper powder to the zinc ferrite is 2 to 4:1, and the reaction is carried out at a temperature of 15 to 40° C.; the zinc ferrite accounts for 40 to 80% of the zinc leaching residue, and the lead sulfate accounts for 5 to 20%;
[0010] S2. separating the mixed solution into solid and liquid to obtain zinc leaching solution.
[0011] Furthermore, after the mixed liquid is separated into solid and liquid, leaching residue is obtained;
[0012] Water is added to the leached residue and the residue is allowed to settle to obtain a sedimentation supernatant and a sedimentation underflow; wherein the phase in the sedimentation underflow includes copper.
[0013] Furthermore, the leached residue includes copper and lead sulfate.
[0014] Furthermore, the sedimentation upper liquid is filtered and separated to obtain a dilute leachate, which includes sulfuric acid.
[0015] Furthermore, in the step S1, the source of sulfuric acid includes the dilute leaching solution, and the source of copper powder includes the sedimentation underflow.
[0016] Furthermore, the concentration of sulfuric acid in the sulfuric acid solution is 50-300 g / L, and the liquid-solid ratio of the sulfuric acid solution to the zinc leaching residue is 5-40 ml:1 g.
[0017] Furthermore, the reaction in step S1 is carried out under stirring, the rotation speed during the stirring process is 300-400 rpm, and the stirring time is 6-7 hours.
[0018] Furthermore, the reaction in step S1 is carried out under static conditions, and the static time is 18 to 24 hours.
[0019] Furthermore, the reaction process is carried out at room temperature.
[0020] The present invention also provides an application of the zinc leaching slag treatment method as described in any one of the above items in the treatment of zinc-containing solid waste.
[0021] Compared with the prior art, the present invention has at least the following advantages:
[0022] The present invention innovatively develops a room temperature efficient leaching process for zinc leaching residue, and introduces copper powder into the zinc leaching residue acid leaching process. The copper powder and the iron oxides represented by zinc ferrite in the zinc leaching residue form galvanic corrosion, which accelerates the decomposition of metal-containing iron oxides, thereby releasing a large amount of metal. Galvanic corrosion reduces the energy barrier for the decomposition of zinc ferrite in the zinc leaching residue, so that easy and efficient zinc leaching can be achieved without relying on heating. Compared with the leaching conditions of medium-high temperature and high acid in the prior art, the present invention significantly reduces the process energy consumption and improves the cleanliness and feasibility of the process. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0024] Figure 1 This is a schematic diagram of a process for treating zinc leaching slag in one embodiment of the present invention;
[0025] Figure 2 is the XRD diagram of the zinc leaching slag in Example 1 of the present invention;
[0026] Figure 3 is the XRD diagram of the leached residue in Example 7 of the present invention;
[0027] Figure 4 is the XRD diagram of the sedimentation underflow in Example 7 of the present invention;
[0028] Figure 5 This is the XRD diagram of the lead-rich silver slag in Example 7 of the present invention.
[0029] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0030] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0032] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention are familiar to those skilled in the art and the description of the present invention, and any methods, equipment and materials of the prior art similar or equivalent to the methods, equipment and materials described in the embodiments of the present invention can also be used to implement the present invention.
[0033] like Figure 1 As shown, the present invention provides a method for treating zinc leaching slag, comprising the steps of:
[0034] S1. Mix zinc leaching residue, copper powder and sulfuric acid and react for 6 to 24 hours to obtain a mixed solution;
[0035] The phases in the zinc leaching residue include zinc ferrite and lead sulfate, the molar ratio of the copper powder to the zinc ferrite is 2 to 4:1, and the reaction is carried out at a temperature of 15 to 40° C. Exemplarily, the reaction can be carried out at room temperature.
[0036] Zinc leaching slag: The zinc ferrite may account for 40-80% of the zinc leaching slag, and the lead sulfate may account for 50-20%.
[0037] In some embodiments, the concentration of sulfuric acid in the sulfuric acid solution may be 50-300 g / L, and the liquid-to-solid ratio of the sulfuric acid solution to the zinc leaching residue may be 5-40 ml:1 g.
[0038] The particle size of the copper powder may be 2 to 200 microns.
[0039] In other embodiments, the mixing and reaction of zinc leaching residue, copper powder and sulfuric acid can be carried out under stirring conditions or static conditions.
[0040] Specific:
[0041] Stirring conditions: the zinc leaching residue, the copper powder and the sulfuric acid can be mixed and stirred at a rotation speed of 300 to 400 rpm. The stirring method is applied throughout the entire reaction process. The stirring time is 6 to 7 hours, that is, under the stirring conditions, the reaction time of the zinc leaching residue, the copper powder and the sulfuric acid is 6 to 7 hours.
[0042] Standing condition: after mixing the zinc leaching residue, the copper powder and the sulfuric acid, the mixture is allowed to stand for 18 to 24 hours to obtain the mixed solution.
[0043] In some preferred embodiments, the mixing and reaction of zinc leaching residue, copper powder and sulfuric acid can be carried out in a flat-bottomed reaction vessel.
[0044] It should be noted that in step S1, the sign of sufficient mixing is that there is no obvious independent block of copper powder or zinc leaching residue in the mixed solution. After the zinc leaching residue, copper powder, and sulfuric acid are fully mixed, the operation in step S2 is performed. The reaction container can be sealed with a lid or open, and can be exposed to light or darkness.
[0045] Step S1 can be performed at room temperature.
[0046] S2. separating the mixed solution into solid and liquid to obtain zinc leaching solution.
[0047] In some embodiments, step S2 may be followed by the following steps S3 and S4:
[0048] S3. The solid-liquid separation of the mixed liquid also obtains leached residue;
[0049] Add water to the leached residue for sedimentation to obtain a sedimentation upper liquid and a sedimentation underflow; wherein the main phase in the sedimentation underflow includes copper, and the main phase in the leached residue includes copper powder and / or lead sulfate.
[0050] The upper liquid of the sedimentation is a suspension of lead sulfate, and the bottom flow of the sedimentation is the residual copper powder. The average particle size of lead sulfate is 7.8μm, and it settles slowly. The average particle size of copper powder is 38.3μm, and it settles quickly, so it can be easily separated by sedimentation.
[0051] S4. Filter and separate the sedimentation liquid to obtain a dilute leaching solution, wherein the main component of the dilute leaching solution is water, containing a small amount of water-soluble ions, including H 2 SO 4 .
[0052] In some embodiments, the filtered separation product of the sedimentation upper liquid also includes lead-rich silver slag, and the physical phase in the lead-rich silver slag mainly includes lead sulfate.
[0053] Lead is a concomitant element of zinc sulfide concentrate, the raw material for zinc smelting. It is enriched in zinc leaching slag in the form of lead sulfate during the zinc smelting process. However, due to the low lead grade of about 10% in zinc leaching slag, which is far from the lead grade of about 50% of the concentrate entering the lead smelter, zinc leaching slag cannot be directly used for lead smelting economically.
[0054] In common technology, the utilization of metallic lead in zinc leaching residue is usually based on the lead-silver residue after zinc extraction. Due to the difficult leaching characteristics of zinc ferrite, a large amount of zinc ferrite is still present in the lead-silver residue, resulting in a low metal grade of the lead-silver residue.
[0055] In comparison, the present application further improves the metal grade in the lead-silver slag through the thorough extraction of zinc, thereby optimizing the subsequent application effect of the lead-silver slag.
[0056] In some preferred embodiments, the dilute leachate and the sedimentation underflow can be used as the sulfuric acid and the copper powder in step S1, respectively, and circulate to participate in the treatment of the zinc leaching residue.
[0057] The chemical reactions mainly involved in the present invention are as follows:
[0058] ZnFe 2 O 4 +Cu+8H + =Zn 2+ +2Fe 2+ +Cu 2+ +4H 2 O
[0059] ZnFe 2 O 4 +Cu+8H + =Zn 2+ +2Fe2+ +2Cu + +4H 2 O
[0060] Compared with the prior art, the present invention has at least the following advantages:
[0061] 1. The present invention innovatively develops a room temperature efficient leaching process for zinc leaching residue, and introduces copper powder into the zinc leaching residue acid leaching process. The copper powder and the iron oxides represented by zinc ferrite in the zinc leaching residue form galvanic corrosion, which accelerates the decomposition of metal-containing iron oxides, thereby releasing a large amount of metal. Galvanic corrosion reduces the energy barrier for the decomposition of zinc ferrite in the zinc leaching residue, so easy and efficient zinc leaching can be achieved without relying on heating. Compared with the medium-high temperature and high-acid leaching conditions in the prior art, the present invention significantly reduces the process energy consumption and improves the cleanliness and feasibility of the process.
[0062] 2. The present invention provides a method for treating zinc leaching residue, which can utilize zinc leaching residue with low consumption and high efficiency, thereby realizing resource recovery and solid waste reduction.
[0063] Specifically, the present invention mixes the zinc leaching residue and the copper powder in a sulfuric acid solution, so that the zinc leaching residue and the copper powder are fully mixed and contacted for a period of time, thereby ensuring that the copper fully reacts with the iron oxide in the zinc leaching residue.
[0064] The present invention can obtain leaching slag and zinc leaching solution by solid-liquid separation of the treatment liquid. The residual copper powder in the leaching slag can be accumulated and then separated by sedimentation, and returned to the mixed treatment for reuse; the separated sedimentation upper liquid is filtered to obtain high metal grade lead-rich silver slag.
[0065] The method can achieve efficient extraction of valuable metals at room temperature and static conditions, effectively improving the cleanliness and feasibility of the process in the zinc leaching slag treatment process of the present invention.
[0066] The present invention also provides an application of the zinc leaching slag treatment method as described in any one of the above items in the treatment of zinc-containing solid waste.
[0067] In order to facilitate those skilled in the art to further understand the present invention, examples are given below:
[0068] Example 1
[0069] The zinc leaching slag from a certain factory was taken as raw material, and the full element analysis was carried out using an ICP-OES spectrometer. The main element composition (mass percentage) of the zinc leaching slag included: Fe 25.2%, Zn 17.3%, Pb 5.78%, and Ag 260g / t.
[0070] See also Figure 2 As shown, the zinc leaching slag was analyzed by X-ray diffraction analysis (XRD), and the obtained phases were mainly zinc ferrite and lead sulfate.
[0071] Among them, the mass proportion of zinc ferrite in the zinc leaching slag is 54.4%, and the mass proportion of lead sulfate in the zinc leaching slag is 8.5%.
[0072] Example 2
[0073] 1 g of zinc leached residue (same as in Example 1) and copper powder were added to a sulfuric acid solution with a sulfuric acid concentration of 150 g / L, the liquid-to-solid ratio of the sulfuric acid solution to the zinc leached residue was 10 ml / g, and after being fully mixed, they were placed in a flat-bottomed glass bottle at room temperature (20° C.).
[0074] The volume of the glass bottle is 15 ml, and it is sealed with a lid and placed in a dark environment for 24 hours.
[0075] The copper powder addition amounts set above are 0.144 g (1 times the molar ratio of zinc ferrite in zinc leaching slag), 0.216 g (1.5 times), 0.288 g (2 times), and 0.576 g (4 times), respectively. The above tests were carried out at each set copper powder addition amount.
[0076] The results are shown in the following table:
[0077]
[0078] It can be seen from the above table that when the addition amount is ≥1.5 times the molar ratio, the zinc leaching rate exceeds 90%, and when the addition amount is ≥2 times, the leaching rate is further improved, exceeding 95%. Therefore, the addition amount is preferably 2 to 4 times the molar ratio of zinc ferrite in the zinc leaching residue.
[0079] Example 3
[0080] 0.2 g zinc leaching residue (same as Example 1) and 0.115 g copper powder (4 times the molar ratio of zinc ferrite in the zinc leaching residue) were added to a sulfuric acid solution of a set concentration. The liquid-to-solid ratio of the sulfuric acid solution to the zinc leaching residue was 40 ml / g. After being fully mixed, the mixture was placed in a flat-bottomed glass bottle at room temperature (20°C).
[0081] The volume of the glass bottle is 15 ml, and it is sealed with a lid and placed in a dark environment for 24 hours.
[0082] The above-mentioned set sulfuric acid concentrations are 50 g / L, 100 g / L, 150 g / L, 200 g / L, and 300 g / L, respectively, and the above-mentioned tests are carried out at each set concentration.
[0083] The results are shown in the following table:
[0084]
[0085] It can be seen from the above table that when the concentration of the sulfuric acid solution is ≥50 g / L, the zinc leaching rate is greater than 95%. Therefore, the sulfuric acid concentration is preferably 50 g / L to 300 g / L.
[0086] Example 4
[0087] 0.2 g of zinc leaching residue (same as Example 1) and 0.115 g of copper powder (4 times the molar ratio of zinc ferrite in the zinc leaching residue) were added to a sulfuric acid solution with a sulfuric acid concentration of 300 g / L, mixed thoroughly and placed in a flat-bottomed glass bottle at room temperature (20°C).
[0088] Among them, for the liquid-to-solid ratio of 3 to 10, the volume of the glass bottle is 3 ml; for the liquid-to-solid ratio of 20 to 40, the volume of the glass bottle is 15 ml, and it is covered and sealed in a dark environment for 24 hours.
[0089] The liquid-to-solid ratios of the sulfuric acid solution to the zinc leaching residue were 3, 4, 5, 6, 8, 10, 20, 30, and 40, respectively, and the above tests were carried out at each solid-to-liquid ratio.
[0090] The results are shown in the following table:
[0091]
[0092] It can be seen from the above table that when the liquid-to-solid ratio is ≥ 5, the zinc leaching rate exceeds 95%. Therefore, the preferred liquid-to-solid ratio is 5-40 ml / g.
[0093] Example 5
[0094] 0.2 g of zinc leached residue (same as in Example 1) and copper powder were added to a sulfuric acid solution with a sulfuric acid concentration of 150 g / L, the liquid-to-solid ratio of the sulfuric acid solution to the zinc leached residue was 10 ml / g, and after being fully mixed, they were placed in a flat-bottomed glass bottle at room temperature (20° C.).
[0095] The volume of the glass bottle is 3 ml, which is sealed and placed in a dark environment for 24 hours. Batch production is used for regular sampling to determine the leaching time. One is taken out for testing at regular intervals.
[0096] The above-set copper powder addition amounts were 0.058 g (2 times) and 0.115 g (4 times), respectively. The above-mentioned test was carried out at each set copper powder addition amount.
[0097] The results are shown in the following table:
[0098]
[0099] It can be seen from the above table that the reaction speed when the addition amount is 4 times is faster than that when the addition amount is 2 times, but the zinc leaching rate exceeds 95% after 18 hours, so the preferred reaction time is 18 to 24 hours.
[0100] Example 6
[0101] 1 g of zinc leached residue (same as in Example 1) and 0.576 g of copper powder (4 times the molar ratio of zinc ferrite in the zinc leached residue) were added to a sulfuric acid solution with a sulfuric acid concentration of 150 g / L, and the liquid-to-solid ratio of the sulfuric acid solution to the zinc leached residue was 10 ml / g. After being fully mixed, they were placed in a flat-bottomed glass bottle at room temperature (20°C).
[0102] Among them, the volume of the glass bottle is 15 ml, and it is produced in batches and subjected to the following conditions: sealed with a cap and placed in a dark environment for 24 hours; left open and placed in a dark environment for 24 hours; sealed with a cap and placed in a light environment for 24 hours.
[0103] The above tests were carried out under different set environmental conditions.
[0104] The results are shown in the following table:
[0105]
[0106] It can be seen from the above table that whether it is airtight or not, and whether there is light or not, has no obvious effect on the reaction.
[0107] Example 7
[0108] 1 g of zinc leached residue (same as in Example 1) and 0.288 g of copper powder (2 times the molar ratio of zinc ferrite in the zinc leached residue) were added to a sulfuric acid solution with a sulfuric acid concentration of 150 g / L, and the liquid-to-solid ratio of the sulfuric acid solution to the zinc leached residue was 10 ml / g. After being fully mixed, they were placed in a flat-bottomed glass bottle at room temperature (20°C).
[0109] The volume of the glass bottle is 15 ml, and it is sealed with a lid and placed in a dark environment for 24 hours.
[0110] The zinc leaching solution is extracted and separated, and the leaching residue is subjected to sedimentation treatment to obtain a sedimentation underflow (rich in residual copper) at the lower layer and a sedimentation upper liquid at the upper layer.
[0111] The upper liquid of the sedimentation is filtered and separated to obtain a dilute leaching solution and lead-silver-rich slag.
[0112] X-ray diffraction analysis (XRD) was used to analyze the phases of leached residue, sedimentation underflow and lead-silver-rich slag.
[0113] See also Figure 3 As shown, the phases in the leached residue are mainly copper and lead sulfate; see Figure 4 As shown, the phase in the sedimentation underflow is mainly copper; see Figure 5 As shown, the physical phase in the lead-rich silver slag is mainly lead sulfate, and the composition of the lead-rich silver slag includes: Pb 19.2%, Si 14.1%, and Ag 720g / t.
[0114] It can be seen that this method achieves efficient utilization of zinc leaching slag at room temperature.
[0115] Example 8
[0116] 1 g of zinc leached residue (same as in Example 1) and copper powder were added to a sulfuric acid solution with a sulfuric acid concentration of 150 g / L, the liquid-to-solid ratio of the sulfuric acid solution to the zinc leached residue being 10 ml / g, and placed in a flat-bottomed glass bottle.
[0117] The volume of the glass bottle was 15 ml, and a magnetic rotor was placed in the bottle to stir the reaction at room temperature (20° C.) for 7 hours at a stirring rate of 300 rpm.
[0118] The copper powder addition amounts set above are 0.144 g (1 times the molar ratio of zinc ferrite in zinc leaching slag), 0.216 g (1.5 times), 0.288 g (2 times), and 0.576 g (4 times), respectively. The above tests were carried out at each set copper powder addition amount.
[0119] The results are shown in the following table:
[0120]
[0121] It can be seen that within the range of 2 to 4 times the addition amount and the reaction time of 6 to 7 hours, the zinc leaching rate exceeds 95%. Compared with standing, stirring significantly promotes the reaction process and shortens the reaction time.
[0122] Comparative Example 1
[0123] 1 g of zinc leached residue (same as in Example 1) was added to a sulfuric acid solution with a sulfuric acid concentration of 150 g / L, the liquid-to-solid ratio of the sulfuric acid solution to the zinc leached residue was 10 ml / g, and after being fully mixed, it was placed in a flat-bottomed glass bottle at room temperature (20° C.).
[0124] The volume of the glass bottle is 15 ml, and it is sealed with a lid and placed in a dark environment for 24 hours.
[0125] The zinc leaching rate is 30.5%. It can be seen that without the addition of copper powder, the zinc leaching rate of zinc leaching residue at room temperature is not high.
[0126] The above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for treating zinc leaching residue, characterized in that: Includes steps: S1. Mix zinc leaching residue, copper powder and sulfuric acid and react for 6 to 24 hours to obtain a mixed solution; The phases in the zinc leaching residue include zinc ferrite and lead sulfate, the molar ratio of the copper powder to the zinc ferrite is 2 to 4:1, and the reaction is carried out at a temperature of 15 to 40° C.; the zinc ferrite accounts for 40 to 80% of the zinc leaching residue, and the lead sulfate accounts for 5 to 20%; S2. separating the mixed solution into solid and liquid to obtain zinc leaching solution.
2. The processing method according to claim 1, characterized in that: After the mixed liquid is separated into solid and liquid, the residue is leached; Water is added to the leached residue and the residue is allowed to settle to obtain a sedimentation supernatant and a sedimentation underflow; wherein the phase in the sedimentation underflow includes copper.
3. The processing method according to claim 1, characterized in that: The leached residue includes copper and lead sulfate.
4. The processing method according to claim 2, characterized in that: The sedimentation upper liquid is filtered and separated to obtain a dilute leachate, which includes sulfuric acid.
5. The processing method according to claim 4, characterized in that: In the step S1, the source of the sulfuric acid includes the dilute leaching solution, and the source of the copper powder includes the sedimentation underflow.
6. The processing method according to claim 1, characterized in that: The concentration of sulfuric acid in the sulfuric acid solution is 50-300 g / L, and the liquid-to-solid ratio of the sulfuric acid solution to the zinc leaching residue is 5-40 ml:1 g.
7. The processing method according to claim 1, characterized in that: The reaction in step S1 is carried out under stirring conditions, the rotation speed during the stirring process is 300-400 rpm, and the stirring time is 6-7 hours.
8. The processing method according to claim 1, characterized in that: The reaction in step S1 is carried out under standing conditions, and the standing time is 18 to 24 hours.
9. The processing method according to claim 1, characterized in that: The reaction process is carried out at room temperature.
10. Use of the zinc leaching slag treatment method according to any one of claims 1 to 9 in the treatment of zinc-containing solid waste.