Method for producing silicon inclusion compound electrode active material and method for producing lithium ion battery
By contacting the silicon inclusion compound containing sodium with hydrogen fluoride solution, and using a mixed solvent of water and organic solvent, the problems of expansion and sodium residue of the silicon inclusion compound electrode active material during charging are solved, which improves the treatment efficiency and reduces the sodium Residual amount, suitable for the negative electrode active substance of lithium-ion batteries.
Patent Information
- Application Number
- CN202410552615.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2024-05-07
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, there are problems in which the silicon inclusion electrode active substance expands during charging, as well as the low treatment efficiency of the silicon inclusion compound containing sodium and large sodium residues.
Sodium is removed from the sodium-containing inclusion compound from which the sodium is contacted with a hydrogen fluoride solution, and a mixed solvent of water and organic solvent is used to improve the sodium removal efficiency and reduce by-product generation.
The efficiency of the sodium removal process is improved, and the amount of sodium remaining in the silicon inclusion electrode active material is reduced. It is suitable for the negative electrode active material of lithium-ion batteries.
Smart Images

Figure BDA0004824897900000101
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method for producing a silicon inclusion compound electrode active material and a method for producing a lithium ion battery. Background Art
[0002] In recent years, the development of batteries has been actively carried out. For example, in the automotive industry, the development of batteries used in electric vehicles or hybrid vehicles is advancing. In addition, silicon is known as an electrode active material used in batteries, especially lithium-ion batteries.
[0003] Silicon electrode active materials have a large theoretical capacity and are effective for increasing the energy density of batteries. However, silicon electrode active materials have a problem of large expansion during charging. In response to this, it is known that silicon inclusion compound electrode active materials can be used as silicon electrode active materials to suppress expansion during charging.
[0004] For example, Patent Document 1 discloses a silicon inclusion compound electrode active material having a silicon inclusion compound II type crystal phase, having voids inside primary particles, and voids with pore diameters of 100 nm or less having a void content of 0.05 cc / g or more and 0.15 cc / g or less.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2021-158004 Summary of the invention
[0008] Problems to be solved by the invention
[0009] A silicon clathrate electrode active material can be produced by removing sodium from a sodium-containing silicon clathrate, but there is a need to improve the efficiency of treating the sodium-containing silicon clathrate in this process and to reduce the amount of residual sodium in the obtained silicon clathrate electrode active material.
[0010] The present disclosure aims to provide a method for producing a silicon clathrate electrode active material, which can improve the processing efficiency of a silicon clathrate containing sodium in a sodium removal step and reduce the amount of sodium remaining in the obtained silicon clathrate electrode active material, and a method for producing a lithium ion battery including producing such a silicon clathrate electrode active material.
[0011] Means for solving problems
[0012] The present inventors have found that the above-mentioned problems can be solved by the following means.
[0013] <Scheme 1>
[0014] A method for producing a silicon inclusion compound electrode active material, comprising the following steps:
[0015] (a) providing a silicon inclusion compound containing sodium; and
[0016] (b) contacting the sodium-containing silicon clathrate with a hydrogen fluoride solution to remove at least a portion of the sodium from the sodium-containing silicon clathrate.
[0017] <Scheme 2>
[0018] The method according to Scheme 1, wherein the solvent of the hydrogen fluoride solution is a mixed solvent of water and an organic solvent.
[0019] <Scheme 3>
[0020] The method according to Option 1 or 2, wherein the silicon inclusion compound containing sodium has a porous structure.
[0021] <Scheme 4>
[0022] The method according to any one of aspects 1 to 3, wherein the silicon inclusion compound electrode active material is used as a negative electrode active material for a lithium ion battery.
[0023] <Scheme 5>
[0024] A method for producing a lithium ion battery, comprising: producing a silicon inclusion compound electrode active material by the method of any one of schemes 1 to 4; and forming an electrode active material layer containing the silicon inclusion compound electrode active material.
[0025] Effects of the Invention
[0026] According to the method of the present disclosure for manufacturing a silicon inclusion compound electrode active material, the processing efficiency of the silicon inclusion compound containing sodium in the sodium removal process can be improved, and the amount of sodium remaining in the obtained silicon inclusion compound electrode active material can be reduced. In addition, the present disclosure can provide a method for manufacturing a lithium ion battery including manufacturing a silicon inclusion compound electrode active material. DETAILED DESCRIPTION
[0027] The following is a detailed description of the embodiments of the present disclosure. However, the present disclosure is not limited to the following embodiments, and can be implemented with various modifications within the scope of the disclosed gist.
[0028] 《Method for producing silicon inclusion compound electrode active material》
[0029] The disclosed method for producing a silicon clathrate electrode active material comprises: (a) providing a silicon clathrate containing sodium; and (b) contacting the silicon clathrate containing sodium with a hydrogen fluoride solution to remove at least a portion of the sodium from the silicon clathrate containing sodium.
[0030] As a method for producing a silicon inclusion compound electrode active material, for example, the following method can be cited: a silicon inclusion compound containing sodium (e.g., Na 20 Si 136 ) is mixed with zinc chloride and fired, thereby removing sodium (Na) from the sodium-containing silicon inclusion compound to produce a silicon inclusion compound with a reduced sodium content (e.g., Na2Si 136 ).
[0031] However, the reaction in this method is a solid phase reaction, so a relatively long reaction time is required. The present inventors have found that Na can be efficiently removed from the sodium-containing silicon inclusion compound by contacting a hydrogen fluoride (HF) solution with the sodium-containing silicon inclusion compound instead of or in addition to this reaction.
[0032] In the present disclosure, the “electrode active material” can be used as a “positive electrode active material” or a “negative electrode active material”, and can be used as a “negative electrode active material” in particular.
[0033] <Provision of silicon inclusion compound containing sodium>
[0034] The method of the present disclosure includes providing a silicon clathrate containing sodium.
[0035] Silicon clathrate containing sodium can be prepared by removing sodium from sodium silicon (NaSi) alloy.
[0036] Specifically, first, a silicon source is reacted with a sodium source such as sodium hydride to prepare a NaSi alloy. Then, the NaSi alloy thus prepared is heated to remove sodium from the NaSi alloy and form a clathrate, thereby preparing a silicon clathrate. Alternatively, the NaSi alloy thus prepared is reacted with aluminum fluoride as a sodium trapping agent to remove sodium from the NaSi alloy and form a clathrate, thereby preparing a silicon clathrate.
[0037] The silicon inclusion compound containing sodium may have a porous structure. In this case, the contact area between the silicon inclusion compound containing sodium and the hydrogen fluoride (HF) solution is large, which is preferable in terms of improving the removal efficiency of Na.
[0038] 〈Removal of sodium〉
[0039] The method disclosed herein comprises contacting a silicon clathrate containing sodium with a hydrogen fluoride solution, and removing at least a portion of the sodium from the silicon clathrate containing sodium.
[0040] The solvent of the hydrogen fluoride solution can be water, an organic solvent, or a mixed solvent of water and an organic solvent. When the solvent contains water, that is, when the solvent is water or a mixed solvent of water and an organic solvent, particularly when the solvent is a mixed solvent of water and an organic solvent, the generation of a by-product such as sodium silicofluoride (Na2SiF6) can be suppressed, and thus it is preferred.
[0041] From the viewpoint of being able to reduce the amount of water remaining in the silicon inclusion compound electrode active material, the solvent preferably contains an organic solvent. The proportion of the organic solvent in the solution may be 80% by mass or more, 90% by mass or more, or 95% by mass or more.
[0042] The organic solvent may be any organic solvent capable of dissolving hydrogen fluoride, and when the organic solvent is mixed with water for use, it may be any organic solvent capable of dissolving hydrogen fluoride and compatible with water. The organic solvent is preferably an alcohol, more preferably a lower alcohol, and still more preferably ethanol.
[0043] In the method disclosed herein, the ratio of the amount (mol) of hydrogen fluoride to the mass (g) of the silicon inclusion compound (HF [mol] / Si [g]) may be 0.01 mol / g or more, 0.02 mol / g or more, 0.03 mol / g or more, or 0.04 mol / g or more, and may be 0.20 mol / g or less. If the ratio is within the above range, Na can be efficiently removed from the silicon inclusion compound containing sodium.
[0044] As a method for bringing the sodium-containing silicon clathrate into contact with the hydrogen fluoride solution, a mixing operation such as stirring can be exemplified, but the method is not limited thereto.
[0045] The time for contacting the sodium-containing silicon clathrate with the hydrogen fluoride solution may be 0.5 hours or more, 1 hour or more, or 2 hours or more, and may be 6 hours or less, 5 hours or less, or 4 hours or less.
[0046] In the silicon inclusion compound electrode active material produced by the method of the present invention, the amount of sodium in the silicon inclusion compound electrode active material may be 6.5 mass % or less, 6.0 mass % or less, 5.5 mass % or less, 5.2 mass % or less, 5.0 mass % or less, 4.8 mass % or less, or 4.6 mass % or less.
[0047] The amount of sodium in the silicon clathrate electrode active material can be measured by, for example, inductively coupled plasma (ICP) analysis.
[0048] <use>
[0049] The silicon inclusion compound electrode active material obtained by the method disclosed in the present invention can be used as a negative electrode active material of a lithium ion battery.
[0050] 《Manufacturing method of lithium-ion battery》
[0051] The disclosed method for manufacturing a lithium-ion battery includes: manufacturing a silicon inclusion compound electrode active material using the disclosed method; and forming an electrode active material layer containing the silicon inclusion compound electrode active material.
[0052] For the method for producing the silicon clathrate electrode active material, reference may be made to the above description related to the method for producing the silicon clathrate electrode active material of the present disclosure.
[0053] The method for forming the electrode active material layer is not particularly limited, and a known method can be used. For example, when the negative electrode active material layer contains the silicon inclusion compound electrode active material disclosed in the present invention, the electrode active material layer formed on the negative electrode collector layer, i.e., the negative electrode active material layer, can be obtained by applying a slurry containing the silicon inclusion compound electrode active material to the negative electrode collector and drying it.
[0054] The method for forming the battery is not particularly limited, and a known method can be adopted. Hereinafter, a method for producing a battery in which the negative electrode active material layer contains the silicon inclusion compound electrode active material disclosed in the present invention will be described.
[0055] The manufacturing method of the battery disclosed in the present invention may include the steps of sequentially configuring a negative electrode collector layer, a negative electrode active material layer, an electrolyte layer, a positive electrode active material layer and a positive electrode collector layer in addition to manufacturing a silicon inclusion compound electrode active material and forming a negative electrode active material layer containing the silicon inclusion compound electrode active material.
[0056] 〈Negative electrode current collector layer〉
[0057] The material used for the negative electrode collector layer is not particularly limited, and any material that can be used as a negative electrode collector for a battery can be appropriately adopted, such as copper, copper alloys, and products obtained by plating or vapor-depositing copper with nickel, chromium, carbon, etc., but is not limited to these.
[0058] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.
[0059] <Negative electrode active material layer>
[0060] The negative electrode active material layer of the present disclosure is a layer containing a negative electrode active material, and optionally an electrolyte, a conductive aid, and a binder.
[0061] (Negative electrode active material)
[0062] The negative electrode active material includes the silicon inclusion compound electrode active material disclosed in the present invention.
[0063] (Electrolytes)
[0064] The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for lithium-ion batteries can be used. For example, the solid electrolyte may be a sulfide solid electrolyte.
[0065] Examples of sulfide solid electrolytes include sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes, but are not limited to these. Specific examples of sulfide solid electrolytes include Li2S-P2S5 (Li7P3S 11 , Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2 (Li 13 GeP3S 16 , Li 10 GeP2S 12 etc.), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x PS 6-x Cl x etc.; or combinations thereof, but not limited to these.
[0066] The sulfide solid electrolyte may be glass or crystallized glass (glass ceramic).
[0067] Furthermore, when the negative electrode active material layer contains a solid electrolyte, the mass ratio of the silicon inclusion compound electrode active material to the solid electrolyte in the negative electrode active material layer (mass of the silicon inclusion compound electrode active material: mass of the solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.
[0068] The electrolyte preferably contains a supporting salt and a solvent.
[0069] As supporting salts (lithium salts) of electrolytes with lithium ion conductivity, for example, inorganic lithium salts such as LiPF6, LiBF4, LiClO4, and LiAsF6; and organic lithium salts such as LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(FSO2)2, and LiC(CF3SO2)3 can be listed.
[0070] Examples of the solvent used in the electrolyte include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC); and chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The electrolyte preferably contains two or more solvents.
[0071] (Conductive additive)
[0072] The conductive additive is not particularly limited and may be, for example, VGCF (vapor grown carbon fiber), acetylene black (AB), Ketjen black (KB), carbon nanotube (CNT), carbon nanofiber (CNF), etc., but is not limited thereto.
[0073] (Adhesive)
[0074] The binder is not particularly limited, and may be, for example, polyvinylidene fluoride (PVdF), butadiene rubber (BR), styrene butadiene rubber (SBR), or a combination thereof, but is not limited thereto.
[0075] The thickness of the negative electrode active material layer can be, for example, 0.1 to 1000 μm.
[0076] 〈Electrolyte layer〉
[0077] The electrolyte layer contains at least an electrolyte. In addition, the electrolyte layer may contain a binder and the like as needed in addition to the electrolyte. For the electrolyte and the binder, reference may be made to the above description related to the negative electrode active material layer of the present disclosure.
[0078] The thickness of the electrolyte layer is, for example, 0.1 to 300 μm, or preferably 0.1 to 100 μm.
[0079] <Positive electrode active material layer>
[0080] The positive electrode active material layer is a layer containing a positive electrode active material and, optionally, an electrolyte, a conductive aid, a binder, and the like.
[0081] There is no particular limitation on the material of the positive electrode active material. For example, the positive electrode active material may be lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2、Li 1+x Mn 2-x-y M y O4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni and Zn) is a heterogeneous element substituted Li-Mn spinel, lithium titanate (Li x TiO y ), lithium metal phosphate (LiMPO4, M is one or more metals selected from Fe, Mn, Co and Ni), etc., but is not limited to these.
[0082] The positive electrode active material may have a coating layer. The coating layer is a layer containing a material having lithium ion conductivity, low reactivity with the positive electrode active material and the solid electrolyte, and capable of maintaining a non-flowing coating layer even when in contact with the active material or the solid electrolyte. Specific examples of materials constituting the coating layer include Li4Ti5O 12 , Li3PO4, etc., but are not limited to these.
[0083] The shape of the positive electrode active material may be, for example, a particle shape. The average particle size (D50) of the positive electrode active material is not particularly limited, and may be, for example, 10 nm or more, or 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material may be, for example, 50 μm or less, or 20 μm or less. The average particle size (D50) may be calculated, for example, by measurement using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).
[0084] For the electrolyte, the conductive aid, and the binder, reference can be made to the above description regarding the negative electrode active material layer of the present disclosure.
[0085] Furthermore, when the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte (mass of the positive electrode active material:mass of the solid electrolyte) in the positive electrode active material layer is preferably 85:15 to 30:70, and more preferably 80:20 to 50:50.
[0086] The thickness of the positive electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.
[0087] 〈Positive electrode collector layer〉
[0088] There is no particular limitation on the material used in the positive electrode collector layer. Materials that can be used as positive electrode collectors for batteries can be appropriately used, such as SUS, nickel, chromium, gold, platinum, aluminum, iron, titanium and zinc, as well as products obtained by plating or vapor-depositing nickel, chromium, carbon, etc. on these metals, but are not limited to these.
[0089] The shape of the positive electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.
[0090] The lithium-ion battery manufactured by the method of the present disclosure may be a liquid battery containing an electrolyte as an electrolyte layer, or a solid battery containing a solid electrolyte layer as an electrolyte layer. In addition, with respect to the present disclosure, a "solid battery" refers to a battery that uses at least a solid electrolyte as an electrolyte, and therefore, a solid battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. In addition, the solid battery of the present disclosure may be an all-solid battery, that is, a battery that uses only a solid electrolyte as an electrolyte.
[0091] The lithium ion battery manufactured by the method disclosed herein may be a primary battery or a secondary battery.
[0092] Examples of the shape of the lithium ion battery include a coin shape, a laminate shape, a cylindrical shape, and a square shape.
[0093] Example
[0094] 《Synthesis of Silicon Inclusion Compound Electrode Active Materials》
[0095] 〈Alloying〉
[0096] Sodium silicon (NaSi) alloy was manufactured using Si powder and sodium hydride (NaH) as a sodium (Na) source. In addition, as NaH, a product previously washed with hexane was used. NaH and Si powder were weighed so that the molar ratio was 1.05:1, and the weighed NaH and Si powder were mixed using a cutting mill. The obtained mixture was heated in a heating furnace under an argon atmosphere at 500°C for 40 hours to obtain a powdered NaSi alloy.
[0097] 〈Inclusion Formation〉
[0098] The obtained NaSi alloy and aluminum fluoride (AlF3) were weighed so that the molar ratio was 1:0.35, and the weighed NaSi alloy and AlF3 were mixed with a cutter to obtain a reaction raw material. The obtained powdered reaction raw material was placed in a stainless steel reaction container and heated in an argon atmosphere in a heating furnace at 310°C for 60 hours to obtain a sodium-containing silicon inclusion compound (Na 20 Si 136 ).
[0099] 〈Sodium Removal〉
[0100] (Example 1)
[0101] In the obtained Na 20 Si 136 100 ml of ethanol and 3.71 ml of a 46 mass % aqueous solution of hydrogen fluoride (HF) were added to the mixture and stirred. The solution was filtered, and the solid separated by filtration was washed 8 times with 25 ml of ethanol and dried at 60°C under reduced pressure overnight.20 Si 136 The silicon inclusion compound electrode active material of Example 1 in which at least a portion of the sodium is removed.
[0102] (Comparative Example 1)
[0103] Weighing Na 20 Si 136 and zinc chloride (ZnCl2) in a molar ratio of 1:0.75. 20 Si 136 and ZnCl2 to obtain a powdered reaction raw material. The powdered reaction raw material is placed in a stainless steel reaction container and sintered at 430°C in an Ar atmosphere in a heating furnace to react. The reaction product is washed with a mixed solvent of HNO3 and H2O in a volume ratio of 10:90. Thus, the by-products in the reaction product are removed. After washing, the solid component separated by filtration is dried at 120°C for more than 3 hours to obtain the silicon inclusion compound electrode active material of Comparative Example 1.
[0104] (Comparative Example 2)
[0105] A silicon clathrate electrode active material of Comparative Example 2 was obtained in the same manner as in Comparative Example 1 except that the calcination temperature was 450°C.
[0106] "evaluate"
[0107] 〈Na 20 Si 136 Capacity that can be processed
[0108] Calculate the Na in the sodium removal process 20 Si 136 The processable amount per day is shown as a relative value when the value of Comparative Example 1 is set to 1.
[0109] 〈Sodium content after sodium removal process〉
[0110] The amount of sodium remaining in the silicon clathrate electrode active material after the sodium removal step was measured by inductively coupled plasma (ICP) analysis.
[0111] "result"
[0112] Table 1 shows the evaluation results.
[0113]
Table 1
[0114]
[0115] As shown in Table 1, the HF treatment was used to carry out the 20 Si 136In the method of Example 1 for removing sodium, Na 20 Si 136 The amount that can be processed is large, and the amount of sodium remaining in the silicon inclusion compound electrode active material is small.
Claims
1. A method for producing a silicon inclusion compound electrode active material, comprising the following steps: (a) providing a silicon inclusion compound containing sodium; and (b) contacting the sodium-containing silicon clathrate with a hydrogen fluoride solution to remove at least a portion of the sodium from the sodium-containing silicon clathrate.
2. The method according to claim 1, wherein: The solvent of the hydrogen fluoride solution is a mixed solvent of water and an organic solvent.
3. The method according to claim 1, wherein: The sodium-containing silicon inclusion compound has a porous structure.
4. The method according to claim 1, wherein: The silicon inclusion compound electrode active material is used as a negative electrode active material of a lithium ion battery.
5. A method for manufacturing a lithium-ion battery, comprising: A method according to any one of claims 1 to 4 is used to prepare a silicon inclusion compound electrode active material; and An electrode active material layer containing the silicon inclusion compound electrode active material is formed.
Citation Information
Patent Citations
Active material, negative electrode layer, battery and these manufacturing methods
JP2021158004A