Preparation process of wool and silk filament spinning
Through the blending technology of ultrafine wool fiber, silk filaments and nylon conductive fibers, the problem of insufficient strength and uniformity of wool silk yarn during the weaving process is solved, and high-strength, soft, and anti-static yarn are prepared, which improves the The performance of yarn and the performance of clothing.
Patent Information
- Application Number
- CN202411127637.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
The existing preparation process of wool silk spinning has problems of insufficient strength and uniformity during the weaving process, and the yarn is prone to static electricity under mechanical action, affecting the performance and user experience of the clothing.
Using the blending technology of ultrafine wool fiber, silk filaments and nylon conductive fibers, high-strength and softness are prepared through multiple steps such as mixing strips, combing, needle combing, roving, fine yarn, winding, twisting and waxing. , anti-static yarns improve the uniformity and conductivity of the yarn.
The obtained yarn has a strength of 700-800 cN/cm, an elongation of 13-14% and an uneven rate of 16-17%. The anti-pulling and pilling grade reaches 3-4, which improves the softness of the yarn. Durability and electrical conductivity enhance weaving and clothing garment garment performance.
Smart Images

Figure CN118996697A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of worsted wool yarn blending, and specifically relates to a preparation process for wool and silk filament spinning. Background Art
[0002] During the weaving process of seamless underwear circular knitting machine yarn, the yarn is subjected to complex mechanical effects. When passing through the yarn guide device and its coils, it will be subjected to different forms of friction. When it is knitted into a loop, it will be subjected to deformation such as stretching, bending, and twisting. The preparation process of this yarn is particularly important. On the one hand, the yarn must be soft and comfortable, warm and breathable, elegant, wear-resistant and durable. On the other hand, it must ensure high strength for subsequent weaving.
[0003] When spinning wool and silk filaments, although the production cost of blending wool and silk staple fibers is lower, the effect is not as good as wool and silk filaments, and the filaments are stronger, more durable and softer.
[0004] In the Chinese patent application publication number CN111424335A, a method for preparing anti-pilling wool sweater is disclosed. Through the organic combination of blending modification and copolymerization modification, the prepared wool sweater is anti-pilling and anti-hair, and has excellent properties of anti-perspiration, delicate hand feeling, affinity and softness, elegant drape, anti-pilling friction greater than 3.5, making the fiber surface smooth and silky, the anti-pilling and anti-hair sweater has the characteristics of glittering, soft fiber, high fastness. However, its overall strength and uniformity are poor. Summary of the invention
[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a preparation process for wool silk filament spinning, which solves the above-mentioned technical problems existing in the prior art.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A preparation process for spinning wool and silk filament yarns comprises the following steps:
[0008] S1, blending: combine, comb and draw multiple wool strips with other fiber strips to make the blended fibers straight and parallel to achieve the mixing of fibers of different colors and components;
[0009] S2, combing: straightening, parallelizing and separating the wool tops and blended fibers in S1 to produce evenly combed wool tops;
[0010] S3, needle combing: stretching, combing and merging wool tops and blended fibers to make multiple fiber tops straight and parallel, and then stretching and merging them again into fiber strips of a certain fineness;
[0011] S4, roving: further stretch the fiber strips combed out by needles to form fiber roving;
[0012] S5, spun yarn: according to the preset yarn count, the fiber roving is drafted and twisted into semi-finished yarn;
[0013] S6, winding: the semi-finished yarn is set after winding and cut into standard sizes;
[0014] S7, two-for-one twisting: the two-ply semi-finished yarn in S6 is twisted on a two-for-one twisting machine to obtain a finished yarn;
[0015] S8, waxing: waxing the finished yarn;
[0016] S7, testing and packaging: Packing the finished yarns that pass the test;
[0017] The finished yarn has a strength of 700-800 cN / cm, an elongation of 13-14%, and an unevenness of 16-17%.
[0018] Furthermore, in S1, ultrafine wool fiber, silk filament and nylon conductive fiber are selected as the blended fiber strip materials, wherein the index parameter of the ultrafine wool fiber is 15.5-17.5 mic.
[0019] Furthermore, in the blended fiber strip material, the ratio of superfine wool fiber, silk filament and nylon conductive fiber is 75%:21%:4%.
[0020] Furthermore, the blending is performed three times, combing is performed once, and six needle combings are performed to obtain the fiber strips.
[0021] Furthermore, the process parameters of the blending are: 10-14 slivers are mixed, the sliver weight is 20-24g / m, and the speed is 170-200m / min;
[0022] The process parameters of combing are: 18-22 strands combined and fed, speed 190m / min.
[0023] Furthermore, the six-track needle combing comprises the following specific steps:
[0024] One-stage needle combing: the drafting multiple is 6.5-7.5, the sliver weight is 28-30g / m, and the speed is 180-240m / min;
[0025] Secondary needle combing: 6-8 blended fibers are fed, the drafting ratio is 6-7, the sliver weight is 26-30g / m, and the speed is 180-240m / min;
[0026] Three-time needle combing: 6-8 blended fibers are fed, the drafting multiple is 6-7, the sliver weight is 22-26g / m, and the speed is 180-240m / min;
[0027] Four-pass needle combing: 3-4 blended fibers are fed, the drafting multiple is 7-8, the sliver weight is 8-12g / m, and the speed is 180-240m / min;
[0028] Five-pass needle combing: 3-4 blended fibers are fed, the drafting ratio is 7-8, the sliver weight is 3.5-4.5g / m, and the speed is 180-240m / min;
[0029] Six-pass needle combing: 3-4 blended fibers are fed, the drafting multiple is 7-8, the sliver weight is 1.5-2.5g / m, and the speed is 180-240m / min.
[0030] Furthermore, in S1-S9, the temperature is adjusted to 25±3°C and the humidity is adjusted to 65±5%.
[0031] Furthermore, the roving feeding used in S4 is single-strand feeding, with a drafting multiple of 11-12, a roving count of 5-7 Nm, and a speed of 150-170 m / min.
[0032] Furthermore, in the spun yarn in S5, one roving and one filament are fed, the drafting multiple is 19, the roving count is 95.8Nm, the speed is 830m / min, and the twist is 920 twists.
[0033] Furthermore, in the two-for-one twisting step used in S7, the preheating temperature is 70° C., the yarn steaming temperature is 90° C., and the vacuum is drawn twice.
[0034] Beneficial effects of the present invention:
[0035] 1. This application uses completely easy-care ultra-fine wool fibers to make the yarn soft, skin-friendly, and machine washable; uses black silk filaments to make the fabric shiny, soft, wrinkle-resistant, and have good moisture absorption properties; uses a small amount of black nylon conductive fibers to make it wash-resistant and anti-static.
[0036] 2. This application uses silk filaments as the covering yarn, which is different from the previous nylon filaments or polyester filaments. The spun yarns are strong, bright in color, good in texture, soft and comfortable, durable, and improve the subsequent weaving performance and the wearing performance of the clothing. Antistatic fibers are added to improve the conductivity of the yarns and prevent static electricity from causing discomfort to the human body.
[0037] 3. In this application, silk filaments are selected instead of commonly used nylon filaments because of their good color, texture and high-end appearance. Wool fibers are very easy to generate static electricity, so 4% of nylon conductive fibers are added to reduce static electricity generated by the yarn, and the yarn anti-pilling level reaches level 3-4. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.
[0039] Figure 1 It is a schematic diagram of the overall process of an embodiment of the present invention. DETAILED DESCRIPTION
[0040] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] like Figure 1 As shown, the embodiment of the present invention provides a preparation process for spinning wool silk filament yarn, comprising the following steps:
[0042] S1. Blending: Combine, comb and stretch several wool strips with other fiber strips to make the blended fibers straight and parallel, so as to achieve the mixing of fibers of different colors and different components; at this time, ultrafine wool fibers, silk filaments and nylon conductive fibers are selected as blended fiber strip materials, among which, completely easy-to-care ultrafine wool fibers (16.5mic / 70Hmm) are selected to make the yarn soft, skin-friendly and machine washable; black silk filaments are selected to make the fabric shiny, soft, wrinkle-resistant and have good moisture absorption properties; a small amount of black nylon conductive fibers are selected to have properties such as washing resistance and antistatic.
[0043] At this time, silk filament replaces the previous nylon filament or polyester filament. The fineness of silk filament is 22dtex, the silk twist is 800Z, and the number of roots is 1. It can be spun into ultra-high count (≥Nm100) or above yarn, and the yarn has high strength, good texture, softness and comfort, and durability. It is a high-end product; nylon filament or polyester filament is often used in medium and low count yarn (nylon filament parameters are: 22dtex, no twist, and the number of roots is commonly used. 6 and 12; polyester filament parameters are: 22dtex, no twist, and the number of roots is commonly used. 12).
[0044] At this time, taking into account the product purpose and production site, the best yarn ratio was determined to be 75% wool, 21% silk filament, and 4% nylon conductive fiber.
[0045] S2, combing: straighten, parallelize and separate the wool tops and blended fibers in S1 (in order to remove weeds, wool particles and other impurities) to make combed wool tops with uniform dryness;
[0046] S3, needle combing: stretching, combing and merging wool tops and blended fibers to make multiple fiber tops straight and parallel, with the function of self-leveling, so that each filament fiber is evenly mixed, and then stretched and merged again into fiber strips of a certain fineness;
[0047] The blending is done three times, combing is done once, and six needle combings are done to obtain fiber strips, and the wool filaments and antistatic nylon (nylon conductive fiber) are fully mixed and drawn.
[0048] The process parameters of sliver blending are: 10-14 slivers mixed, sliver weight 20-24g / m, speed 170-200m / min;
[0049] The process parameters of combing are: 18-22 strands combined and fed, speed 190m / min.
[0050] At the same time, the specific steps (process parameters) in the six-pass needle combing include the following:
[0051] One-stage needle combing: the drafting multiple is 6.5-7.5, the sliver weight is 28-30g / m, and the speed is 180-240m / min;
[0052] Secondary needle combing: 6-8 blended fibers are fed, the drafting ratio is 6-7, the sliver weight is 26-30g / m, and the speed is 180-240m / min;
[0053] Three-time needle combing: 6-8 blended fibers are fed, the drafting multiple is 6-7, the sliver weight is 22-26g / m, and the speed is 180-240m / min;
[0054] Four-pass needle combing: 3-4 blended fibers are fed, the drafting multiple is 7-8, the sliver weight is 8-12g / m, and the speed is 180-240m / min;
[0055] Five-pass needle combing: 3-4 blended fibers are fed, the drafting ratio is 7-8, the sliver weight is 3.5-4.5g / m, and the speed is 180-240m / min;
[0056] Six-pass needle combing: 3-4 blended fibers are fed, the drafting multiple is 7-8, the sliver weight is 1.5-2.5g / m, and the speed is 180-240m / min.
[0057] S4, roving: the fiber strips combed out by needles are further stretched to form fiber roving; when the roving is fed, it is single-strand feeding, and the drafting multiple is 11-12, the roving count is 5-7Nm, and the speed is 150-170m / min.
[0058] S5, spun yarn: according to the preset yarn count, the fiber roving is drawn and twisted into a semi-finished yarn; one roving and one filament are fed, the drafting multiple is 19, the roving count is 95.8Nm, the speed is 830m / min, and the twist is 920 twists.
[0059] S6. Winding: The semi-finished yarn is set after winding and cut into standard size, and harmful hairiness, foreign fibers, uneven thickness, etc. are cut off.
[0060] S7, two-for-one twisting: The two-ply semi-finished yarn in S6 is twisted on a two-for-one twisting machine to make the yarn more stable, thereby obtaining a finished yarn; the preheating temperature is 70°C, the steaming temperature is 90°C, and vacuuming is performed twice.
[0061] S8. Waxing: Waxing the finished yarn to reduce hairiness and improve the weavability of the yarn.
[0062] S7, testing and packaging: Packing of finished yarns that pass the test.
[0063] The finished yarn has a strength of 700-800 cN / cm, an elongation of 13-14%, and an unevenness of 16-17%.
[0064] During the spinning process of S1-S9, the temperature was adjusted to 25±3°C and the humidity to 65±5%.
[0065] When the yarn count is determined, the filament composition is determined accordingly. When the yarn trade count is 100, the composition is 79% wool and 21% nylon filament, the wool fineness is changed to determine the best wool fineness. When the wool fineness is 16.5mic, the strength is the best, the elongation is the best, the coarse and fine parts are the least, and the yarn uniformity is better.
[0066] As shown in Table 1 below, the spinning parameters are compared under different parameter conditions.
[0067] Table 1
[0068]
[0069] Because silk filaments have good color, texture, and high-end atmosphere, silk filaments are selected to replace commonly used nylon filaments. Wool fibers are very easy to generate static electricity, so 4% of nylon conductive fibers are added to reduce the static electricity generated by the yarn. The yarn anti-pilling level reaches level 3-4. Due to the addition of conductive fibers, the yarn uniformity cannot be tested. The test results of the yarn strength performance are shown in Table 2 below:
[0070] Table 2
[0071] Strength cN / cm Elongation % Unevenness CV% Pilling Grade 752 13.28 16.6 3-4
[0072] This preparation process uses silk filaments as the covering yarn, which is different from the previous nylon filaments or polyester filaments. The spun yarns are strong, bright in color, good in texture, soft and comfortable, and durable, which improves the subsequent weaving performance and the wearing performance of clothing. Antistatic fibers are added to improve the conductivity of the yarns and prevent static electricity from causing discomfort to the human body.
[0073] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A preparation process for spinning wool silk filament yarn, characterized in that: The following steps are involved: S1, blending: combine, comb and draw multiple wool strips with other fiber strips to make the blended fibers straight and parallel to achieve the mixing of fibers of different colors and components; S2, combing: straightening, parallelizing and separating the wool tops and blended fibers in S1 to produce evenly combed wool tops; S3, needle combing: stretching, combing and merging wool tops and blended fibers to make multiple fiber tops straight and parallel, and then stretching and merging them again into fiber strips of a certain fineness; S4, roving: further stretch the fiber strips combed out by needles to form fiber roving; S5, spun yarn: according to the preset yarn count, the fiber roving is drafted and twisted into semi-finished yarn; S6, winding: the semi-finished yarn is set after winding and cut into standard sizes; S7, two-for-one twisting: the two-ply semi-finished yarn in S6 is twisted on a two-for-one twisting machine to obtain a finished yarn; S8, waxing: waxing the finished yarn; S7, testing and packaging: Packing the finished yarns that pass the test; The finished yarn has a strength of 700-800 cN / cm, an elongation of 13-14%, and an unevenness CV of 16-17%.
2. The preparation process of wool silk filament spinning according to claim 1, characterized in that: In S1, ultrafine wool fiber, silk filament and nylon conductive fiber are selected as the blended fiber strip materials, wherein the index parameter of the ultrafine wool fiber is 15.5-17.5 mic.
3. The preparation process of wool silk filament spinning according to claim 2, characterized in that: In the blended fiber strip material, the proportion of superfine wool fiber, silk filament and nylon conductive fiber is 75%:21%:4%.
4. The preparation process of wool silk filament spinning according to claim 1, characterized in that: The blending is performed three times, and at the same time, the fiber strip is combed once and combed six times to obtain the fiber strip.
5. The preparation process of wool silk filament spinning according to claim 4, characterized in that: The process parameters of the mixed strips are: 10-14 strips are mixed, the weight of the strips is 20-24g / m, and the speed is 170-200m / min; The process parameters of combing are: 18-22 strands combined and fed, speed 190m / min.
6. The process for preparing wool silk filament spinning according to claim 4, characterized in that: The specific steps of the six-way needle combing include the following: One-stage needle combing: the drafting multiple is 6.5-7.5, the sliver weight is 28-30g / m, and the speed is 180-240m / min; Secondary needle combing: 6-8 blended fibers are fed, the drafting ratio is 6-7, the sliver weight is 26-30g / m, and the speed is 180-240m / min; Three-time needle combing: 6-8 blended fibers are fed, the drafting multiple is 6-7, the sliver weight is 22-26g / m, and the speed is 180-240m / min; Four-pass needle combing: 3-4 blended fibers are fed, the drafting multiple is 7-8, the sliver weight is 8-12g / m, and the speed is 180-240m / min; Five-pass needle combing: 3-4 blended fibers are fed, the drafting ratio is 7-8, the sliver weight is 3.5-4.5g / m, and the speed is 180-240m / min; Six-pass needle combing: 3-4 blended fibers are fed, the drafting multiple is 7-8, the sliver weight is 1.5-2.5g / m, and the speed is 180-240m / min.
7. The preparation process of wool silk filament spinning according to claim 1, characterized in that: In S1-S9, the temperature is adjusted to 25±3°C and the humidity is adjusted to 65±5%.
8. The process for preparing wool silk filament spinning according to claim 1, characterized in that: The roving feeding adopted in S4 is single-strand feeding, and the drafting multiple is 11-12, the roving count is 5-7Nm, and the speed is 150-170m / min.
9. The process for preparing wool silk filament spinning according to claim 1, characterized in that: In the S5, one roving and one filament are fed into the spun yarn, the draft multiple is 19, the roving count is 95.8Nm, the speed is 830m / min, and the twist is 920 twists.
10. The preparation process of wool silk filament spinning according to claim 1, characterized in that: The two-for-one twisting step in S7 has a preheating temperature of 70° C., a yarn steaming temperature of 90° C., and is vacuumed twice.
Citation Information
Patent Citations
Method for producing and processing wool blended yarn
CN107245782A
Production process of silk, cow suede and wool blended yarns
CN109989143A
High-count wool-blended elastomeric yarn and preparation method thereof
CN110184701A
Preparation process of conductive fiber wool blended yarn
CN112239905A
Preparation method of high-end circular knitting machine yarn with stable anti-pilling performance
CN114108147A