Polyurethane moistened leather and preparation method thereof

Through wet coating and dry filming processes, the thickness, feel and peel strength of synthetic leather are improved, and the problems of the existing synthetic leather are not light enough and soft enough, achieving higher physical properties and wider applications .

CN118996868APending Publication Date: 2024-11-22ZHEJIANG HEXIN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411098865.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing synthetic leather is not thin enough, the feel is not soft enough, and the peeling strength needs to be improved, which cannot meet the needs of use.

Method used

Wet coating and dry filming are used to modify the performance and bonding interface of the base cloth, and film transfer technology is used to apply filming to improve the utilization efficiency and bonding performance of materials, reduce resource waste, and use specific resins The formulation and process parameters are optimized to form a thinner, softer and higher peel strength polyurethane hydrating leather.

Benefits of technology

The obtained polyurethane hydrating leather has thinner thickness, softer feel, higher peel strength, better overall physical properties, and is suitable for a wider range of application fields and has higher practicality and competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996868A_ABST
    Figure CN118996868A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of synthetic leather preparation, and particularly relates to polyurethane moisturized leather and a preparation method thereof. The preparation process of the polyurethane moistened leather comprises two steps of a wet method and a dry method. In the wet process, the fitting interface of the base cloth is adjusted by changing the performance of the base cloth, and a foundation is laid for subsequent dry fitting. In the dry-method film-making process, an advanced film transfer technology is used, and an integrated film-forming method is adopted, so that the utilization efficiency of materials is improved, and resource waste is reduced. The polyurethane moistened leather provided by the invention has more product advantages, the ultrathin thickness of 0.7 mm, and high peel strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of synthetic leather preparation, and particularly relates to polyurethane moisturizing leather and a preparation method thereof. Background Art

[0002] Synthetic leather is a plastic product that simulates the composition and structure of natural leather and can be used as a substitute material for it. It is usually made of impregnated non-woven fabric as a mesh layer and a microporous polyurethane layer as a grain layer. Both its front and back sides are very similar to leather and have a certain degree of air permeability, which is closer to natural leather than ordinary artificial leather. It is widely used in the production of shoes, boots, bags and balls. In 2008, after long-term research, my country successfully developed dry synthetic leather, wet synthetic leather and other process technologies, ending the monopoly of domestic and foreign giants on the synthetic leather industry, and using water-based polyurethane technology in clothing leather, sofa leather and other fields.

[0003] In the development of synthetic leather, there is still a big gap in the diversity of ultra-soft synthetic leather. For example, the thickness of synthetic leather is still not thin enough to meet the needs of use; the feel is not soft enough, and the peel strength still needs to be improved. Summary of the invention

[0004] The purpose of the present invention is to provide a polyurethane water-moistened leather, which has good simulation and excellent usability.

[0005] The technical solution adopted by the present invention to solve its technical problem is:

[0006] A method for preparing polyurethane water-moistened leather, the method comprising the following steps:

[0007] S1. Wet coating

[0008] The base fabric is completely immersed in the impregnation liquid, and after the base fabric is completely soaked, it is rolled by a rolling mill, and after the grey fabric is fully impregnated, the excess impregnation liquid is rolled out; the impregnation liquid is an N,N-dimethylformamide (DMF) aqueous solution with a mass concentration of 15% to 25%;

[0009] Coating a wet slurry on the impregnated base fabric, wherein the formula of the wet slurry is: 100 parts of polyether polyurethane resin, 25-35 parts of carboxymethyl cellulose, 8-12 parts of protein-imitation additive, 0.1-1 part of defoaming agent, 140-150 parts of N,N-dimethylformamide, and 0-10 parts of color paste in parts by weight;

[0010] The base fabric coated with the wet slurry is immersed in a coagulation liquid at 25°C-32°C to stably combine the coating material with the base fabric. The coagulation liquid is an N,N-dimethylformamide aqueous solution with a mass concentration of 15% to 20%.

[0011] At a temperature of 40℃-60℃, use a rolling mill to remove the residual slurry, additives, etc. in the solidified wet-process Base semi-finished product;

[0012] Pre-drying;

[0013] After the pre-drying treatment, the wet-process Base semi-finished product is thoroughly dried to remove the N,N-dimethylformamide solvent and completely solidify the coating material to form the final form of the wet-process Base;

[0014] S2, dry film lamination

[0015] The film transfer technology is adopted, and a pressure roller is used to laminate the surface film onto the wet base, and the product is obtained after drying.

[0016] The preparation method of the polyurethane water-moistened leather provided by the present invention first changes the bonding interface of the grey cloth by a wet process, and then changes the bonding interface by a dry process, thereby improving the physical properties of the soft synthetic leather. The prepared product is thinner, softer in feel, and has higher peeling strength than other similar soft synthetic leather products. The comprehensive physical properties are better and more practical.

[0017] As a preference, in S1, the rolling mill pressure is 5-6 kg / cm 2 .

[0018] Preferably, in S1, the impregnated base fabric is passed through an oven or a hot pressing roller in advance, and the temperature of the base fabric is controlled at 60° C.-70° C. to increase the viscosity of the coating material before coating the wet slurry.

[0019] Preferably, in S1, when the wet slurry is coated, the coating scraper height is about 0.8-1.0 mm; the coating process requires secondary coating to ensure that the wet slurry is completely and evenly coated on the base fabric.

[0020] Preferably, the product obtained by S2 dry film lamination is sent to a continuous texture processing machine for surface texture treatment.

[0021] Preferably, the surface film formula is: 60-80 parts by weight of polycarbonate polyurethane resin, 20-40 parts by weight of polyester polyurethane resin, appropriate amount of color paste and solvent, and the film is fixed to the wet base through an adhesive layer.

[0022] Preferably, the formula of the bonding layer is 100 parts of polyether polyurethane resin with a solid content of 35%, 12 parts of oily color paste, 40 parts of N,N-dimethylformamide, and 20 parts of ethyl acetate.

[0023] Preferably, pre-drying is achieved using an oven, and there are 10 groups of ovens in total, the first oven is 60°C, the second oven is 100°C, the third, fourth and fifth ovens are 140°C, and the sixth to tenth ovens are 170°C; the total drying time is controlled between 15 minutes and 20 minutes.

[0024] Preferably, the formula of the wet slurry is: 100 parts of polyether polyurethane resin, 30 parts of carboxymethyl cellulose, 10 parts of protein-imitation additive, 0.3 parts of defoaming agent, 140-150 parts of N,N-dimethylformamide, and 0-10 parts of color paste in parts by weight.

[0025] A polyurethane water-moisturized leather prepared by the preparation method of the present invention.

[0026] The beneficial effects of the present invention are:

[0027] 1. The preparation process of the polyurethane water-moistened leather of the present invention includes two steps: wet process and dry process. In the wet process, the bonding interface of the base fabric is adjusted by changing the performance of the base fabric, laying the foundation for the subsequent dry bonding. In the dry film-making process, advanced film transfer technology is used to improve the utilization efficiency of materials and reduce resource waste through an integrated film-forming method. The reuse of N,N-dimethylformamide reduces waste gas pollution and plays a positive role in environmental protection.

[0028] 2. Traditional polyurethane synthetic leather mainly uses solvent-based polyurethane resin as the material for the surface layer and base layer. The development of polyurethane water-moisturized leather includes two parts: wet base and dry veneer attached to the wet base. The synthetic leather prepared in this way is better than traditional soft synthetic leather in performance and physical properties. Such design process also helps to avoid the situation where the dry veneer leaks the fabric texture, which can give the synthetic leather more unique style.

[0029] 3. For the current synthetic leather market, the polyurethane moisturized leather of the present invention has more product advantages. The ultra-thin thickness of 0.7 mm and high peel strength both demonstrate the excellent properties of polyurethane moisturized leather. It also has a wider range of application fields and can be used in products such as luggage. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is an electron microscope structure diagram of the product cross section. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is further described in detail below through specific embodiments. It should be understood that the implementation of the present invention is not limited to the following embodiments, and any form of modification and / or change made to the present invention will fall within the protection scope of the present invention.

[0032] In the present invention, unless otherwise specified, all parts and percentages are by weight, and the equipment and raw materials used can be purchased from the market or are commonly used in the art. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.

[0033] The reagents used in the following examples, unless otherwise specified, can be purchased from conventional biochemical reagent stores.

[0034] Polyether polyurethane resin, solid content 32%, polymer of polyether polyol and diisocyanate; polycarbonate polyurethane resin, bisphenol A polycarbonate, model 1880W; polyester polyurethane resin, 8120, solid content 30%; polyether polyurethane resin, 9521, solid content 35%, all resins were purchased from Zhejiang Hexin Technology Co., Ltd.;

[0035] Carboxymethyl cellulose, model 325; protein-imitation additive, polyether-modified aminopolysiloxane compound, model LX-3068-6; defoamer, block copolymer of ethylene oxide and propylene oxide, model DX-25, all three additives were purchased from Zhejiang Luoxing New Materials Co., Ltd.

[0036] Color paste, high pigment content resin-free system, commercially available; oil-based color paste, commercially available.

[0037] Example 1

[0038] A method for preparing polyurethane water-moistened leather, the method comprising two processes of wet coating and dry film lamination, the specific steps are as follows:

[0039] S1. Wet coating

[0040] Wet coating is used to improve the bonding effect of the grey fabric bonding surface. The improvement of the bonding interface provides a guarantee for the subsequent dry film bonding.

[0041] 1. Unwinding of base fabric: The selected base fabric is passed through the unwinding device, the base fabric is fully unfolded, and a certain tension is given to the base fabric to prepare for the subsequent impregnation process; the thickness of the base fabric is about 0.55mm.

[0042] 2. Impregnation: Immerse the base fabric completely in an aqueous solution containing 20% ​​N,N-dimethylformamide, and then roll it with a rolling mill. The rolling mill pressure is 5-6kg / cm 2 , after the grey cloth is fully impregnated, the excess impregnation liquid is squeezed out;

[0043] 3. Heating: The impregnated base fabric is passed through a hot pressing roller at a temperature of about 65°C to heat the front side of the base fabric in a single round to increase the viscosity of the coating material;

[0044] 4. Coating: Coat the prepared wet slurry on the impregnated base fabric, and the coating scraper height is about 0.8-1.0mm. The coating process requires secondary coating to ensure that the wet slurry is completely and evenly coated on the base fabric; the wet slurry formula is shown in Table 1.

[0045] Table 1 Wet slurry raw material ratio (unit kg)

[0046] Polyurethane resin Polyether polyurethane resin (solid content 32%) 100 Additives Carboxymethyl cellulose 30 Additives Protein-like additives 10 Additives Defoaming agent 0.3 Solvents N,N-Dimethylformamide 140-150 Color paste High pigment content resin-free system 0-10

[0047] 5. Solidification: The base fabric coated with wet slurry is immersed in a solidification liquid at 25℃-32℃ to ensure a stable combination of the coating material and the base fabric;

[0048] The coagulation liquid is a 20% N,N-dimethylformamide aqueous solution. The base fabric is completely immersed in the coagulation liquid, which is used to absorb the DMF in the product. 6. Water washing: The residual slurry, additives, etc. in the coagulated wet-process Base semi-finished product are removed through the rolling mill equipment. The water washing temperature is 40℃-60℃;

[0049] 7. Pre-drying: Pre-dry the washed wet-process Base semi-finished product to remove some moisture and prepare for subsequent complete drying.

[0050] Pre-drying is achieved by using an oven, and there are 10 sets of ovens in total, the first oven is 60°C, the second oven is 100°C, the third, fourth and fifth ovens are 140°C, and the sixth to tenth ovens are 170°C. The total drying time is controlled between 15 minutes and 20 minutes.

[0051] 8. Drying: After the pre-drying treatment, the wet-process Base semi-finished product is thoroughly dried to remove the N,N-dimethylformamide solvent, so that the coating material is completely solidified to form the final form of the wet-process Base.

[0052] 9. Rewinding: The dried wet-based Base is passed through the rewinding device and rolled onto a roller for use in the dry process.

[0053] Through the wet process, the improvement of the bonding interface provides guarantee for subsequent production and processing.

[0054] S2, dry film lamination

[0055] Use polycarbonate polyurethane resin with the appropriate type of color paste to make a uniformly dispersed film-forming slurry. Through precise control of the equipment coating knife, a coating with a thickness of less than 10μm is formed on the surface of the release paper. According to the characteristics of the polycarbonate polyurethane material, a wax-like material is given to the surface of the product, making the surface of the product feel smoother. After the temperature of the oven is controlled, it is ensured that the surface material is dried while avoiding excessive temperature that causes film peeling, cracking, and denaturation. After the surface film is formed, the subsequent film-forming process is carried out to add a polyurethane film with certain properties. Select polyether polyurethane resin, select color paste with good applicability, and prepare the film-forming slurry. Through the second film-forming process, this film-forming empowers the overall performance of the product. Polyether polyurethane materials have better strength, tear strength, wear resistance and other properties. Polyether polyol molecules with low cohesive energy in ether bonds are easier to rotate, which makes polyether polyurethane materials have better low-temperature flexibility. The use of polyether polyurethane materials can better improve the durability and usability of the product. While ensuring the fashion of the products, the products have high physical properties and are more competitive in the synthetic leather market.

[0056] Control the oven temperature and monitor the wetness and dryness of the slurry. When the slurry is in a semi-dry state before it completely becomes a skin, use a pressing roller to stick the surface film to the wet base. After drying in the oven, the designed product is formed.

[0057] Using film transfer technology, the surface film is laminated on the wet base obtained in the previous step using a pressure roller, and the product is obtained after sufficient drying. The film is fixed to the wet base through the adhesive layer.

[0058] The specific dry material formula is shown in Table 2.

[0059] Table 2 (Unit: kg)

[0060]

[0061]

[0062] S3, continuous texture post-processing

[0063] After the dry process is completed, the product is sent to the continuous texture processor for processing. The continuous texture processor can better improve the surface texture of the product. The electron microscope structure of the cross section of the product is shown in Figure 1 .

[0064] Comparative Example 1

[0065] A method for preparing polyurethane water-moistened leather, the method comprising two processes of wet coating and dry film lamination, the specific steps are the same as those in Example 1, except that:

[0066] 1. The thickness of the base fabric is 0.75mm.

[0067] 2. The wet slurry raw materials do not contain protein-imitation additives, and the polyether polyurethane resin is changed to polycarbonate polyurethane resin, and the dosage remains unchanged.

[0068] The reason why a thicker base cloth is used in this comparative example is that if a base cloth of the same thickness as that of Example 1 is used, the physical properties such as strength and wear resistance after testing do not meet the standards.

[0069] Comparative Example 2

[0070] A method for preparing polyurethane water-moistened leather comprises two processes of wet coating and dry film lamination. The specific steps are the same as those in Example 1, except that the polyether polyurethane resin is replaced by a polycarbonate polyurethane resin, and the dosage remains unchanged.

[0071] This comparative example only changes the type of polyurethane resin used in the wet slurry raw material. Conclusion: Changing the wet resin has a great impact on the wet semi-finished product, directly affecting the stripping performance of the product and the overall practicality of the product.

[0072] Comparative Example 3

[0073] A method for preparing polyurethane water-moistened leather comprises two processes of wet coating and dry film lamination. The specific steps are the same as those in Example 1, except that: the amount of polyether polyurethane resin (solid content 32%) in the wet slurry raw material in Table 1 is 80 kg.

[0074] This comparative example only changes the amount of polyurethane resin used in the wet slurry raw material. Conclusion: The main body of polyether polyurethane is to control the softness of the wet semi-finished product. Reducing the amount of polyether resin used will reduce the softness of the product and affect the product use effect.

[0075] Comparative Example 4

[0076] A method for preparing polyurethane water-moistened leather comprises two processes of wet coating and dry film lamination. The specific steps are the same as those in Example 1, except that: the amount of polyether polyurethane resin (solid content 32%) in the wet slurry raw material in Table 1 is 90 kg.

[0077] This comparative example only changes the amount of polyurethane resin used in the wet slurry raw material. Conclusion: Compared with comparative example 3, the wet semi-finished product of comparative example 4 has higher softness and makes the product feel softer.

[0078] Comparative Example 5

[0079] A method for preparing polyurethane water-moistened leather comprises two processes of wet coating and dry film lamination. The specific steps are the same as those in Example 1, except that the pre-drying in step 7 is omitted and direct drying is performed.

[0080] The wet-process Base results in serious DMF residue, excessive humidity resulting in uneven distribution of the wet-process slurry, affecting the muscle-forming effect of the wet-process slurry, and affecting the physical properties of the product.

[0081] Comparative Example 6

[0082] A method for preparing polyurethane moisturized leather comprises two processes of wet coating and dry film lamination. The specific steps are the same as those in Example 1, except that: Step 7, pre-drying: no gradient drying is set, but direct drying at 130° C. to 140° C. for 15 to 20 minutes is adopted.

[0083] Problems that arise: The wet semi-finished product is not completely dried, resulting in a "surface drying" phenomenon, and the slurry that penetrates into the base fabric is not completely dried, which has an adverse effect on the subsequent dry process.

[0084] Comparative Example 7

[0085] A method for preparing polyurethane moisturized leather comprises two processes of wet coating and dry film lamination. The specific steps are the same as those in Example 1, except that the formula of the adhesive layer in Table 2 is changed to: 80 kg of polyether polyurethane resin (solid content 35%), 12 kg of oily color paste, 50 kg of N,N-dimethylformamide, and 30 kg of ethyl acetate.

[0086] Problems that arise: The dry film and the wet semi-finished product are not firmly bonded, the physical properties of the product are reduced, and the physical properties such as wear resistance and peeling are not up to expectations.

[0087] Comparative Example 8

[0088] A method for preparing polyurethane moisturized leather comprises two processes of wet coating and dry film lamination. The specific steps are the same as those in Example 1, except that: in the formula of the surface layer in Table 2, 80 kg of polycarbonate polyurethane resin and 20 kg of polyester polyurethane resin (solid content 30%) are changed to 100 kg of polyester polyurethane resin (solid content 30%).

[0089] Problems that arise: The product is not soft enough and not smooth enough, which will cause problems such as low customer satisfaction.

[0090] Performance test

[0091] The products obtained by the above method were tested, and the comparison results of experimental test data are shown in Table 3.

[0092] Table 3

[0093]

[0094] Table 3 continued

[0095]

[0096] The average softness of the product in comparative example 1 is about 5.9 mm, and the thickness is about 0.82 mm, while the average softness of the new product prepared by the present invention is about 7.0 mm, and the thickness is reduced to about 0.65 mm. The present invention adds the use of protein-like additives in the wet slurry, changes the choice of resin, and finally achieves the effect of excellent softness and lightness of the product.

[0097] The present invention adopts a wet coating process to improve the intrinsic strength of the substrate, applies advanced interface engineering and innovative processes to improve the bonding performance between polyurethane and the substrate, and achieves a synthetic leather peel strength of more than 18N / 3CM. The material adopts an innovative formula to increase the interaction between polyurethane molecular chains, giving the product high durability. The present invention uses an appropriate amount of protein-like additives in the wet process to give the product a softer and more elastic characteristic, making the product more soft like baby skin.

[0098] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0099] The above is a detailed introduction to a polyurethane water-moistened leather and a preparation method thereof provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, the present invention can also be improved and modified in a number of ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing polyurethane water-moistened leather, characterized in that The method comprises the following steps: S1. Wet coating The base fabric is completely immersed in the impregnation liquid, and after the base fabric is completely soaked, it is rolled by a rolling mill, and after the grey fabric is fully impregnated, the excess impregnation liquid is rolled out; the impregnation liquid is an N,N-dimethylformamide (DMF) aqueous solution with a mass concentration of 15% to 25%; Coating a wet slurry on the impregnated base fabric, wherein the formula of the wet slurry is: 100 parts of polyether polyurethane resin, 25-35 parts of carboxymethyl cellulose, 8-12 parts of protein-imitation additive, 0.1-1 part of defoaming agent, 140-150 parts of N,N-dimethylformamide, and 0-10 parts of color paste in parts by weight; The base fabric coated with the wet slurry is immersed in a coagulation liquid at 25°C-32°C to stably combine the coating material with the base fabric. The coagulation liquid is an N,N-dimethylformamide aqueous solution with a mass concentration of 15% to 20%. At a temperature of 40℃-60℃, use a rolling mill to remove the residual slurry, additives, etc. in the solidified wet-process Base semi-finished product; Pre-drying; After the pre-drying treatment, the wet-process Base semi-finished product is thoroughly dried to remove the N,N-dimethylformamide solvent and completely solidify the coating material to form the final form of the wet-process Base; S2, dry film lamination The film transfer technology is adopted, and a pressure roller is used to laminate the surface film onto the wet base, and the product is obtained after drying.

2. The method for preparing polyurethane water-moistened leather according to claim 1, characterized in that: In S1, the rolling mill pressure is 5-6kg / cm 2 .

3. The method for preparing polyurethane water-moistened leather according to claim 1, characterized in that: In S1, the impregnated base fabric is passed through an oven or a hot pressing roller in advance, and the temperature of the base fabric is controlled at 60° C.-70° C. to increase the viscosity of the coating material before coating the wet slurry.

4. The method for preparing polyurethane water-moistened leather according to claim 1, characterized in that: In S1, when the wet slurry is applied, the coating scraper height is about 0.8-1.0 mm; the coating process requires secondary coating to ensure that the wet slurry is completely and evenly applied to the base fabric.

5. The method for preparing polyurethane water-moistened leather according to claim 1, characterized in that: The products obtained by S2 dry film lamination are sent to the continuous texture processing machine for surface texture treatment.

6. The method for preparing polyurethane water-moistened leather according to claim 1, characterized in that: The formula of the surface film is: 60-80 parts by weight of polycarbonate polyurethane resin, 20-40 parts by weight of polyester polyurethane resin, appropriate amount of color paste and solvent, and the film is fixed to the wet base through an adhesive layer.

7. The method for preparing polyurethane water-moistened leather according to claim 6, characterized in that: The formula of the bonding layer is 100 parts of polyether polyurethane resin with a solid content of 35%, 12 parts of oily color paste, 40 parts of N,N-dimethylformamide, and 20 parts of ethyl acetate.

8. The method for preparing polyurethane water-moistened leather according to claim 1, characterized in that: Pre-drying is achieved using an oven. There are 10 groups of ovens in total. The first oven is 60°C, the second oven is 100°C, the third, fourth and fifth ovens are 140°C, and the sixth to tenth ovens are 170°C; the total drying time is controlled between 15 minutes and 20 minutes.

9. The method for preparing polyurethane water-moistened leather according to claim 1, characterized in that: The formula of the wet slurry is: 100 parts of polyether polyurethane resin, 30 parts of carboxymethyl cellulose, 10 parts of protein-imitation additive, 0.3 parts of defoaming agent, 140-150 parts of N,N-dimethylformamide, and 0-10 parts of color paste in parts by weight.

10. A polyurethane water-moistened leather prepared by the preparation method according to claim 1.