Paper tube base paper with good bursting resistance and preparation method thereof
By mixing waste paper with nanocellulose and modified starch and treating it with surface glue, the problem of poor paper strength and breakage resistance of paper tube base paper is solved, and the physical properties and quality of paper is effectively improved, satisfying the satisfaction of the satisfaction of the Demand in the high-end market.
Patent Information
- Application Number
- CN202411254885.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-22
AI Technical Summary
The paper-forming strength and breakability of existing paper tube base paper are poor, and cannot meet the requirements of the high-end market.
After mixing waste paper pulp, nanocellulose organic pulp and modified starch, it is sprayed to the mesh surface to dehydrate and form, coated with surface glue and dried to prepare paper with good break resistance. Tube of base paper. The method includes the cross-linking structure of nanocellulose and modified starch, which enhances the fiber binding force, and the surface glue is closely combined with the paper fiber through hydrogen bonds to improve the physical properties of the paper.
It significantly improves the tensile strength, thermal stability, chemical stability and breakage resistance of paper, improves the overall quality and economic efficiency of paper, and meets the needs of the high-end market.
Smart Images

Figure BDA0005033722440000141
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of paper tube base paper, and in particular to a paper tube base paper with good bursting resistance and a preparation method thereof. Background Art
[0002] Paper tube base paper is a general term for various raw paper used to make paper tubes. It is a very popular industrial paper, including chemical fiber paper tubes, textile yarn tubes, industrial paper tubes for papermaking, paper tubes for plastic films, etc. It has the advantages of low cost, light weight, easy recycling, and pollution-free. Paper tube base paper is mainly produced from various fiber raw materials such as recycled fibers from waste cardboard boards. It is an environmentally friendly and ecological product. At present, under the dual pressure of environment and resources, waste paper fibers are reused many times, resulting in the decline of quality, fiber strength, fiber elasticity, and fiber bonding force of waste paper fibers used as raw materials for paper tube base paper. The produced paper has poor strength and tear resistance, and can only be used in the mid- and low-end markets, and cannot meet the requirements of the high-end market. Summary of the invention
[0003] The purpose of the present invention is to provide a paper tube base paper with good bursting resistance and a preparation method thereof, so as to solve the problem that the current paper tube base paper has poor paper strength and poor bursting resistance.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0005] A method for preparing a paper tube base paper with good burst resistance, the preparation method comprising:
[0006] Waste paper pulp, nanocellulose organic pulp and modified starch are mixed and stirred evenly to obtain a mixed pulp; the mixed pulp, dry strength agent, waterproofing agent and deionized water are mixed, and then the pulp for mesh is obtained through slag removal, degassing and screening; the pulp for mesh is sprayed onto the mesh surface for dehydration; base paper is obtained through forming, extrusion and drying; surface glue is applied on the surface of the base paper, and the paper is dried and rewound to obtain a paper tube base paper with good tear resistance.
[0007] As a limitation of the present invention, the paper tube base paper raw material with good burst resistance includes, by mass fraction, 2.2-6.8% of nano-cellulose fiber organic pulp, 1.0-1.6% of dry strength agent, 1.5-2.5% of waterproofing agent, 1.0-1.6% of starch, 0.4-1.0% of auxiliary agent, and the rest is waste paper pulp.
[0008] As a limitation of the present invention, the method for preparing the waste paper pulp is:
[0009] The waste paper is pre-treated by screening, impurity removal and pulverization. 10 to 14 parts of pre-treated waste paper, 85 to 89 parts of deionized water and 0.5 to 1.5 parts of an auxiliary agent are mixed by weight and soaked for 3 to 5 hours to obtain a mixture. The mixture is dissociated and impurities are removed to obtain waste paper pulp.
[0010] As a limitation of the present invention, the additives include, by mass fraction, 38-42% sodium hydroxide, 6-10% sodium dodecyl sulfate, 10-14% fatty alcohol polyoxyethylene ether, 13-17% methylene dithiocyanate, and 23-27% polyethylene oxide.
[0011] As a limitation of the present invention, the method for preparing the nanocellulose fiber organic pulp is:
[0012] Mix nano-titanium dioxide with toluene, and ultrasonically disperse for 25 to 35 minutes to obtain a nano-titanium dioxide dispersion, add KH-550 and triethylamine to the nano-titanium dioxide dispersion, react at 90 to 100° C. for 5 to 7 hours, filter, wash with ethanol, and vacuum dry to obtain modified nano-titanium dioxide;
[0013] The modified nano titanium dioxide and deionized water are fully mixed and ultrasonically dispersed for 10 to 20 minutes to obtain a modified nano titanium dioxide dispersion. The bleached kraft softwood pulp board is crushed, mixed with deionized water, and fully soaked for 3 to 5 hours to obtain a coarse pulp. The coarse pulp and deionized water are mixed and beaten at a beating speed of 7500 to 8500r to obtain a fiber pulp. The fiber pulp is mixed with the modified nano titanium dioxide dispersion to obtain a nanocellulose organic fiber pulp.
[0014] As a limitation of the present invention, the preparation method of the modified starch is:
[0015] Starch and deionized water are mixed and stirred to obtain starch latex, 3% sodium hydroxide solution is added to the starch latex to adjust the pH to 9.5-10.5, sodium trimetaphosphate is added, and the reaction is carried out at 40-50° C. and 20-40 rpm for 1-3 hours, and then the pH of the reaction system is adjusted to 7.5-8.5 with hydrochloric acid, acetic anhydride is added, and the reaction is continued at 40-50° C. and 20-40 rpm for 1-2 hours, and the reaction system is neutralized with hydrochloric acid and dried to obtain modified starch.
[0016] As a limitation of the present invention, the preparation method of the surface glue is:
[0017] At 85-95°C, polyvinyl alcohol and deionized water are mixed and stirred to obtain a polyvinyl alcohol solution. The polyvinyl alcohol solution and KH-550 are mixed, and the pH value of the reaction system is adjusted to 7-8 with sodium hydroxide solution. The reaction is carried out at 55-65°C and 150-250rpm for 1-3h to obtain a polyvinyl alcohol-coupling agent solution. The polyvinyl alcohol solution, the polyvinyl alcohol-coupling agent solution and propylene glycol are mixed and stirred to obtain a surface adhesive solution.
[0018] As a limitation of the present invention, the mass ratio of the polyvinyl alcohol solution, the polyvinyl alcohol-coupling agent solution, and glycerol is (3.8-4.2):(0.8-1.2):(0.8-1.2).
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The starch modified by cross-linking and esterification with sodium trimetaphosphate and acetic anhydride introduces ester groups and cross-linking structures, which enhances hydrophilicity, mechanical strength, resistance to mechanical shear, and viscosity stability. It can combine well with paper fibers and improves the tear resistance of the finished paper.
[0021] Nanocellulose has a large number of hydroxyl groups on its surface and can easily form flocs in water. After being blended with nano-titanium dioxide modified with a silane coupling agent, the modified nano-titanium dioxide particles and cellulose are tightly combined together through intermolecular forces, which not only improves the dispersibility of nanocellulose in water, but also improves the tensile strength, thermal stability, and chemical stability of paper.
[0022] The surface sizing process will greatly improve the physical properties and printability of paper, and improve the quality grade and economic efficiency of paper. Polyvinyl alcohol, as a surface glue, contains a large number of hydroxyl groups in its macromolecular chain, which can form hydrogen bonds with paper fibers to improve the physical properties of paper. After polyvinyl alcohol is modified with silane coupling agent, the physical properties of paper can be further improved. Polyvinyl alcohol modified with silane coupling agent is applied to paper as a surface glue. The modified polyvinyl alcohol forms hydrogen bonds with paper fibers through the hydroxyl groups in the molecular chain, thus tightly bonding together, thereby improving the physical properties of paper such as tear resistance and tensile strength. DETAILED DESCRIPTION
[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Waste paper (national waste COCC12#) and starch (S18760) were provided by Shanghai Jizhi, nano titanium dioxide (R007222), polyvinyl alcohol (Mn=27000), KH-550 silane coupling agent (R003068), and polyethylene oxide (Mn=600000) were provided by Shanghai Yien Chemical, bleached kraft coniferous wood pulp board (whiteness 89) was provided by Dalian Yangrun, JH1216 dry strength agent (solid content 20%) was provided by Qingzhou Jinhao, EUM782 waterproofing agent (solid content 41%) was provided by Shanghai Aiken, and fatty alcohol polyoxyethylene ether (AEO-9) was provided by Wuhan Jiyesheng.
[0025] Calculated by mass fraction, the additives include 40% sodium hydroxide, 8% sodium dodecyl sulfonate, 12% fatty alcohol polyoxyethylene ether, 15% methylene dithiocyanate, and 25% polyethylene oxide.
[0026] Embodiment 1: A paper tube base paper with good burst resistance, the preparation method is as follows:
[0027] Step 1: Preparation of modified starch
[0028] By mass, 1.15 parts of starch and 1.48 parts of deionized water were mixed and stirred to obtain starch latex. A 3% sodium hydroxide solution was added to the starch latex to adjust the pH to 10.0, 0.0132 parts of sodium trimetaphosphate were added, and the mixture was reacted at 45° C. and 30 rpm for 2 hours. The pH of the reaction system was adjusted to 8.0 with hydrochloric acid, acetic anhydride was added, and the reaction was continued at 45° C. and 30 rpm for 1.5 hours. The pH of the reaction system was neutralized to neutral with hydrochloric acid, and the mixture was dried to obtain modified starch.
[0029] Step 2: Preparation of modified nano-titanium dioxide
[0030] Mix 5 parts of nano-titanium dioxide and 218 parts of toluene, and ultrasonically disperse for 30 minutes to obtain a nano-titanium dioxide dispersion. Add 1.89 parts of KH-550 silane coupling agent and 0.4 parts of triethylamine to 223 parts of the nano-titanium dioxide dispersion, react at 95°C for 6 hours, filter, wash with ethanol, and vacuum dry to obtain modified nano-titanium dioxide.
[0031] Step 3: Preparation of Nanocellulose Organic Fiber Pulp
[0032] By mass, 1.5 parts of modified nano titanium dioxide and 18.5 parts of deionized water were fully mixed and ultrasonically dispersed for 15 minutes to obtain a modified nano titanium dioxide dispersion. 10 parts of bleached sulfate softwood pulp boards were crushed and mixed with 40 parts of deionized water. After being fully soaked for 4 hours, they were dispersed to obtain a coarse pulp. 50 parts of the coarse pulp and 30 parts of deionized water were mixed and pulped at a beating speed of 8000r to obtain fiber pulp. 80 parts of the fiber pulp were mixed with 20 parts of the modified nano titanium dioxide dispersion to obtain nanocellulose organic fiber pulp.
[0033] Step 4: Prepare the surface glue
[0034] By mass, at 90°C, 1 part of polyvinyl alcohol and 9 parts of deionized water were mixed and stirred to obtain a polyvinyl alcohol solution; 9 parts of polyvinyl alcohol solution and 1.2 parts of KH-550 silane coupling agent were mixed, and the pH of the reaction system was adjusted to 7.5 with 10% sodium hydroxide solution, and the reaction was carried out at 60°C and 200rpm for 2h to obtain a polyvinyl alcohol-coupling agent solution; the polyvinyl alcohol solution, the polyvinyl alcohol-coupling agent solution and propylene glycol were mixed in a mass ratio of 4.0:1.0:1.0, and stirred to obtain a surface glue solution.
[0035] Step 5: Prepare the mixed slurry
[0036] The waste paper is first screened, impurity-removed, and crushed for pretreatment. 12 parts of pretreated waste paper, 87 parts of deionized water, and 1 part of an additive are mixed by mass and soaked for 4 hours to obtain a mixture. After 4 hours, the mixture is dissociated and impurities are removed to obtain waste paper pulp. 90 parts of waste paper pulp, 6 parts of nanocellulose fiber organic pulp, and 1.5 parts of modified starch are mixed to obtain a mixed pulp.
[0037] Step 6: Prepare paper tube base paper with good tear resistance
[0038] 97.5 parts of mixed pulp, 1 part of JH1216 dry strength agent, 1.5 parts of EUM782 waterproofing agent and 875 parts of deionized water were mixed by weight, and the pulp was obtained after slag removal, degassing and screening; the pulp was sprayed onto the mesh surface for dehydration, and the base paper was obtained after forming, extrusion and drying. 3.25 parts of surface glue were evenly coated on 96.75 parts of the base paper, and dried at 95°C for 15 minutes to obtain a paper tube base paper with good tear resistance.
[0039] Embodiment 2: A paper tube base paper with good burst resistance, the preparation method is as follows:
[0040] Step 1: Preparation of modified starch
[0041] By mass, 1.15 parts of starch and 1.48 parts of deionized water were mixed and stirred to obtain starch latex. A 3% sodium hydroxide solution was added to the starch latex to adjust the pH to 10.0, 0.0132 parts of sodium trimetaphosphate were added, and the mixture was reacted at 45° C. and 30 rpm for 2 hours. The pH of the reaction system was adjusted to 8.0 with hydrochloric acid, acetic anhydride was added, and the reaction was continued at 45° C. and 30 rpm for 1.5 hours. The pH of the reaction system was neutralized to neutral with hydrochloric acid, and the mixture was dried to obtain modified starch.
[0042] Step 2: Preparation of modified nano-titanium dioxide
[0043] Mix 5 parts of nano-titanium dioxide and 218 parts of toluene, and ultrasonically disperse for 30 minutes to obtain a nano-titanium dioxide dispersion. Add 1.89 parts of KH-550 silane coupling agent and 0.4 parts of triethylamine to 223 parts of the nano-titanium dioxide dispersion, react at 95°C for 6 hours, filter, wash with ethanol, and vacuum dry to obtain modified nano-titanium dioxide.
[0044] Step 3: Preparation of Nanocellulose Organic Fiber Pulp
[0045] By mass, 1.5 parts of modified nano titanium dioxide and 18.5 parts of deionized water were fully mixed and ultrasonically dispersed for 15 minutes to obtain a modified nano titanium dioxide dispersion. 10 parts of bleached sulfate softwood pulp boards were crushed and mixed with 40 parts of deionized water. After being fully soaked for 4 hours, they were dispersed to obtain a coarse pulp. 50 parts of the coarse pulp and 30 parts of deionized water were mixed and pulped at a beating speed of 8000r to obtain fiber pulp. 80 parts of the fiber pulp were mixed with 20 parts of the modified nano titanium dioxide dispersion to obtain nanocellulose organic fiber pulp.
[0046] Step 4: Prepare the surface glue
[0047] By mass, at 90°C, 1 part of polyvinyl alcohol and 9 parts of deionized water were mixed and stirred to obtain a polyvinyl alcohol solution; 9 parts of polyvinyl alcohol solution and 1.2 parts of KH-550 silane coupling agent were mixed, and the pH of the reaction system was adjusted to 7.5 with 10% sodium hydroxide solution, and the reaction was carried out at 60°C and 200rpm for 2h to obtain a polyvinyl alcohol-coupling agent solution; the polyvinyl alcohol solution, the polyvinyl alcohol-coupling agent solution and propylene glycol were mixed in a mass ratio of 4.0:1.0:1.0, and stirred to obtain a surface glue solution.
[0048] Step 5: Prepare the mixed slurry
[0049] The waste paper is first pretreated by screening, impurity removal and pulverization. 12 parts of pretreated waste paper, 87 parts of deionized water and 1 part of an additive are mixed by mass and soaked for 4 hours to obtain a mixture. After 4 hours, the mixture is dissociated and impurities are removed to obtain waste paper pulp. 90 parts of waste paper pulp, 5.5 parts of nanocellulose fiber organic pulp and 1.5 parts of modified starch are mixed to obtain a mixed pulp.
[0050] Step 6: Prepare paper tube base paper with good tear resistance
[0051] 97 parts of mixed pulp, 1 part of JH1216 dry strength agent, 2 parts of EUM782 waterproofing agent and 875 parts of deionized water were mixed by weight, and the pulp was obtained after slag removal, degassing and screening; the pulp was sprayed onto the mesh surface for dehydration, and the base paper was obtained after forming, extrusion and drying. 3.25 parts of surface glue were evenly coated on 96.75 parts of the base paper, and dried at 95°C for 15 minutes to obtain a paper tube base paper with good tear resistance.
[0052] Embodiment 3: A paper tube base paper with good burst resistance, the preparation method is as follows:
[0053] Step 1: Preparation of modified starch
[0054] By mass, 1.15 parts of starch and 1.48 parts of deionized water were mixed and stirred to obtain starch latex. A 3% sodium hydroxide solution was added to the starch latex to adjust the pH to 10.0, 0.0132 parts of sodium trimetaphosphate were added, and the mixture was reacted at 45° C. and 30 rpm for 2 hours. The pH of the reaction system was adjusted to 8.0 with hydrochloric acid, acetic anhydride was added, and the reaction was continued at 45° C. and 30 rpm for 1.5 hours. The pH of the reaction system was neutralized to neutral with hydrochloric acid, and the mixture was dried to obtain modified starch.
[0055] Step 2: Preparation of modified nano-titanium dioxide
[0056] Mix 5 parts of nano-titanium dioxide and 218 parts of toluene, and ultrasonically disperse for 30 minutes to obtain a nano-titanium dioxide dispersion. Add 1.89 parts of KH-550 silane coupling agent and 0.4 parts of triethylamine to 223 parts of the nano-titanium dioxide dispersion, react at 95°C for 6 hours, filter, wash with ethanol, and vacuum dry to obtain modified nano-titanium dioxide.
[0057] Step 3: Preparation of Nanocellulose Organic Fiber Pulp
[0058] By mass, 1.5 parts of modified nano titanium dioxide and 18.5 parts of deionized water were fully mixed and ultrasonically dispersed for 15 minutes to obtain a modified nano titanium dioxide dispersion. 10 parts of bleached sulfate softwood pulp boards were crushed and mixed with 40 parts of deionized water. After being fully soaked for 4 hours, they were dispersed to obtain a coarse pulp. 50 parts of the coarse pulp and 30 parts of deionized water were mixed and pulped at a beating speed of 8000r to obtain fiber pulp. 80 parts of the fiber pulp were mixed with 20 parts of the modified nano titanium dioxide dispersion to obtain nanocellulose organic fiber pulp.
[0059] Step 4: Prepare the surface glue
[0060] By mass, at 90°C, 1 part of polyvinyl alcohol and 9 parts of deionized water were mixed and stirred to obtain a polyvinyl alcohol solution; 9 parts of polyvinyl alcohol solution and 1.2 parts of KH-550 silane coupling agent were mixed, and the pH of the reaction system was adjusted to 7.5 with 10% sodium hydroxide solution, and the reaction was carried out at 60°C and 200rpm for 2h to obtain a polyvinyl alcohol-coupling agent solution; the polyvinyl alcohol solution, the polyvinyl alcohol-coupling agent solution and propylene glycol were mixed in a mass ratio of 4.0:1.0:1.0, and stirred to obtain a surface glue solution.
[0061] Step 5: Prepare the mixed slurry
[0062] The waste paper is first screened, impurity-removed, and crushed for pretreatment. 12 parts of pretreated waste paper, 87 parts of deionized water, and 1 part of an additive are mixed by mass and soaked for 4 hours to obtain a mixture. After 4 hours, the mixture is dissociated and impurities are removed to obtain waste paper pulp. 90 parts of waste paper pulp, 5 parts of nanocellulose fiber organic pulp, and 1 part of modified starch are mixed to obtain a mixed pulp.
[0063] Step 6: Prepare paper tube base paper with good tear resistance
[0064] By mass, 96 parts of mixed pulp, 1.5 parts of JH1216 dry strength agent, 2.5 parts of EUM782 waterproofing agent and 875 parts of deionized water are mixed, and the pulp on the mesh is obtained after slag removal, degassing and screening; the pulp on the mesh is sprayed onto the mesh surface for dehydration, and the base paper is obtained after forming, extrusion and drying. 3.25 parts of surface glue are evenly coated on 96.75 parts of the base paper, and dried at 95°C for 15 minutes to obtain a paper tube base paper with good tear resistance.
[0065] Based on Example 1, control experiments were carried out, specifically Comparative Example 1, Comparative Example 2 and Comparative Example 3, as described below:
[0066] Comparative Example 1: No starch modification was performed, and other conditions were the same as those in Example 1.
[0067] A paper tube base paper with good tear resistance, the preparation method of which is as follows:
[0068] Step 1: Preparation of modified nano-titanium dioxide
[0069] Mix 5 parts of nano-titanium dioxide and 218 parts of toluene, and ultrasonically disperse for 30 minutes to obtain a nano-titanium dioxide dispersion. Add 1.89 parts of KH-550 silane coupling agent and 0.4 parts of triethylamine to 223 parts of the nano-titanium dioxide dispersion, react at 95°C for 6 hours, filter, wash with ethanol, and vacuum dry to obtain modified nano-titanium dioxide.
[0070] Step 3: Preparation of Nanocellulose Organic Fiber Pulp
[0071] By mass, 1.5 parts of modified nano titanium dioxide and 18.5 parts of deionized water were fully mixed and ultrasonically dispersed for 15 minutes to obtain a modified nano titanium dioxide dispersion. 10 parts of bleached sulfate softwood pulp boards were crushed and mixed with 40 parts of deionized water. After being fully soaked for 4 hours, they were dispersed to obtain a coarse pulp. 50 parts of the coarse pulp and 30 parts of deionized water were mixed and pulped at a beating speed of 8000r to obtain fiber pulp. 80 parts of the fiber pulp were mixed with 20 parts of the modified nano titanium dioxide dispersion to obtain nanocellulose organic fiber pulp.
[0072] Step 4: Prepare the surface glue
[0073] By mass, at 90°C, 1 part of polyvinyl alcohol and 9 parts of deionized water were mixed and stirred to obtain a polyvinyl alcohol solution; 9 parts of polyvinyl alcohol solution and 1.2 parts of KH-550 silane coupling agent were mixed, and the pH of the reaction system was adjusted to 7.5 with 10% sodium hydroxide solution, and the reaction was carried out at 60°C and 200rpm for 2h to obtain a polyvinyl alcohol-coupling agent solution; the polyvinyl alcohol solution, the polyvinyl alcohol-coupling agent solution and propylene glycol were mixed in a mass ratio of 4.0:1.0:1.0, and stirred to obtain a surface glue solution.
[0074] Step 5: Prepare the mixed slurry
[0075] The waste paper is first pre-treated by screening, impurity removal and pulverization. 12 parts of pre-treated waste paper, 87 parts of deionized water and 1 part of an additive are mixed by mass and soaked for 4 hours to obtain a mixture. After 4 hours, the mixture is dissociated and impurities are removed to obtain waste paper pulp. 90 parts of waste paper pulp, 6 parts of nanocellulose fiber organic pulp and 1.5 parts of starch are mixed to obtain a mixed pulp.
[0076] Step 6: Prepare paper tube base paper with good tear resistance
[0077] 97.5 parts of mixed pulp, 1 part of JH1216 dry strength agent, 1.5 parts of EUM782 waterproofing agent and 875 parts of deionized water were mixed by weight, and the pulp was obtained after slag removal, degassing and screening; the pulp was sprayed onto the mesh surface for dehydration, and the base paper was obtained after forming, extrusion and drying. 3.25 parts of surface glue were evenly coated on 96.75 parts of the base paper, and dried at 95°C for 15 minutes to obtain a paper tube base paper with good tear resistance.
[0078] Comparative Example 2: No modified nano titanium dioxide was added, and the other conditions were the same as those in Example 1.
[0079] A paper tube base paper with good tear resistance, the preparation method of which is as follows:
[0080] Step 1: Preparation of modified starch
[0081] By mass, 1.15 parts of starch and 1.48 parts of deionized water were mixed and stirred to obtain starch latex. A 3% sodium hydroxide solution was added to the starch latex to adjust the pH to 10.0, 0.0132 parts of sodium trimetaphosphate were added, and the mixture was reacted at 45° C. and 30 rpm for 2 hours. The pH of the reaction system was adjusted to 8.0 with hydrochloric acid, acetic anhydride was added, and the reaction was continued at 45° C. and 30 rpm for 1.5 hours. The pH of the reaction system was neutralized to neutral with hydrochloric acid, and the mixture was dried to obtain modified starch.
[0082] Step 3: Preparation of Nanocellulose Organic Fiber Pulp
[0083] By mass, 1.5 parts of modified nano titanium dioxide and 18.5 parts of deionized water were fully mixed and ultrasonically dispersed for 15 minutes to obtain a modified nano titanium dioxide dispersion. 10 parts of bleached sulfate softwood pulp boards were crushed and mixed with 40 parts of deionized water. After being fully soaked for 4 hours, they were dispersed to obtain a coarse pulp. 50 parts of the coarse pulp and 50 parts of deionized water were mixed and pulped at a beating speed of 8000r to obtain nanocellulose organic fiber pulp.
[0084] Step 4: Prepare the surface glue
[0085] By mass, at 90°C, 1 part of polyvinyl alcohol and 9 parts of deionized water were mixed and stirred to obtain a polyvinyl alcohol solution; 9 parts of polyvinyl alcohol solution and 1.2 parts of KH-550 silane coupling agent were mixed, and the pH of the reaction system was adjusted to 7.5 with 10% sodium hydroxide solution, and the reaction was carried out at 60°C and 200rpm for 2h to obtain a polyvinyl alcohol-coupling agent solution; the polyvinyl alcohol solution, the polyvinyl alcohol-coupling agent solution and propylene glycol were mixed in a mass ratio of 4.0:1.0:1.0, and stirred to obtain a surface glue solution.
[0086] Step 5: Prepare the mixed slurry
[0087] The waste paper is first screened, impurity-removed, and crushed for pretreatment. 12 parts of pretreated waste paper, 87 parts of deionized water, and 1 part of an additive are mixed by mass and soaked for 4 hours to obtain a mixture. After 4 hours, the mixture is dissociated and impurities are removed to obtain waste paper pulp. 90 parts of waste paper pulp, 6 parts of nanocellulose fiber organic pulp, and 1.5 parts of modified starch are mixed to obtain a mixed pulp.
[0088] Step 6: Prepare paper tube base paper with good tear resistance
[0089] 97.5 parts of mixed pulp, 1 part of JH1216 dry strength agent, 1.5 parts of EUM782 waterproofing agent and 875 parts of deionized water were mixed by weight, and the pulp was obtained after slag removal, degassing and screening; the pulp was sprayed onto the mesh surface for dehydration, and the base paper was obtained after forming, extrusion and drying. 3.25 parts of surface glue were evenly coated on 96.75 parts of the base paper, dried at 95°C for 15 minutes, and rewound into a roll to obtain a paper tube base paper with good tear resistance.
[0090] Comparative Example 3: No modification treatment was performed on the polyvinyl alcohol, and other conditions were the same as those in Example 1.
[0091] A paper tube base paper with good tear resistance, the preparation method of which is as follows:
[0092] Step 1: Preparation of modified starch
[0093] By mass, 1.15 parts of starch and 1.48 parts of deionized water were mixed and stirred to obtain starch latex. A 3% sodium hydroxide solution was added to the starch latex to adjust the pH to 10.0, 0.0132 parts of sodium trimetaphosphate were added, and the mixture was reacted at 45° C. and 30 rpm for 2 hours. The pH of the reaction system was adjusted to 8.0 with hydrochloric acid, acetic anhydride was added, and the reaction was continued at 45° C. and 30 rpm for 1.5 hours. The pH of the reaction system was neutralized to neutral with hydrochloric acid, and the mixture was dried to obtain modified starch.
[0094] Step 2: Preparation of modified nano-titanium dioxide
[0095] Mix 5 parts of nano-titanium dioxide and 218 parts of toluene, and ultrasonically disperse for 30 minutes to obtain a nano-titanium dioxide dispersion. Add 1.89 parts of KH-550 silane coupling agent and 0.4 parts of triethylamine to 223 parts of the nano-titanium dioxide dispersion, react at 95°C for 6 hours, filter, wash with ethanol, and vacuum dry to obtain modified nano-titanium dioxide.
[0096] Step 3: Preparation of Nanocellulose Organic Fiber Pulp
[0097] By mass, 1.5 parts of modified nano titanium dioxide and 18.5 parts of deionized water were fully mixed and ultrasonically dispersed for 15 minutes to obtain a modified nano titanium dioxide dispersion. 10 parts of bleached sulfate softwood pulp boards were crushed and mixed with 40 parts of deionized water. After being fully soaked for 4 hours, they were dispersed to obtain a coarse pulp. 50 parts of the coarse pulp and 30 parts of deionized water were mixed and pulped at a beating speed of 8000r to obtain fiber pulp. 80 parts of the fiber pulp were mixed with 20 parts of the modified nano titanium dioxide dispersion to obtain nanocellulose organic fiber pulp.
[0098] Step 4: Prepare the surface glue
[0099] By mass, 1 part of polyvinyl alcohol and 9 parts of deionized water were mixed at 90° C. and stirred evenly to obtain a polyvinyl alcohol solution. The polyvinyl alcohol solution and propylene glycol were mixed at a mass ratio of 4.0:1.0 and stirred evenly to obtain a surface glue solution.
[0100] Step 5: Prepare the mixed slurry
[0101] The waste paper is first screened, impurity-removed, and crushed for pretreatment. 12 parts of pretreated waste paper, 87 parts of deionized water, and 1 part of an additive are mixed by mass and soaked for 4 hours to obtain a mixture. After 4 hours, the mixture is dissociated and impurities are removed to obtain waste paper pulp. 90 parts of waste paper pulp, 6 parts of nanocellulose fiber organic pulp, and 1.5 parts of modified starch are mixed to obtain a mixed pulp.
[0102] 97.5 parts of mixed pulp, 1 part of JH1216 dry strength agent, 1.5 parts of EUM782 waterproofing agent and 875 parts of deionized water were mixed by weight, and the pulp was obtained after slag removal, degassing and screening; the pulp was sprayed onto the mesh surface for dehydration, and the base paper was obtained after forming, extrusion and drying. 3.25 parts of surface glue were evenly coated on 96.75 parts of the base paper, and dried at 95°C for 15 minutes to obtain a paper tube base paper with good tear resistance.
[0103] Detection experiment:
[0104] Paper tube base paper with good bursting resistance required for the test was prepared according to the preparation methods in Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, and Comparative Example 3 respectively.
[0105] Quantitative test: According to "Determination of Quantitative Weight of Paper and Paperboard" (GB / T 451.2-2002), use a special sample cutter to take horizontal samples on the paper tube base paper. The sample size is 100mm×100mm. Use a balance to measure the mass of each sample and calculate the quantitative weight of each sample.
[0106] Ring compression strength test: According to "Determination of Ring Compression Strength of Paper and Paperboard" (GB / T2679.8-1995), use a special sample cutter to take samples horizontally on the paper tube base paper. The sample size is 152.0mm×17.0mm. Use a fixed pressure plate type electronic compression instrument to fix the sample on the sample holder, start the instrument, and compress the sample until the sample is crushed. Calculate the ring compression strength index of the sample.
[0107] Burst resistance test: According to "Determination of Burst Resistance of Paper" (GB / T 454-2002), use a special cutter to take horizontal samples on the paper tube base paper. The sample size is 70mm×70mm. Place the sample on the elastic film and clamp the periphery of the sample. Pump in hydraulic fluid to make the film bulge until the sample breaks. Stop pumping, record the pressure at this time, and calculate the burst resistance of the sample.
[0108]
[0109] Conclusion: It can be seen from the experiment that the sample obtained by the preparation method of Example 1 is better than the samples obtained by the preparation methods of Comparative Example 1, Comparative Example 2 and Comparative Example 3 in the test. The paper tube base paper prepared in Example 1 is better than the paper tube base paper prepared in Comparative Example 1, Comparative Example 2 and Comparative Example 3 in terms of tear resistance and other aspects, effectively solving the problem of insufficient tear resistance of ordinary paper tube base paper.
[0110] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
Claims
1. A method for preparing a paper tube base paper with good burst resistance, characterized in that: The preparation method is: Waste paper pulp, nanocellulose organic pulp and modified starch are mixed and stirred evenly to obtain a mixed pulp; the mixed pulp, dry strength agent, waterproofing agent and deionized water are mixed, and then the pulp for mesh is obtained through slag removal, degassing and screening; the pulp for mesh is sprayed onto the mesh surface for dehydration; base paper is obtained through forming, extrusion and drying; surface glue is applied on the surface of the base paper, and the paper is dried and rewound to obtain a paper tube base paper with good tear resistance.
2. The method for preparing a paper tube base paper with good bursting resistance according to claim 1, characterized in that: Calculated by mass fraction, the raw materials of the paper tube base paper include 2.2-6.8% of nano-cellulose fiber organic pulp, 1.0-1.6% of modified starch, 1.0-1.6% of dry strength agent, 1.5-2.5% of waterproofing agent, 0.4-1.0% of auxiliary agent, and the rest is waste paper pulp.
3. The method for preparing a paper tube base paper with good bursting resistance according to claim 2, characterized in that: The preparation method of waste paper pulp is as follows: The waste paper is pre-treated by screening, impurity removal and pulverization. 10 to 14 parts of pre-treated waste paper, 85 to 89 parts of deionized water and 0.5 to 1.5 parts of an auxiliary agent are mixed by weight and soaked for 3 to 5 hours to obtain a mixture. The mixture is dissociated and impurities are removed to obtain waste paper pulp.
4. The method for preparing a paper tube base paper with good bursting resistance according to claim 3, characterized in that: Calculated by mass fraction, the additives include 38-42% sodium hydroxide, 6-10% sodium dodecyl sulfonate, 10-14% fatty alcohol polyoxyethylene ether, 13-17% methylene dithiocyanate, and 23-27% polyethylene oxide.
5. The method for preparing a paper tube base paper with good bursting resistance according to claim 2, characterized in that: The preparation method of nanocellulose fiber organic pulp is: The nano-titanium dioxide and toluene are mixed, and ultrasonically dispersed for 25 to 35 minutes to obtain a nano-titanium dioxide dispersion liquid. KH-550 and triethylamine are added to the nano-titanium dioxide dispersion liquid, and reacted at 90 to 100° C. for 5 to 7 hours. The mixture is filtered, washed with ethanol, and vacuum dried to obtain modified nano-titanium dioxide. The modified nano titanium dioxide and deionized water are fully mixed and ultrasonically dispersed for 10 to 20 minutes to obtain a modified nano titanium dioxide dispersion. The bleached sulfate softwood pulp board is crushed, mixed with deionized water, and fully soaked for 3 to 5 hours to obtain a coarse pulp. The coarse pulp and deionized water are mixed and pulped at a beating speed of 7500 to 8500 rpm to obtain a fiber pulp. The fiber pulp is mixed with the modified nano titanium dioxide dispersion to obtain a nanocellulose organic fiber pulp.
6. The method for preparing a paper tube base paper with good bursting resistance according to claim 2, characterized in that: The preparation method of modified starch is: Starch and deionized water are mixed and stirred to obtain starch latex, 3% sodium hydroxide solution is added to the starch latex to adjust the pH to 9.5-10.5, sodium trimetaphosphate is added, and the reaction is carried out at 40-50° C. and 20-40 rpm for 1-3 hours, and then the pH of the reaction system is adjusted to 7.5-8.5 with hydrochloric acid, acetic anhydride is added, and the reaction is continued at 40-50° C. and 20-40 rpm for 1-2 hours, and the reaction system is neutralized with hydrochloric acid and dried to obtain modified starch.
7. The method for preparing a paper tube base paper with good bursting resistance according to claim 2, characterized in that: The preparation method of the surface glue is as follows: At 85-95°C, polyvinyl alcohol and deionized water are mixed and stirred to obtain a polyvinyl alcohol solution. The polyvinyl alcohol solution and KH-550 are mixed, and the pH value of the reaction system is adjusted to 7-8 with sodium hydroxide solution. The reaction is carried out at 55-65°C and 150-250rpm for 1-3h to obtain a polyvinyl alcohol-coupling agent solution. The polyvinyl alcohol solution, the polyvinyl alcohol-coupling agent solution and propylene glycol are mixed and stirred to obtain a surface adhesive solution.
8. The method for preparing a paper tube base paper with good bursting resistance according to claim 7, characterized in that: The mass ratio of polyvinyl alcohol solution, polyvinyl alcohol-coupling agent solution and propylene glycol is (3.8-4.2):(0.8-1.2):(0.8-1.2).
Citation Information
Patent Citations
Method for producing corrugated paper and textile spool paper by manioc slag and wine stillage slag
CN101413225A
Method for preparing nanometer hydrophobic paper by utilizing corrugated paper / nanometer titanium dioxide
CN103388273A
Environment-friendly type starch-based modified starch used for wallpaper glue and preparation method thereof
CN106256836A
Environment-friendly high-barrier paper bag and application thereof
CN118241502A
Bobbin base paper and bobbin base paper manufacturing method
CN118241504A
Cited By
Tensile wear-resistant washable kraft paper and preparation process thereof
CN119531188A