Load transmission efficiency measuring method for biaxial cross tensile sample
By measuring and calculating the thickness change of the specimen and combining it with material parameters, the problem of accuracy in evaluating the load transfer efficiency of the cruciform specimen is solved, providing a fast and direct evaluation method that overcomes the shortcomings of simulation evaluation.
Patent Information
- Application Number
- CN202410872898.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-22
AI Technical Summary
In the existing technology, the evaluation of load transfer efficiency of cross specimens mainly relies on simulation methods, lacking direct measurement means, which leads to insufficient accuracy and reliability of the evaluation results.
A method for calculating the load transfer efficiency of a cruciform specimen based on thickness variation is proposed. The load transfer efficiency is calculated by measuring the initial width and thickness of the test area and the thickness change at the center point after applying the load, combined with material parameters, and evaluated using a formula.
This method enables rapid and direct measurement of the load transfer efficiency of cruciform specimens, overcoming the limitations of simulation evaluation and improving the accuracy and reliability of the evaluation.
Smart Images

Figure CN119000263A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of testing technology and tests or analyzes materials by means of measuring the physical properties of the materials. Specifically, it relates to a method for measuring the load transfer efficiency of a biaxial cross tensile specimen. Background Art
[0002] During actual use, materials will be subjected to various forms of loads, and tensile load is one of the common forms of loads. Therefore, it is very important to study the performance and performance changes of materials when subjected to tensile loads. A uniaxial tensile test device has been proposed to apply a tensile load in one direction to the material. However, the load applied by the uniaxial tensile test device is in a single direction and cannot well restore the actual load on the material. For this reason, a biaxial tensile test device has been proposed, which applies tensile loads to the material in two directions perpendicular to each other to better restore the actual load on the material.
[0003] Patent document 1 (authorization announcement number: CN218121601U; patentee: National University of Defense Technology of the People's Liberation Army of China; classification number: G01N3 / 08, utility model name: a biaxially stretched solid propellant sample and a molding device thereof) proposes a biaxially stretched solid propellant sample and a molding device thereof, wherein the biaxially stretched solid propellant sample is a cross-shaped structure, and the molding device includes a base plate, a cover plate, a connecting piece and a mold, wherein the base plate is arranged on the lower side of the sample model, the cover plate is arranged on the upper side of the sample model, and the base plate and the cover plate are connected by a connecting piece; the mold is arranged between the base plate and the cover plate, and a mold groove and a mold casting groove are arranged on the mold, wherein the model groove is a "cross"-shaped groove that penetrates the mold, and the mold casting groove is interconnected with the model groove, and is used in conjunction with the base plate casting groove arranged on the base plate.
[0004] Patent document 2 (application publication number: CN113405910A; applicant: Rocket Force Engineering University of the Chinese People's Liberation Army; classification number: G01N3 / 10, invention name: A biaxial tensile mechanical properties testing device and method for a multi-configuration test piece) proposes a biaxial tensile mechanical properties testing device and method for a multi-configuration test piece, which relates to the technical field of mechanical properties testing of materials under complex stress loading. The testing device includes an upper clamp and a lower clamp connected to a testing machine and arranged correspondingly up and down. The upper clamp includes an upper clamp body in an orthogonal cross configuration. The four extending arms of the upper clamp body are upper support arms. The center lines of the four upper support arms are located in the same plane. An upper clamping portion for connecting to the testing machine is fixedly arranged at the center of the upper clamp body, and the upper clamping portion extends in a direction away from the lower clamp.
[0005] Patent document 3 (application publication number: CN110658078A; applicant: PLA Rocket Force Engineering University; classification number: G01N3 / 14, invention name: biaxial load adjustable tensile creep test device and method) proposes a biaxial load adjustable tensile creep test device and method. The test device includes a support frame, a base is provided at the bottom of the support frame, a support assembly is provided on the support frame, a tensile assembly is connected to the support assembly, and the tensile assembly is connected to the measuring assembly to test the specimen.
[0006] For cross-type biaxial tensile specimens, the load from the orthogonal direction is transferred to the center along the tensile arm and forms a plane stress state in the central area. However, during the transfer process, the load will be affected by the shape of the tensile arm, the cross section, and the stress concentration at the fillet, resulting in different degrees of loss. Therefore, the load transfer efficiency is one of the important indicators for evaluating the rationality of the tensile specimen.
[0007] At present, the load transfer efficiency of the cross specimen is mostly defined based on the ratio of the resultant force between the clamping end and the stretching end. However, in actual experiments, in the test devices including the above three patent documents, the resultant force on the cross section of the central area of the cross specimen cannot be measured, so the force-based load transfer efficiency evaluation method is mostly obtained through simulation. For example, Zhou Huasen and Yang Xiaoxiang proposed a finite element analysis method in "Design and Finite Element Analysis of Rubber Isobiaxial Tensile Cross Specimens" (published in "Rubber Industry" Vol. 65, 2018). However, simulation itself has certain limitations, and other methods need to be proposed to evaluate the load transfer efficiency. Summary of the invention
[0008] Based on the inventor's research and practical experience in this field, the following improved technical solution is proposed here.
[0009] In view of this, the present invention proposes a method for calculating the load transfer efficiency of a cross specimen based on thickness variation. This is a calculation method that can be used for a variety of cross configurations, and it evaluates and calculates the load transfer efficiency of a specific configuration through observable thickness variation.
[0010] Specifically, the present invention provides a method for measuring the load transfer efficiency of a biaxial cross tensile specimen, the method comprising:
[0011] Measuring the initial width of the test area of the sample and the initial thickness at the center point of the sample;
[0012] Apply load to the cross-shaped specimen;
[0013] After stretching, measure the thickness at the center point;
[0014] The load transfer efficiency is calculated based on the initial width, the initial thickness, the applied load, the thickness at the center point after the stretching is completed, and the material parameters of the specimen.
[0015] According to one aspect of the present invention, the load transfer efficiency is calculated by the following formula:
[0016]
[0017] Where, β is the load transfer efficiency, which is equal to the ratio of the load at the clamping end to the load on the axis of symmetry of the specimen, E is the elastic modulus of the specimen, h0 is the initial thickness of the center of the test area, a is the initial width of the test area, F is the load applied to the tensile end of the specimen, v is the Poisson's ratio of the specimen, h is the thickness of the specimen at the center after the test, and the coefficient of variation of the center thickness is
[0018] According to one aspect of the present invention, the sample is a solid propellant.
[0019] It can be seen from the above that the present invention provides a method for measuring the load transfer efficiency of a cross specimen based on biaxial tension, which can quickly obtain the load transfer efficiency by calculation after the test, thus overcoming the limitation of the prior art that efficiency evaluation can only be performed through simulation. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Exemplary embodiments of the present invention are described with reference to the accompanying drawings, in which:
[0021] Figure 1 A schematic diagram of a specimen used in a method for measuring load transfer efficiency of a biaxial cross tensile specimen of the present invention is shown.
[0022] Figure 2 A schematic diagram showing the observation of a load transfer efficiency measurement method for a biaxial cross tensile specimen of the present invention.
[0023] Figure 3 The schematic diagram of the structure of different cross-shaped specimens used in a method for measuring load transfer efficiency of a biaxial cross tensile specimen of the present invention is shown.
[0024] Figure 4 A schematic diagram comparing the load transfer efficiency obtained by a load transfer efficiency measurement method for a biaxial cross tensile specimen of the present invention and the load transfer efficiency obtained by simulation calculation is shown. DETAILED DESCRIPTION
[0025] The specific implementation of the present invention is described below with reference to the accompanying drawings.
[0026] Figure 1A schematic diagram of a specimen used in a method for measuring the load transfer efficiency of a biaxial cross-tensile specimen of the present invention is shown. Specifically, the cross-tensile specimen is generally in the shape of a "cross", and its four arms are connected to a biaxial tensile mechanism so as to withstand a tensile load F. The tensile arms of the cross configuration are usually distributed perpendicular to each other at intervals of 90°, and intersect at the center to form a test area. The load is transmitted from the clamping end along the tensile arm to the center, so a more complex biaxial stress state can be studied by setting different loading ratios. It should be noted that the load will be affected by factors such as shape, cross-section and stress concentration during the transmission process, resulting in unnecessary losses, so it is necessary to evaluate the transmission efficiency of the specimen. Figure 1 The direction of the tensile load F is shown by an arrow. Figure 1 The test area located at the center of the cross tensile specimen is also shown. Specifically, considering that the cross-shaped specimens have different structures, the present invention defines the "test area" as follows:
[0027] (1) For a cross specimen that has been thinned in the center, the thinned area is defined as the test area. Generally speaking, the thinning process is to set a square area in the center with a thickness smaller than that of other parts of the specimen, and the length of the area is a.
[0028] (2) For cross specimens that have not been thinned in the center, the test area is defined as a circular area with the center of the cross specimen as the center and a diameter of 0.6 times the arm width of the cross specimen.
[0029] Figure 2 The schematic diagram of the load transfer efficiency measurement method for a biaxial cross tensile specimen of the present invention is shown. The biaxial tensile device used in the present invention can be any device known in the prior art, as long as it can apply the required load to the cross specimen. Figure 2 A three-dimensional digital image correlation (3D-DIC) measuring device is also shown, which can be used to observe the thickness data of the test area. Of course, other methods can also be used to measure the required thickness data.
[0030] The applicant has found through research that for a cross-shaped specimen, its load transfer efficiency can be calculated by the following formula:
[0031]
[0032] In the above formula, β is the load transfer efficiency, which is equal to the ratio of the load at the clamping end to the load on the axisymmetric line of the specimen, E is the elastic modulus of the specimen, h0 is the initial thickness at the center of the test area, a is the initial width of the test area, F is the load applied at the tensile end of the specimen, and v is the Poisson's ratio of the specimen.
[0033] In addition, the coefficient of variation of the center thickness of the specimen is defined where h is the thickness at the center of the specimen after the test.
[0034] Therefore, the present invention proposes the following measurement method:
[0035] Measure the initial width of the test area and the initial thickness at the center of the specimen;
[0036] Apply load to the cross-shaped specimen;
[0037] After stretching, measure the thickness at the center point.
[0038] Therefore, the various parameters required by the above formula can be obtained through the above method, so that the load transfer efficiency β can be calculated.
[0039] Figure 3 The schematic diagram of the structure of different cross-shaped specimens used in a method for measuring load transfer efficiency of a biaxial cross tensile specimen of the present invention is shown. Figure 4 The figure shows a comparison diagram of the load transfer efficiency obtained by a load transfer efficiency measurement method for a biaxial cross tensile specimen of the present invention and the load transfer efficiency obtained by simulation calculation. Figure 3 The various types of cross-shaped specimens shown in the figure were subjected to biaxial tensile tests, and the load transfer efficiency was obtained by the method proposed by the present invention and the simulation. The results obtained by the two methods are compared. Figure 4 shown.
[0040] Specifically, No. 1 is based on slits and square thinning configuration; No. 2 is based on slits, arms and second-order circular thinning configuration; No. 3 is based on comprehensive circular thinning and slits on arms; No. 4 is designed as a non-slit comparison configuration of sample 3; No. 5 is based on large fillet radius and circular thinning configuration; No. 6 is based on large fillet radius and short arm configuration; No. 7 is based on fillet concave design configuration; No. 8 is a cross configuration with grooves in the arm. The material parameters of samples 1 to 8 are elastic modulus of 1MPa and Poisson's ratio of 0.495. The simulation loading conditions are that each tensile end is stretched at a constant speed of 20mm / min for 15s. The thickness of the test area of the sample is uniformly 5mm, and the initial thickness of the thinning samples is 20mm.
[0041] By testing the above-mentioned cross-shaped specimens in different forms respectively, and using the method of the present invention and simulation to obtain the load transfer efficiency respectively, it is found through comparison that the results of the method proposed by the present invention and the simulation are basically consistent in size.
[0042] It can be seen that the present invention provides a method for measuring the load transfer efficiency of a cross specimen based on biaxial tension, which can overcome the limitation of the prior art that efficiency evaluation can only be performed through simulation.
[0043] The above-mentioned biaxial tensile test device can be used for testing viscoelastic materials, especially for testing solid propellants. The charge structure of solid propellants is subjected to a complex stress state during ignition and pressure buildup, and the interior of the middle section is approximately in a biaxial tensile stress state. The method of the present invention can quickly determine the load transfer efficiency.
[0044] The above description is merely an exemplary embodiment of the spirit and principle of the present invention. It will be appreciated by those skilled in the art that various changes may be made to the described examples without departing from the spirit and principle, and these changes and their various equivalents are all anticipated by the inventors and fall within the scope defined by the claims of the present invention.
Claims
1. A method for measuring the load transfer efficiency of a biaxial cross tensile specimen, characterized in that: The method comprises: Measuring the initial width of the test area of the sample and the initial thickness at the center point of the sample; Apply load to the cross-shaped specimen; After stretching, measure the thickness at the center point; The load transfer efficiency is calculated based on the initial width, the initial thickness, the applied load, the thickness at the center point after the stretching is completed, and the material parameters of the specimen.
2. The method for measuring load transfer efficiency of a biaxial cross tensile specimen according to claim 1, characterized in that: The load transfer efficiency is calculated by the following formula: Where, β is the load transfer efficiency, which is equal to the ratio of the load at the clamping end to the load on the axis of symmetry of the specimen, E is the elastic modulus of the specimen, h0 is the initial thickness of the center of the test area, a is the initial width of the test area, F is the load applied to the tensile end of the specimen, v is the Poisson's ratio of the specimen, h is the thickness of the specimen at the center after the test, and the coefficient of variation of the center thickness is 3. The method for measuring the load transfer efficiency of a biaxial cross tensile specimen according to claim 1 or 2, characterized in that: The sample is a solid propellant.
Citation Information
Cited By
Experimental equipment for variable-proportion biaxial stretching of material
CN119394797A