Manufacturing method of standard map for testing quality of wrought aluminum alloy cast ingot through fluorescent penetrant
Through fluorescence penetration inspection methods and standardized treatment, a domestic quality grade evaluation standard map of deformed aluminum alloy ingots was formulated, which solved the problem of lack of evaluation standards in my country, and ensured the safety of aircraft materials and the localization process.
Patent Information
- Application Number
- CN202411141537.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-22
AI Technical Summary
my country lacks a comparison map of the quality grade evaluation standard for deformed aluminum alloy ingots, which leads to the inability to effectively detect and evaluate the internal quality of the ingots, affecting the safety of aircraft and defense manufacturing products.
By selecting samples that meet foreign standards, etching, fluorescence penetration test and imaging treatment, the best detection parameters and shooting conditions are determined, and the quality evaluation of domestic fluorescence penetration tests and deformed aluminum alloy ingots is formulated. Standard map.
It successfully breaks the foreign technology blockade, provides domestic fluorescence penetration inspection quality level evaluation standards, ensures the safety and domestic production of aircraft materials, and improves the quality control method of deformed aluminum alloy raw materials.
Smart Images

Figure CN119000706A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nondestructive testing, and in particular relates to a method for preparing a standard spectrum for fluorescent penetrant testing of quality of deformed aluminum alloy ingots. Background Art
[0002] Porosity, pores and microcracks in deformed aluminum alloy ingots are discontinuity defects, which are the main factors affecting the final quality of deformed aluminum alloy processed products. The existence of these defects will endanger the application safety of aircraft and defense manufacturing products, and may even cause immeasurable and significant economic losses. The organization of deformed aluminum alloy ingots used to manufacture aircraft and defense products is not allowed to have these discontinuity defects.
[0003] Domestically, low-magnification inspection methods are usually used to detect these micron-level defects, which can be found in low-magnification inspections. However, aluminum processing manufacturing industries with different needs have different quality control requirements for the size, dispersion, and density of ingot loose defects. Foreign aircraft manufacturers use fluorescent penetrant inspection methods to evaluate the quality level of deformed aluminum alloy ingot samples and monitor the internal quality of the ingots.
[0004] The basic principle of the fluorescent penetrant testing method is to apply a penetrant containing fluorescent dyes on the surface of the sample to be inspected. Under the action of capillaries, after a certain period of time, the penetrant penetrates into the surface opening defects, removes the excess penetrant on the working surface, and after drying, applies an adsorbent developer to the surface of the workpiece. Also under the action of capillaries, the developer will absorb the penetrant in the defects and make the penetrant seep back onto the sample inspection surface. When there are micron-sized discontinuous defects such as tiny needles and microcracks on the sample surface, under a certain black light source, yellow-green fluorescent penetrant display traces can be observed at the defects, thereby detecting the morphology and distribution of the defects. The fluorescent penetrant testing method is to inspect surface opening defects. The smaller and deeper the opening, the higher the sensitivity of the inspection of tiny defects, especially micron-sized microcracks and tiny discontinuity defects, which are incomparable to other non-destructive testing methods. Fluorescent penetrant testing can detect micron-level defects, and its detection capability is two orders of magnitude higher than that of low-power inspection methods. Since the technology related to the fluorescent penetrant inspection method for deformed aluminum alloy ingots has long been protected by foreign patents and technical blockades, my country is currently still in a blank stage for the fluorescent penetrant inspection method for deformed aluminum alloy ingots, and therefore there are no relevant inspection standards and grade assessment comparison charts. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a standard atlas for fluorescent penetrant testing of the quality of deformed aluminum alloy ingots, so as to effectively solve the problem that my country lacks a standard comparison atlas for quality grade assessment of fluorescent penetrant testing of deformed aluminum alloy ingots.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0007] A method for preparing a standard spectrum for fluorescent penetrant testing of the quality of deformed aluminum alloy ingots comprises the following steps: S1, sample selection and processing.
[0008] According to the characteristics of the ingot casting process and the distribution law of pores and crack defects, samples are selected from the homogenized deformed aluminum alloy ingots. The surface of the sample is smooth and continuous, and the surface roughness is better than 0.32μm. The surface of the sample is etched and washed, and the inspection surface of the sample is kept clean without any pollution and damage.
[0009] S2. Determine the best detection process.
[0010] Fluorescence penetrant inspection was carried out on the samples with different inspection parameter settings. The test results were compared with the foreign standard atlas for quality grade assessment of fluorescent penetrant inspection of deformed aluminum alloy ingot samples to determine the optimal parameters for fluorescent penetrant inspection.
[0011] Samples with no porosity and samples with different pore sizes and densities were selected for fluorescent penetrant inspection tests. The displays of the test samples obtained were compared with the foreign standard atlas for quality grade assessment of fluorescent penetrant inspection of deformed aluminum alloy ingot samples to evaluate the quality grade of each sample.
[0012] S3. Determine the best time and method to take photos of fluorescent penetrant inspection displays.
[0013] The fluorescent penetrant imaging time of the samples was tested with different imaging time settings to determine the best display timing, and pictures were taken. According to the quality of the pictures, the comparison chart of the domestic quality grade assessment standard of fluorescent penetrant inspection of deformed aluminum alloy ingots was determined.
[0014] Further, in step S1, the method for sample selection includes: S11, selecting samples that conform to the grade I to grade VII chart of the foreign deformed aluminum alloy ingot sample fluorescent penetrant inspection quality grade assessment standard chart from homogenized aluminum alloy ingots of different alloys and different specifications.
[0015] S12. The samples cut from the deformed aluminum alloy ingot must represent the manufacturing structure of the ingot. The ingot is cut off at the head and tail before deformation. The length of the head is ≥425mm, and the length of the tail is ≥625mm. After the head and tail of the ingot are cut off to the specified length, samples with a thickness of 25mm±5mm are cut transversely at both ends of the head and tail, and marked.
[0016] Further, in step S1, the process flow of etching is: A1, alkali washing: the liquid used for washing is 12g / L-150g / L sodium hydroxide and 12g / L-25g / L sodium sulfide, the washing time is 2-5min, and the washing temperature is 40±5℃.
[0017] A2. Water washing: The liquid used for washing is water. Immerse the sample in water and stir. The washing time is 5-8 minutes and the washing temperature is room temperature.
[0018] A3. Pickling: The liquid used for washing is 190g / L-380g / L nitric acid, the washing time is 2-5min, and the washing temperature is room temperature.
[0019] A4. Water washing: The liquid used for washing is deionized water, the washing time is 5-8 minutes, and the washing temperature is room temperature.
[0020] A5. Place the sample washed with water in step A4 at room temperature and evaporate to dryness naturally.
[0021] Further, in step S2, the inspection conditions of the fluorescent penetrant inspection test are: the inspection temperature is 20±5°C, the penetrant complies with the provisions of GB / T18851.2 "Non-destructive testing penetrant testing Part 2: Inspection of penetrants", and the working test block selected for penetrant inspection sensitivity is a type B five-point test block, which complies with GB / T23911 "Test blocks for non-destructive testing penetrant testing". Before the sample is tested, the penetrant and the test process used are calibrated on the type B five-point test block, and star-shaped cracks of no less than 3 points are clearly observed on the test block.
[0022] Further, in step S2, the steps of the fluorescent penetrant inspection test include: S21, applying a penetrant.
[0023] Apply a water-washable penetrant to the test surface of the sample by dipping, so that the penetrant evenly covers the test surface of the sample. The penetration time is not less than 10 minutes, and the sample is immersed in the penetrant for no more than 1 / 2 of the penetration time.
[0024] S22. Removal of penetrant.
[0025] First immersion washing and then spray washing, the cleaning process is carried out under the irradiation of a black light lamp, the wavelength range of the black light lamp is 320-400nm, and the peak wavelength of the black light lamp is 365±5nm.
[0026] Use a water nozzle with a rotary spray function, control the water temperature at 10-38℃, the water pressure less than 0.275MPa, the spray time is 1-3min, and the water distance is not less than 300mm; or use manual spraying to make the water column fan-shaped or cone-shaped to remove excess penetrant from the test surface of the sample.
[0027] When the ambient white light illuminance is less than 20lx, the black light irradiance shall not be less than 50μW / cm 2 ; When the ambient white light illumination is 20-100lx, the black light irradiance is not less than 100μW / cm 2 .
[0028] S23. Drying.
[0029] The samples are dried in a drying oven or by blowing with compressed air. When drying in a drying oven, the drying temperature shall not exceed 71°C, the drying time shall not exceed 20 minutes, and the drying oven shall be equipped with a hot air circulation system, a temperature controller and a temperature display. When drying with compressed air, the drying temperature shall be room temperature, the air pressure of the compressed air shall not exceed 0.172MPa, and the distance between the compressed air outlet and the sample surface shall not be less than 300mm.
[0030] S24, imaging.
[0031] Use explosive powder electrostatic spraying or pneumatic spraying to evenly apply a layer of dry powder developer on the test surface of the sample. The residence time of the dry powder developer shall not be less than 10 minutes and not more than 1 hour.
[0032] Excess dry powder developer on the test surface of the sample shall be blown away using clean and dry compressed air before observation and evaluation of the sample. The pressure of the compressed air shall not exceed 0.034MPa.
[0033] Furthermore, in step S23, before the sample is dried, compressed air is used to remove moisture from the sample surface, and the compressed air is clean, dry, oil-free, water-free, and solid particle-free.
[0034] Further, in step S3, the sample to be photographed is placed in a fixture, and four black light lamps are fixed on the fixture. The four black light lamps are arranged at 90° intervals in the circumferential direction, and the distance and angle between the black light lamps and the surface of the sample to be photographed are adjustable. The background of the fixture does not produce any reflection or luminescence, the shooting environment is clean, and there is no fluorescence interference display when observed under the black light lamp.
[0035] The camera lens beam is perpendicular to the central area of the sample to be photographed, the black beam is inclined at about 45° to the surface of the sample to be photographed, the focal points of the four black beams coincide, and the four black beam areas cover the sample to be photographed.
[0036] Compared with the prior art, the beneficial technical effects of the present invention are: (1) The present invention successfully produces a comparison chart of quality grade assessment standards for fluorescent penetrant inspection of domestic deformed aluminum alloy ingot samples, which is of great significance for breaking the foreign technology blockade, ensuring the safe operation of aircraft, the safe use of domestic large aircraft materials, and improving the quality control inspection method of deformed aluminum alloy raw materials.
[0037] (2) The present invention provides a sample fluorescent penetrant inspection process for the best grade assessment map and an optimal shooting method and shooting conditions for the standard quality grade assessment map of the fluorescent penetrant inspection of deformed aluminum alloy ingots, which is of great significance for formulating the fluorescent penetrant inspection method and acceptance grade of deformed aluminum alloy ingot samples. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 It is a standard atlas for evaluating the quality grade of fluorescent penetrant inspection of deformed aluminum alloy ingot samples for a foreign aviation industry.
[0039] Figure 2 It is a comparison chart of quality grade evaluation standards for domestic deformed aluminum alloy ingot fluorescent penetrant inspection produced by the present invention.
[0040] Figure 3 This is a micrograph of the 01st sample of CXXX9 melt number in Example 1.
[0041] Figure 4 This is the fluorescent penetration test result diagram of the 01st sample of CXXX9 melt number in Example 1.
[0042] Figure 5 This is a micrograph of the ingot sample with melting point BGXX710 in Example 3.
[0043] Figure 6 This is the fluorescent penetration test result diagram of the ingot sample with melting number BGXX710 in Example 3.
[0044] Figure 7 This is a fluorescence penetration test result diagram of the 3104 alloy square ingot sample in Example 4.
[0045] Figure 8 This is a micrograph of the 3104 alloy square ingot sample in Example 4.
[0046] Fig. 9 This is a diagram showing the fluorescent penetration test results of the 5A06 alloy square ingot sample in Example 5. DETAILED DESCRIPTION
[0047] A method for preparing a standard spectrum for fluorescent penetrant testing of quality of deformed aluminum alloy ingots comprises the following steps.
[0048] S1. Sample selection and processing.
[0049] According to the characteristics of the ingot casting process and the distribution law of pores and crack defects, the sample is selected from the homogenized deformed aluminum alloy ingot. The surface of the sample is smooth and continuous, and the surface roughness is better than 0.32μm. The surface of the sample is etched and washed, and the inspection surface of the sample is kept clean without any pollution and damage; and the sample should be prevented from being over-etched and under-etched. Over-etching will cause false display of the sample fluorescence detection result and enlargement of the display of small defects, which cannot truly reflect the organization of the ingot itself; under-etching will make it difficult to detect small defects.
[0050] In step S1, the method for sample selection includes: (1) selecting samples that conform to the grade I to grade VII spectrum of the foreign deformed aluminum alloy ingot sample fluorescent penetrant inspection quality grade assessment standard spectrum from homogenized aluminum alloy ingots of different alloys and different specifications.
[0051] Grade I samples should be selected from samples with good quality inside the ingot. Grade I samples have uniform grain structure and no tiny discontinuity defects. Grade II to Grade VII samples should be selected from ingots with unsatisfactory degassing effects.
[0052] (2) The sample cut from the deformed aluminum alloy ingot must represent the manufacturing structure of the ingot. During the casting process of the ingot, the head and tail of the ingot are more loose, so the ingot is cut off at the head and tail before deformation. The length of the head cut is ≥425mm, and the length of the tail cut is ≥625mm. After the head and tail of the ingot are cut off to the specified length, the samples with a thickness of 25mm±5mm are cut horizontally at both ends of the head and tail, and marked. The sampling position is determined according to the processing technology of the deformed aluminum alloy ingot and the production and processing rules of the ingot alloy that is prone to looseness and oxide film defects.
[0053] In step S1, the process flow of etching the surface of the sample is as follows: (1) alkali washing: the liquid used for washing is 12g / L-150g / L sodium hydroxide and 12g / L-25g / L sodium sulfide, the washing time is 2-5min, and the washing temperature is 40±5°C; (2) water washing: the liquid used for washing is water, the sample is immersed in water and stirred, the washing time is 5-8min, and the washing temperature is room temperature (the room temperature in this embodiment is about 20°C); (3) acid washing: the liquid used for washing is 190g / L-380g / L nitric acid, the washing time is 2-5min, and the washing temperature is room temperature; (4) water washing: the liquid used for washing is deionized water, the washing time is 5-8min, and the washing temperature is room temperature; (5) the washed sample is placed at room temperature for natural evaporation and drying.
[0054] S2. Determine the best detection process.
[0055] Fluorescence penetrant testing was performed on the samples using different test parameter settings, and the test results were compared with a foreign standard for quality grade assessment of fluorescence penetrant testing of deformed aluminum alloy ingot samples for aviation (e.g. Figure 1 A comparative analysis was conducted to determine the optimal parameters for fluorescent penetration testing.
[0056] From a large number of samples, samples with no porosity and samples with different pore sizes and densities were selected for fluorescent penetrant testing. The obtained test sample displays were compared with a foreign aviation deformed aluminum alloy ingot sample fluorescent penetrant testing quality grade evaluation standard atlas (such as Figure 1 The quality level of each sample was evaluated by comparison.
[0057] In step S2, the test conditions of the fluorescent penetrant test are as follows: (1) The test temperature is preferably 20±5°C. (2) The penetrant should comply with the provisions of GB / T18851.2 "Non-destructive testing penetrant testing Part 2: Penetrant testing". (3) The working test block selected for penetrant test sensitivity determination is a type B five-point test block, which complies with GB / T23911 "Test block for non-destructive testing penetrant testing". Before the sample is tested, the penetrant and the test process used are calibrated on the type B five-point test block, and no less than 3 star-shaped cracks should be clearly observed on the test block.
[0058] In step S2, the steps of the fluorescent penetrant inspection test include: (1) application of penetrant: applying a water-washable penetrant on the inspection surface of the sample by dipping, so that the penetrant is evenly covered on the inspection surface of the sample, and the penetration time is not less than 10 minutes to ensure that the penetrant can well enter the surface opening of the tiny discontinuity defect. The time the sample is immersed in the penetrant is not more than 1 / 2 of the penetration time.
[0059] (2) Removal of penetrant: First immerse and then spray to avoid blind spots in cleaning. The cleaning process should be carried out under the irradiation of a black light. The wavelength range of the black light is 320-400nm. Since the spectral intensity of the black light is more concentrated at a wavelength of 365nm, the peak wavelength of the black light is required to be 365±5nm. Under the premise of ensuring that the sample surface does not produce an excessively high fluorescent background, the water washing time should be limited to a minimum to prevent the sample from being over-cleaned. The degree of cleaning should be such that the penetrant is basically removed and a slight amount of the original color of the penetrant is used as the observation background. After cleaning, use a black light to check the cleaning effect of the sample. If it is found that the sample has an excessively high fluorescent background or is over-cleaned, the sample needs to be cleaned and the penetrant needs to be re-applied.
[0060] When spraying, use a water nozzle with a rotary spray function, the water temperature is controlled at 10-38℃, the water pressure is less than 0.275MPa, the spray time is 1-3min, and the water distance is not less than 300mm. You can also use manual spraying to make the water column fan-shaped or cone-shaped to remove excess penetrant from the test surface of the sample.
[0061] When the ambient white light illuminance is less than 20lx, the black light irradiance shall not be less than 50μW / cm 2 ; When the ambient white light illumination is 20-100lx, the black light irradiance is not less than 100μW / cm 2 .
[0062] (3) Drying: The sample needs to be dried before development, because the dry powder developer uses capillary phenomenon to infiltrate the penetrant in the defect back to the sample surface. If the sample is not dry, the development will fail after the dry powder developer is applied due to moisture or water in the sample, and the conditions for the capillary phenomenon to occur will be lost.
[0063] Before drying the sample, use compressed air to remove moisture from the sample surface. The compressed air should be clean, dry, oil-free, water-free and free of solid particles. When drying, use a drying oven or compressed air to dry the sample. When using a drying oven for drying, the drying temperature shall not exceed 71°C, and the drying time shall not exceed 20 minutes. The drying oven shall be equipped with a hot air circulation system, a temperature controller and a temperature display; when using compressed air for drying, the drying temperature shall be room temperature, the air pressure of the compressed air shall not exceed 0.172MPa, and the distance between the compressed air outlet and the sample surface shall not be less than 300mm.
[0064] (4) Imaging: Use explosive powder electrostatic spraying or pneumatic spraying to evenly apply a layer of dry powder developer on the test surface of the sample. The residence time of the dry powder developer should be no less than 10 minutes and no more than 1 hour. The residence time of the dry powder developer directly affects the display results. If the time is too short, it will not be continuous and cannot be completely exuded, resulting in missed inspections; if the time is too long, it will cause display distortion and fail to intuitively display the morphology and size of the defects.
[0065] In order to provide better observation conditions, the excess dry powder developer on the test surface of the sample should be blown away with clean and dry compressed air before the sample is observed and evaluated. The pressure of the compressed air should not exceed 0.034MPa. There should be no other external non-related displays on the sample.
[0066] S3. Determine the best time and method to take photos of fluorescent penetrant inspection displays.
[0067] The fluorescent penetrant imaging time of the sample was tested with different imaging time settings to determine the best display time and capture pictures. According to the quality of the pictures taken, the domestic deformed aluminum alloy ingot fluorescent penetrant inspection quality grade evaluation standard comparison chart was determined to fill the domestic gap.
[0068] In step S3, the following points should be noted: (1) When observing the sample to be photographed, the discontinuity display to be detected should be clearly distinguished from the sample background display, and the sample with too high fluorescent background should be reprocessed. There are many factors that produce fluorescent display under black light, so all fluorescence-related displays and non-related displays on the sample should be evaluated and interpreted. The sample used for shooting the inspection quality grade evaluation standard comparison map should not have any non-related display.
[0069] (2) Place the sample under a black light and observe and identify all fluorescence-related displays. In order to obtain the best fluorescence penetrant inspection rating quality grade evaluation standard comparison chart, only one sample is tested at a time. The sample inspection results are compared with the Figure 1 The standard charts of a foreign aviation industry are compared and graded. The best display pictures are selected as the preliminary candidates.
[0070] (3) The sample selected for the fluorescent penetrant inspection quality grade assessment standard comparison chart should not have any other false display. The sample to be photographed is placed in a fixture, on which four black light lamps are fixed. The four black light lamps are located in a circumferential position and are distributed adjacent to each other at 90 degrees. The distance and angle between the black light lamp and the surface of the sample to be photographed are adjustable. The background of the fixture does not produce any reflection or luminescence, the shooting environment is clean, and there is no fluorescence interference display when observed under the black light.
[0071] (4) The camera lens beam is perpendicular to the center area of the sample to be photographed, the black light beam is inclined at about 45° to the surface of the sample to be photographed, the focal points of the four black light beams coincide, and the four black light beam areas cover the sample to be photographed. The camera, black light, and sample to be photographed should be placed in a fixed position.
[0072] (5) For the sample with fluorescent penetrant display, you should not stop and take a snapshot immediately. The display on the photo should not have any other false display except the required tiny discontinuity defect display.
[0073] (6) The optimal inspection process parameters of the comparison chart of the quality grade evaluation standard of the fluorescent penetrant inspection of deformed aluminum alloy ingots were determined by conducting a large number of inspection tests. The fluorescent penetrant inspection standard quality grade samples were selected from a large number of fluorescent penetrant inspection samples. The selected preliminary candidate chart was compared with the Figure 1The comparison of the quality grade evaluation standard graphs of fluorescent penetrant inspection of a foreign aviation deformed aluminum alloy ingot sample is shown in the figure, and a set of optimal inspection quality grade evaluation standard comparison graphs is determined as the domestic deformation aluminum alloy ingot fluorescent penetrant inspection quality grade evaluation standard comparison graphs, such as Figure 2 shown.
[0074] The standard comparison map prepared by the present invention is to show the discontinuity defect level evaluation of the casting structure of the ingot sample from no micropores, a few micropores, dispersed micropores, relatively dense micropores, dense micropores, high-density pores, etc. The pores refer to the pores and looseness in the ingot. The microscopic characteristics of the looseness are irregular black holes distributed on the dendrites of the ingot, mostly at the junction of three dendrites; while the microscopic characteristics of the pores are black circular holes with smooth inner walls, which are irregularly distributed in the solid solution of the ingot.
[0075] The foreign deformed aluminum alloy ingot sample fluorescence penetration test quality grade evaluation standard comparison atlas is not officially obtained, so the obtained physical effect is not ideal and cannot be used as a standard comparison atlas. Therefore, the present invention breaks the foreign technology blockade, ensures the safe operation of aircraft, the safe use of localized large aircraft materials, improves the quality control inspection method of deformed aluminum alloy raw materials, and successfully produces the domestic deformed aluminum alloy ingot sample fluorescence penetration test quality grade evaluation standard comparison atlas, which is of great significance for formulating the deformed aluminum alloy ingot sample fluorescence penetration inspection method and acceptance grade.
[0076] The present invention will be further described in detail below with reference to the embodiments and drawings.
[0077] Example 1: Using the method of the present invention, samples of 11 round ingots of 7075 alloy with a diameter of 600 mm were taken for fluorescent penetrant testing. Figure 2 The test grade was evaluated by comparing the domestic quality grade evaluation standard comparison chart of the fluorescent penetrant inspection of deformed aluminum alloy ingots, and the results are shown in Table 1. The grade II sample (see Figure 4 ) on the defect display position to take a high-magnification sample for high-magnification microstructure analysis, the analysis results are loose defects (such as Figure 3 shown).
[0078] Table 1 Fluorescence penetrant test results of 7075 alloy round ingot samples with a diameter of 600 mm
[0079]
[0080] Example 2: Using the method of the present invention, samples were taken from 6 square ingots of 7050 alloy for fluorescent penetrant testing. Figure 2The domestic deformed aluminum alloy ingot fluorescent penetrant inspection quality grade assessment standard comparison chart was compared to evaluate the inspection grade. The results are shown in Table 2.
[0081] Table 2 Fluorescence penetrant test results of 7050 alloy square ingot samples
[0082] Serial number Melting number Test results Specifications (mm) 1 BGXX020 Level I 590*1260*7050 2 BGXX732 Level I 438*1530*5780 4 BGXX930 Level I 436*1530*5670 5 BHXX230 Level I 404*1480*3350 6 BHXX810 Level I 455*1545*3615
[0083] Example 3: Using the method of the present invention, samples of four square ingots of 2024 alloy were taken for fluorescent penetrant testing. Figure 2 The test grade was evaluated by comparing the domestic deformation aluminum alloy ingot fluorescent penetrant inspection quality grade evaluation standard comparison chart, and the results are shown in Table 3. The grade II sample (see Figure 6 ) on the defect display position to take a high-magnification sample for high-magnification microstructure analysis, the analysis results are loose defects (such as Figure 5 shown).
[0084] Table 3 Fluorescence penetrant test results of 2024 alloy square ingot samples
[0085] Serial number Melting number Test results Specifications (mm) 1 BGXX020 Level I 480*1560*5050 2 BGXX530 Level I 522*2090*4300 3 BGXX122 Level I 428*1530*4902 4 BGXX710 Level II 403*1810*3400
[0086] Example 4: Using the method of the present invention, a sample of a square ingot of 3104 alloy was taken for fluorescent penetrant testing, and the results of the fluorescent test were compared with the results of the fluorescent test. Figure 2 The domestic deformation aluminum alloy ingot fluorescent penetrant inspection quality grade evaluation standard comparison chart was compared to evaluate the inspection grade, and the evaluation result was grade VII (see Figure 7 ). Take a high-magnification sample from the defect position on the sample for high-magnification microstructure analysis, and the analysis result is a loose defect (see Figure 8 ).
[0087] Example 5: A sample of a square ingot of 5A06 alloy was taken for fluorescent penetrant testing using the method of the present invention. Figure 2 The domestic deformation aluminum alloy ingot fluorescent penetrant inspection quality grade evaluation standard comparison chart was compared to evaluate the inspection grade, and the evaluation result was grade VII (see Fig. 9 ).
[0088] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. A method for preparing a standard spectrum for fluorescent penetrant testing of the quality of deformed aluminum alloy ingots, characterized in that: The following steps are involved: S1. Sample selection and processing; According to the characteristics of the ingot casting process and the distribution law of pores and crack defects, the sample is selected from the homogenized deformed aluminum alloy ingot. The surface of the sample is smooth and continuous, and the surface roughness is better than 0.32μm. The surface of the sample is etched and washed, and the inspection surface of the sample is kept clean without any pollution and damage. S2. Determine the best detection process; The fluorescent penetrant test was carried out on the samples with different test parameter settings, and the test results were compared and analyzed with the foreign standard atlas for quality grade assessment of fluorescent penetrant test of deformed aluminum alloy ingot samples to determine the optimal parameters for fluorescent penetrant test. Select samples with no porosity and samples with different pore sizes and densities for fluorescent penetrant testing. Compare the obtained test sample displays with the foreign standard chart for quality grade assessment of fluorescent penetrant testing of deformed aluminum alloy ingot samples to evaluate the quality grade of each sample. S3. Determine the best time and method to take photos of the fluorescent penetrant inspection display; The fluorescent penetrant imaging time of the samples was tested with different imaging time settings to determine the best display timing, and pictures were taken. According to the quality of the pictures, the comparison chart of the domestic quality grade assessment standard of fluorescent penetrant inspection of deformed aluminum alloy ingots was determined.
2. The method for preparing a standard atlas for fluorescent penetrant testing of quality of deformed aluminum alloy ingots according to claim 1, characterized in that: In step S1, the method for selecting a sample includes: S11, selecting a sample that meets the grade I to grade VII chart of the foreign deformed aluminum alloy ingot sample fluorescent penetrant inspection quality grade assessment standard chart from the homogenized aluminum alloy ingots of different alloys and different specifications; S12. The samples cut from the deformed aluminum alloy ingot must represent the manufacturing structure of the ingot. The ingot is cut off at the head and tail before deformation. The length of the head is ≥425mm, and the length of the tail is ≥625mm. After the head and tail of the ingot are cut off to the specified length, samples with a thickness of 25mm±5mm are cut transversely at both ends of the head and tail, and marked.
3. The method for preparing a standard atlas for fluorescent penetrant testing of quality of deformed aluminum alloy ingots according to claim 2, characterized in that: In step S1, the process flow of etching is: A1. Alkali washing: The liquid used for washing is 12g / L-150g / L sodium hydroxide and 12g / L-25g / L sodium sulfide, the washing time is 2-5min, and the washing temperature is 40±5℃; A2. Water washing: The liquid used for washing is water. Immerse the sample in water and stir. The washing time is 5-8 minutes and the washing temperature is room temperature. A3, pickling: the liquid used for washing is 190g / L-380g / L nitric acid, the washing time is 2-5min, and the washing temperature is room temperature; A4. Water washing: The liquid used for washing is deionized water, the washing time is 5-8 minutes, and the washing temperature is room temperature; A5. Place the sample washed with water in step A4 at room temperature and evaporate to dryness naturally.
4. The method for preparing a standard atlas for fluorescent penetrant testing of quality of deformed aluminum alloy ingots according to claim 3, characterized in that: In step S2, the inspection conditions of the fluorescent penetrant inspection test are as follows: the inspection temperature is 20±5°C, the penetrant complies with the provisions of GB / T18851.2 "Nondestructive Testing Penetrant Testing Part 2: Inspection of Penetrants", and the working test block selected for penetrant inspection sensitivity is a type B five-point test block, which complies with GB / T23911 "Test Blocks for Nondestructive Testing Penetrant Testing". Before the sample is tested, the penetrant and the test process used are calibrated on the type B five-point test block, and star-shaped cracks of no less than 3 points are clearly observed on the test block.
5. The method for preparing a standard atlas for fluorescent penetrant testing of quality of deformed aluminum alloy ingots according to claim 4, characterized in that: In step S2, the steps of the fluorescent penetrant inspection test include: S21, application of penetrant; Apply a water-washable penetrant to the test surface of the sample by dipping, so that the penetrant covers the test surface of the sample evenly. The penetration time is not less than 10 minutes, and the time the sample is immersed in the penetrant is not more than 1 / 2 of the penetration time. S22, removal of penetrant; First immersion washing followed by spray washing, the cleaning process is carried out under the irradiation of a black light lamp, the wavelength range of the black light lamp is 320-400nm, and the peak wavelength of the black light lamp is 365±5nm; Use a water nozzle with a rotary spray function, with the water temperature controlled at 10-38℃, the water pressure less than 0.275MPa, the spray time of 1-3min, and the water distance of not less than 300mm; or use manual spraying to make the water column fan-shaped or cone-shaped to remove excess penetrant from the test surface of the sample; When the ambient white light illuminance is less than 20lx, the black light irradiance shall not be less than 50μW / cm 2 ; When the ambient white light illumination is 20-100lx, the black light irradiance is not less than 100μW / cm 2 ; S23, drying; The sample is dried by drying in a drying oven or by blowing with compressed air. When drying in a drying oven, the drying temperature shall not exceed 71°C, the drying time shall not exceed 20 minutes, and the drying oven shall be equipped with a hot air circulation system, a temperature controller and a temperature display. When drying with compressed air, the drying temperature shall be room temperature, the air pressure of the compressed air shall not exceed 0.172MPa, and the distance between the compressed air outlet and the sample surface shall not be less than 300mm. S24, imaging; Use explosive powder electrostatic spraying or pneumatic spraying to evenly apply a layer of dry powder developer on the test surface of the sample. The residence time of the dry powder developer shall not be less than 10 minutes and not more than 1 hour; Excess dry powder developer on the test surface of the sample shall be blown away using clean and dry compressed air before observation and evaluation of the sample. The pressure of the compressed air shall not exceed 0.034MPa.
6. The method for preparing a standard atlas for fluorescent penetrant testing of quality of deformed aluminum alloy ingots according to claim 5, characterized in that: In step S23, before the sample is dried, compressed air is used to remove moisture from the sample surface, and the compressed air must be clean, dry, oil-free, water-free, and free of solid particles.
7. The method for preparing a standard atlas for fluorescent penetrant testing of quality of deformed aluminum alloy ingots according to claim 6, characterized in that: In step S3, the sample to be photographed is placed in a fixture, and four black light lamps are fixed on the fixture. The four black light lamps are located in a circumferential position and are distributed adjacent to each other at 90 degrees. There is no reflection or luminescence phenomenon in the background of the fixture. The shooting environment is clean, and there is no fluorescence interference display when observed under the black light lamp; The camera lens beam is perpendicular to the central area of the sample to be photographed, the black beam is inclined at about 45° to the surface of the sample to be photographed, the focal points of the four black beams coincide, and the four black beam areas cover the sample to be photographed.