Method for performing failure positioning on back surface of discrete semiconductor device
By performing hot spot positioning on the back of the semiconductor discrete device, combined with infrared microscope and chemical acid corrosion technology, the problems of damage to the front of the chip and damage to the silicon wafer in the existing technology are solved, and the failure position of the semiconductor device is achieved quickly and accurately. Ensures the reliability and stability of the analysis.
Patent Information
- Application Number
- CN202411072071.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-22
AI Technical Summary
Existing hot spot positioning methods usually require the opening of the front of the semiconductor device, resulting in the damage of the chip plastic sealing material, affecting the leakage channel, and mechanical abrasion may damage the silicon wafer, making it difficult to accurately locate the failure position, especially after the HTRB or HAST test. When the leakage channel disappears.
Hot spot positioning is performed through the back of the semiconductor discrete device, and infrared microscope system combined with chemical acid corrosion technology is used to remove metal plates and solder on the back, retain the plastic sealing material on the front of the chip, and use the penetration of the infrared microscope to identify the front structure of the chip and accurately position it Failure position to avoid wear and tear.
The plastic sealing material on the front of the chip was successfully retained, avoiding the change of leakage channels, ensuring the integrity of the silicon wafer, and being able to quickly and accurately locate the failure position, which is convenient for subsequent analysis. The method is highly stable and the leakage current changes are controllable.
Smart Images

Figure CN119001387A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semiconductor device failure analysis methods, and in particular to a method for locating failures from the back side of a discrete semiconductor device. Background Art
[0002] Semiconductor device failures have always been a hot topic in the industry. Failure analysis is usually performed by locating the failure point of abnormal chips (electrical / reliability test abnormalities), and the chip failure mechanism is determined in combination with the chip design. Failure location can locate the physical location of the failure problem without destroying the sample or partially destroying the sample by using relevant analysis methods.
[0003] The three commonly used methods for semiconductor failure analysis and defect location are EMMI, THERMAL, and OBIRCH. All of them involve hotspot location. The principle of hotspot location is based on the following: when the laser acts on the semiconductor material, two effects will be generated, one is the thermal effect (thermal radiation), and the other is the photogenerated carrier effect (photon radiation). If the energy of the laser wavelength is less than the semiconductor energy band, the semiconductor will only have a thermal effect; when it is greater than or close to the semiconductor energy band, heat and photogenerated carriers will be generated, and the carriers will play a dominant role. Both photon radiation and thermal radiation can cause changes in semiconductor resistance or generate current.
[0004] OBIRCH (Optical Beam Induced Resistance Change) is the most effective positioning method in advanced processes. By scanning the surface of the voltage-applied chip with a highly focused laser, the short circuit / leakage fault point can be found. The laser scanning method has two laser bands of 1340nm and 1064nm, which can be applied to the front and back analysis of silicon wafers and III-V devices.
[0005] EMMI is the optical emission microscope leakage detection and positioning hot spot analysis: photons may be emitted at the fault or non-fault location. These photon streams are collected and amplified by optical gain, and then converted by CCD photoelectric conversion and image processing to obtain a luminescence image. The luminescence image and the optical emission image on the surface of the device are superimposed to locate the failure point and defect. The wavelength of light radiation generated by defects such as ohmic short circuit, metal interconnect short circuit, surface inversion layer and diffusion resistance is not in the visible light range or the signal is too weak, which is generally not suitable for positioning using EMMI.
[0006] Thermal means using an infrared microscope system (Thermal Emission microscopy system), for example, using a highly sensitive InSb detector to detect when the IC is powered on, and locating the fault point (hot spot) by receiving the abnormal thermal radiation generated by the fault point.
[0007] For plastic-encapsulated devices, most existing hotspot location methods first remove the plastic encapsulation material on the chip surface, connect the probe to the front of the chip, and then use the thermal positioning equipment to detect the failure point. However, for some failure causes of discrete devices, such as the need to locate the failure point due to excessive leakage after HTRB or HAST testing, if the front is opened, the leakage may change due to the dissection process, such as worse leakage current or disappearance of leakage channel, which will make failure analysis more difficult.
[0008] Therefore, it is necessary to invent a method for performing hot spot analysis from the back side to ensure that the plastic packaging material on the front side of the chip is not damaged. Summary of the invention
[0009] In order to solve the above technical problems, a method for locating failures from the back of a discrete semiconductor device is provided. The method of the present invention can completely retain the plastic packaging material on the front of the chip and ensure the integrity of the silicon wafer, while not changing the leakage path of the failed sample itself, and avoiding the grinding damage to the chip in the prior art; the present invention utilizes the penetration of the infrared microscope system to identify the front structure of the chip from the back of the device; the method of the present invention can quickly and accurately locate the failure position, which is convenient for subsequent failure analysis.
[0010] In order to achieve the above objectives, the present invention is implemented through the following technical solutions:
[0011] A method for locating failures from the back side of a discrete semiconductor device comprises the following steps:
[0012] S1. Provide a packaged semiconductor discrete device that needs to be subjected to failure analysis, and completely seal and cure the pins of the semiconductor discrete device. After sealing and curing, the pins can be protected from corrosion in the next step, thereby forming a first intermediate sample;
[0013] S2, removing the metal plate, solder and chip back gold on the back of the first intermediate sample to obtain a second intermediate sample;
[0014] S3, removing the sample sealing solidified material outside the pins of the second intermediate sample, thereby completely exposing the pins to obtain a failed sample; the operation of exposing the pins is to facilitate the probe in subsequent testing to detect the device through the exposed pins;
[0015] S4. Hot spot positioning: After the thermal positioning equipment is powered on, the hot spot is positioned from the back of the failed sample. The hot spot position is positioned by receiving the abnormal thermal radiation generated by the fault point. The hot spot position is the failure position (also called defect position, fault position).
[0016] Furthermore, the semiconductor discrete device is selected from one of an IGBT discrete device, a MOSFET discrete device, and a FRED discrete device.
[0017] Further, in S1, a transparent epoxy resin is used to seal and cure the exposed pins, and the size of the seal and cure can completely cover the pin size of the semiconductor discrete device. Preferably, the size of the seal and cure is: 4-5 cm in length, 1.5-2.5 cm in width, and 0.5-1.5 cm in thickness. The typical size of the seal and cure is 4.5 cm in length×2 cm×1 cm in thickness.
[0018] The epoxy resin is selected from epoxy cold mounting resin, such as TROJAN TJ2221 (AB glue), etc. This resin has the characteristics of low viscosity and fast curing, and can complete the mounting process without heating, so it is named "cold mounting".
[0019] Furthermore, in S2, nitric acid and / or aqua regia are used to perform acid decay on the first intermediate sample; when the nitric acid is used alone for acid decay, the mass fraction thereof is 65%-68%.
[0020] Preferably, in S2, the first intermediate sample is first soaked in nitric acid for 50-80 minutes to corrode and remove the metal plate on the back of the sample, and then the first intermediate sample is taken out and soaked in aqua regia for 20-40 minutes to continue to corrode the solder remaining on the back and the back gold of the chip. Usually, the metal plate is a copper plate and the solder is solder.
[0021] Further, in S3, a degumming solvent is used to dissolve the sample seal solid until the pins are completely exposed, and the degumming solvent is selected from one or more of benzene, toluene, xylene, acetone, tetrahydrofuran, methanol, ethanol, dimethylformamide, and dimethylacetamide, and heating or room temperature treatment is performed during degumming;
[0022] Alternatively, in S3, the sealant of the pin is removed by mechanical grinding and polishing until the pin is completely exposed.
[0023] Furthermore, the thermal positioning device is an infrared microscope system with three probes. During testing, the positive probe is contacted with the back collector of the device, and the other two probes are used as negative electrodes to contact the gate pin and emitter pin of the device respectively. The test voltage setting needs to be less than the rated voltage of the device, and the upper limit of the leakage current is set to 1mA.
[0024] Beneficial technical effects:
[0025] The present invention retains the plastic packaging material on the front side of the chip for the failed sample when performing hotspot location analysis, and has little impact on the leakage channel of the failed sample itself; this is because the present invention uses chemical acid corrosion to ensure the integrity of the silicon wafer and avoid chip grinding damage; the nitric acid and / or aqua regia used in the present invention will not have any effect on the silicon wafer; conventional treatments such as mechanical grinding remove the copper base plate and solder by grinding the back surface, but if there is a tilt during the mechanical grinding process, the silicon wafer may be damaged, and further analysis will not be possible; the present invention uses chemical acid corrosion to remove the material on the back and ensure the integrity of the silicon wafer; the back side processing and the penetration of the infrared microscope system from the back side of the device can identify the front side structure of the device chip, and the failure position can be accurately located. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 A flow chart of a method for locating failures from the back side of a discrete semiconductor device according to the present invention;
[0027] Figure 2 The actual operation process of the first three steps of the method for locating failures from the back of a discrete semiconductor device in Example 1 and the corresponding product physical pictures;
[0028] Figure 3 A probe connection diagram in method S4 of locating failure from the back side of a discrete semiconductor device in Example 1;
[0029] Figure 4 A hot spot location map obtained by locating failures from the back side of a discrete semiconductor device according to Example 1;
[0030] Figure 5 This is a hot spot analysis result diagram after processing using Comparative Example 1. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention are within the scope of protection of the present invention.
[0032] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.
[0033] In addition, it should be noted that the use of terms such as "first" and "second" to limit intermediate samples is only to facilitate the distinction between the intermediate samples produced in each step. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.
[0034] The experimental methods in the following examples without specifying specific conditions are usually measured in accordance with national standards; if there is no corresponding national standard, the method is carried out in accordance with the general standard requirements or general methods.
[0035] The aqua regia used below is a mixture of concentrated nitric acid and concentrated hydrochloric acid in a volume ratio of 1:3, wherein the mass fraction of the concentrated nitric acid is 65%-68%, and the mass fraction of the concentrated hydrochloric acid is 36%-38%.
[0036] Example 1
[0037] The method for locating failures from the back of discrete semiconductor devices is shown in the flowchart below: Figure 1 As shown, the following steps are included:
[0038] S1. Provide a packaged, failed IGBT discrete device (75A 650V model MM75G3T65B), and use epoxy cold mounting resin to completely seal and cure the pins of the IGBT discrete device to form a first intermediate sample;
[0039] The process of completely sealing and curing the pins of the IGBT discrete device is as follows: the epoxy cold embedding resin: TROJAN TJ2221A (A glue) and TJ2221B (B glue) are mixed and stirred in proportion (the mass ratio of A glue to B glue is 2:1) until the two colloids are completely dissolved in each other to form a mixed glue, and then the mixed glue is poured into a mold (mold size: 4.5cm×2cm×1cm), and then the pins of the IGBT discrete device are inserted into the mold containing the mixed glue for sealing and curing (curing at room temperature for 5h) to form the first intermediate sample. It should be noted that only the pins need to be sealed and cured, and the copper plate on the back of the sample should not be sealed;
[0040] This step is mainly to protect the pins from being corroded by acid in the next step, to avoid affecting the subsequent hotspot positioning test, and also to facilitate the next step of corroding only the back copper plate;
[0041] S2, removing the metal plate, solder and chip back gold on the back of the first intermediate sample to obtain a second intermediate sample;
[0042] The removal process is as follows: the first intermediate sample is immersed in about 50 mL of nitric acid (mass fraction 65%-68%) (immersion time is about 1 hour), and the copper plate on the back of the first intermediate sample is completely corroded, and then the first intermediate sample is taken out and immersed in about 50 mL of aqua regia again, and the residual solder and chip back gold on the back of the sample are further corroded (immersion time is about 30 minutes), so as to form a second intermediate sample;
[0043] S3, removing the sample sealing solidified material outside the pins of the second intermediate sample, thereby completely exposing the pins to obtain a failed sample, wherein the operation of exposing the pins is to facilitate the subsequent detection of the device by a probe through the exposed pins;
[0044] Method for removing the sample sealing solidified material: using a degumming solvent, the degumming solvent is selected from one or more of benzene, toluene, xylene, acetone, tetrahydrofuran, methanol, ethanol, dimethylformamide, dimethylacetamide, heating or room temperature treatment during degumming, for the places that are not cleanly removed by the degumming solvent, grinding and polishing, using pliers and other tools to remove manually; or directly using grinding and polishing, pliers and other tools to remove the epoxy resin of the clean pin; the process does not matter, the purpose is to cleanly remove the sample sealing solidified material at the pin and completely expose the pin to form a failed sample that can be used for back detection;
[0045] The actual operation process of each of the above three steps and the corresponding product pictures are as follows Figure 2 As shown;
[0046] S4. Hot spot positioning: Thermal positioning equipment - After the infrared microscope system is powered on, the hot spot is positioned from the back of the failed sample. The infrared microscope system has three probes. During the test, the positive probe is in contact with the collector C on the back of the device, and the other two probes are in contact with the gate G pin and the emitter E pin of the device as the negative poles. The actual picture of the probe connection is as follows: Figure 3 As shown in the figure, the test voltage is set to be less than the rated voltage of the device, the upper limit of the leakage current is set to 1mA, and the hot spot is located by receiving the abnormal thermal radiation generated by the fault point. The hot spot is the failure position, defect position or fault position. The result is as follows Figure 4 As shown by Figure 4 It can be seen that the structure of the front side of the device chip can be identified from the back side of the device using the penetration of the infrared microscope system. The circled position in the figure is the located hotspot position (the hotspot position is the failure position or defect position or fault position), and the failure position can be accurately located.
[0047] Comparative Example 1
[0048] The method for locating failures on the back side of discrete semiconductor devices in this case is the same as that in Example 1, except that the removal process in S2 is as follows: the first intermediate sample is immersed in about 50 mL of nitric acid (mass fraction 65%-68%) as a whole without subsequent aqua regia treatment.
[0049] The hot spot analysis results of this case are as follows: Figure 5 As shown, the chip structure is blocked by residual solder or chip back gold, which affects the hot spot identification. Therefore, the solution of Example 1 can better accurately locate the failure position.
[0050] Example 2
[0051] Ten normal IGBT discrete devices were processed using the method of Example 1 to obtain a plurality of samples to be tested.
[0052] Comparative Example 2
[0053] The conventional front processing method - laser unsealing method was used to process ten normal IGBT discrete devices to obtain the samples to be tested:
[0054] ①First, laser open the epoxy resin on the surface of the discrete device to remove part of the plastic sealing material on the surface.
[0055] Until the bonding aluminum wire is exposed, a square groove will be etched on the surface of the device;
[0056] ② Prepare a mixed acid solution with sulfuric acid (98% by mass) and fuming nitric acid (98% by mass) in a ratio of 1:3;
[0057] ③ Place the semi-opened discrete device on a heating plate, set the temperature to 100°C, and use a dropper to drop the prepared mixed acid solution into the square groove of the device;
[0058] ④ When the solution begins to corrode and produce a lot of black foam, rinse it with acetone solution;
[0059] ⑤ Repeat operations ③ and ④ for multiple times until all the surface plastic packaging materials are removed, exposing the front chip structure, obtaining a failed sample, and locating its hot spots.
[0060] Note: Since the failure conditions of each failed IGBT discrete device are different, it is impossible to make a horizontal comparison, let alone a vertical comparison of the method. Therefore, both Example 2 and Comparative Example 2 use normal, non-failed IGBT discrete devices of the same model to verify the test stability of the method (each method processes ten).
[0061] The samples to be tested obtained after processing in Example 2 and Comparative Example 2 were numbered and the collector cut-off current I CES The test results (refer to GB / T 29332-2012) are shown in Table 1.
[0062] Table 1 Leakage changes of normal samples before and after opening
[0063]
[0064]
[0065] (Note: Amplitude = (After preparation I CES -Preparation I CES ) / Preparation I CES )
[0066] As can be seen from Table 1, when the back side is opened in the manner of Example 1, the leakage current changes slightly, and the increase can be controlled within 1 to 20; while when the front side is opened in the manner of Comparative Example 2, the leakage current changes very unstably, with an increase ranging from 1 to 9500, and the probability of an increase exceeding 20 is more than 70%. It can be seen that the back side treatment of the present invention has little effect on the leakage channel of the sample, and the method of the present invention has good reliability and stability. The back side treatment and the penetration of the infrared microscope system from the back side of the device can identify the front side structure of the device chip, and the failure position can be accurately located.
[0067] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. Method for locating failures from the back of discrete semiconductor devices. It is characterized in that The steps include: S1. providing a packaged semiconductor discrete device that needs to be subjected to failure analysis, and completely sealing and curing the pins of the semiconductor discrete device to form a first intermediate sample; S2, removing the metal plate, solder and chip back gold on the back of the first intermediate sample to obtain a second intermediate sample; S3, removing the sample sealing solidified material outside the pins of the second intermediate sample, thereby completely exposing the pins, and obtaining a failed sample; S4. Hot spot location: After the thermal positioning device is powered on, the hot spot is located from the back of the failed sample. The hot spot position is located by receiving the abnormal thermal radiation generated by the fault point. The hot spot position is the failure position.
2. The method for locating failures from the back side of a discrete semiconductor device according to claim 1, It is characterized in that The semiconductor discrete device is selected from one of an IGBT discrete device, a MOSFET discrete device, and a FRED discrete device.
3. The method for locating failures from the back side of a discrete semiconductor device according to claim 1, It is characterized in that In S1, a transparent epoxy resin is used to seal and cure the exposed pins, and the size of the sealed and cured sample can completely cover the size of the pins of the semiconductor discrete device; the epoxy resin is selected from epoxy cold embedding resin.
4. The method for locating failures from the back side of a discrete semiconductor device according to claim 1, It is characterized in that In S2, nitric acid and / or aqua regia are used to perform acid decay on the first intermediate sample.
5. The method for locating failures from the back side of a discrete semiconductor device according to claim 4, It is characterized in that In S2, the first intermediate sample is first immersed in nitric acid for 50-80 minutes to corrode and remove the metal plate on the back of the sample, and then the first intermediate sample is taken out and immersed in aqua regia for 20-40 minutes to continue to corrode the residual solder on the back and the back gold of the chip.
6. The method for locating failures from the back side of a discrete semiconductor device according to claim 1, It is characterized in that In S3, a degumming solvent is used to dissolve the sample seal solid until the pins are completely exposed; the degumming solvent is selected from one or more of benzene, toluene, xylene, acetone, tetrahydrofuran, methanol, ethanol, dimethylformamide, and dimethylacetamide, and the degumming is performed by heating or at room temperature; Alternatively, in S3, the sealant of the pin is removed by mechanical grinding and polishing until the pin is completely exposed.
7. The method for locating failures from the back side of a discrete semiconductor device according to claim 1, It is characterized in that The thermal positioning device is an infrared microscope system with three probes. During testing, the positive probe is contacted with the back collector of the device, and the other two probes are used as negative electrodes to contact the gate pin and emitter pin of the device respectively. The test voltage setting needs to be less than the rated voltage of the device, and the upper limit of the leakage current is set to 1mA.