Mixed micro / nano structure matrix array surface and preparation and test method thereof

By designing a mixed micro/nanostructure matrix array list on the copper surface, including micro-ribbed columns, microchannels and superhydrophilic CuO nanoclads, the problems of boiling start hysteresis and low heat transfer coefficient in traditional pool boiling technology are solved, significantly improving the It has boiling heat transfer performance and is suitable for high heat flow density applications.

CN119008556AActive Publication Date: 2024-11-22SICHUAN UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411092200.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Traditional pool boiling heat transfer technology has problems such as nuclear boiling start hysteresis, low heat transfer coefficients of the two phases and low critical heat flow density, making it difficult to comprehensively improve the comprehensive performance of boiling heat transfer.

Method used

Using a hybrid micro/nanostructure matrix array, the copper surface is divided into matrix grid arrays, including micro-rib columns and microchannels, and a micropore array and superhydrophilic CuO nano-covered structure are installed on its surface to enhance boiling transmission. Thermal performance.

Benefits of technology

The nuclear boiling start in the case where the wall is low is low, significantly improving the two-phase heat transfer coefficient and critical heat flow density, improving the boiling heat transfer performance, and is suitable for application scenarios for high heat flow density heat dissipation requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008556A_ABST
    Figure CN119008556A_ABST
Patent Text Reader

Abstract

The invention discloses a mixed micro / nano structure matrix array surface and a preparation and test method thereof, and belongs to the technical field of multiphase flow and heat transfer, a copper surface is divided into a matrix grid array, and the matrix grid array comprises micro-rib columns serving as nuclear boiling activation areas and micro-channels serving as liquid siphon supplement areas. Micropore arrays are arranged on the surfaces of the micro-rib columns, and the micro-channels are arranged in gaps of the micro-rib columns. The micro-rib columns are made of pure copper materials, and the micro-channels are filled with copper foam grids. The mixed micro / nano structure matrix array surface for improving boiling heat transfer aims at combining unique advantages of different surface structures, efficiently utilizing a solid-liquid heat transfer interface and achieving comprehensive improvement of boiling heat transfer performance. The hybrid matrix array surface is convenient to prepare, low in manufacturing cost and firm in structure, and has huge potential in application scenes with high heat flux heat dissipation requirements in the future.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of multiphase flow and heat transfer, and particularly relates to a hybrid micro / nano structure matrix array surface and a preparation and testing method thereof. Background Art

[0002] With the progress in the field of microelectronics in recent decades, electronic devices have shown iterative leaps in performance and efficiency, which are inevitably accompanied by the continuous improvement of heat dissipation density. The increasing heat flux density of electronic components and the gradual reduction in the size of equipment components have put forward more stringent requirements and technical challenges for cooling technology. How to solve the problems of reduced efficiency and shortened life caused by overheating of high-power components has always been an important issue of concern. Traditional air cooling and single-phase liquid cooling methods are subject to the problems of low heat transfer coefficient and poor heat transfer performance. The two-phase flow cooling method with greater performance potential has gradually attracted more attention. Among them, pool boiling / immersion cooling technology has many practical advantages such as high heat transfer coefficient, stable hydraulic and thermodynamic properties, good direct contact temperature control effect, and flexible selection of active or passive methods according to actual needs.

[0003] However, for decades, pool boiling heat transfer has been plagued by three major problems, including: nucleate boiling start-up (ONB) hysteresis, low two-phase heat transfer coefficient (HTC), and low critical heat flux (CHF). Researchers in this field have proposed many methods to enhance the surface structure of boiling heat transfer performance. However, most methods use a single microstructure design or a combination of two microstructures. Therefore, a single structural form usually only brings significant advantages in one or two aspects of boiling heat transfer characteristics such as ONB, HTC or CHF, and it is often difficult to comprehensively improve the comprehensive performance of boiling heat transfer. Summary of the invention

[0004] The purpose of the present invention is to provide a hybrid micro / nanostructure matrix array surface and its preparation and testing methods, aiming to combine the unique advantages of different surface structures, efficiently utilize the solid-liquid heat transfer interface, and achieve a comprehensive improvement in boiling heat transfer performance. The hybrid matrix array surface is easy to prepare, has low manufacturing cost, and has a strong structure. It will show great potential in future application scenarios with high heat flux density heat dissipation requirements.

[0005] To achieve the above-mentioned purpose, the present invention provides a hybrid micro / nanostructure matrix array surface, which divides the copper surface into a matrix grid array, wherein the matrix grid array includes micro-ribs as nucleate boiling activation areas and micro-channels as liquid siphon replenishment areas, and the surface of the micro-ribs is arranged with a micropore array as a boiling activation core, and the micro-channels are arranged in the gaps between the micro-ribs.

[0006] Preferably, the micro-ribs are made of pure copper, the micro-channels are filled with copper foam grids, and the height of the copper foam grids is not higher than the height of the micro-ribs.

[0007] Preferably, the cavity radius of the micropore array is 40 um to 100 um.

[0008] Preferably, a super-hydrophilic CuO nano-coating structure is provided on the surface of the copper foam grid.

[0009] The present invention also provides a method for preparing a hybrid micro / nano structure matrix array surface, comprising the following steps:

[0010] S1, dividing a 10 mm × 10 mm copper surface into a matrix grid array to form micro-ribs and micro-channels with height differences;

[0011] S2, using a laser cutting machine to cut the pure copper foam into a copper foam grid that matches the size of the microchannel, cleaning it with an ultrasonic water bath device, and then performing an oxidation treatment to form a super-hydrophilic CuO nano-coating structure on the surface of the copper foam grid, and embedding the copper foam grid into the microchannel;

[0012] S3. Calculate the preferred diameter range of the pore size of the micropore array for nucleate boiling based on the boiling phase change activation theory; then design the planar layout based on the specific size of the selected pores; finally, according to the design drawing, use laser etching to drill the cavity array on the surface of the top of the micro-rib column.

[0013] Preferably, in step S2, the cleaning solution in the ultrasonic water bath device is dilute hydrochloric acid, the oxidation treatment solution is a mixed solution of sodium hydroxide and ammonium persulfate, and the oxidation treatment condition is heating in a 70° C. water bath for 30 min.

[0014] The present invention also provides a method for testing the surface of a hybrid micro / nano structure matrix array, which uses a pool boiling experimental device to continuously provide heat to a test sample on the surface of a hybrid micro / nano structure matrix array to deduce the surface temperature of the test sample.

[0015] Preferably, the pool boiling experimental device includes: a boiling water pool cavity, a bottom heating module, a heat transfer surface performance test part, a liquid temperature control unit, a power supply regulator, a data acquisition and processing system, a computer, a high-speed camera and a high-illuminance lamp. The heat transfer surface performance test part is arranged between the boiling water pool cavity and the bottom heating module, the boiling water pool cavity is electrically connected to the liquid temperature control unit, the heat transfer surface performance test part and the liquid temperature control unit are connected to the data acquisition and processing system, and the computer controls the data acquisition and processing system, the high-speed camera and the high-illuminance lamp.

[0016] Preferably, a serpentine condenser and a cover plate for maintaining the water level are provided on the upper part of the boiling water pool cavity, an auxiliary heating rod electrically connected to the liquid temperature control unit is provided inside the boiling water pool cavity, and the test sample is sealed and fixed to the bottom partition of the boiling water pool cavity by high temperature resistant glue;

[0017] The bottom heating module includes a copper column and a heating copper base arranged below the copper column. Three T-type thermocouples are inserted into the copper column. An insert heating rod is arranged below the heating copper base.

[0018] The test sample is set on the copper column of the bottom heating module. The contact surface between the copper column and the test sample is made of high thermal conductivity gallium-based liquid alloy. The gap between the inserted heating rod and the heating copper base is filled with silicone grease with good thermal conductivity. The outer side of the heating copper base is wrapped with mica stone and alumina high-temperature resistant ceramics.

[0019] Preferably, the test sample is inserted with a T-type thermocouple for detecting the temperature of the test sample. The copper column has three T-type thermocouples inserted longitudinally. The T-type thermocouple is connected to the heat transfer surface performance test part. The surface temperature of the test sample is calculated based on the temperatures of the four T-type thermocouples.

[0020] Therefore, the present invention adopts the above-mentioned hybrid micro / nanostructure matrix array surface and its preparation and testing method, and its beneficial effects are:

[0021] 1. By constructing a hybrid surface, the present invention realizes nucleate boiling when the wall superheat is only 2°C. Compared with ordinary copper surface, the two-phase heat transfer coefficient HTC increment is as high as 85%, and the critical heat flux density CHF increment is significantly increased by 226% (332.4W / cm 2 ).

[0022] 2. The present invention provides a new idea of ​​preparing a hybrid micro / nanostructure matrix array surface on the surface of a material to improve its boiling heat transfer performance. It is not limited to copper materials, and other materials with high thermal conductivity such as aluminum materials can be used, and even semiconductor silicon Si can also be used.

[0023] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A conceptual diagram of the hybrid micro / nanostructure matrix array surface proposed in the present invention;

[0025] Figure 2 Schematic diagram of the partition design of the surface of the hybrid micro / nanostructure matrix array and the planar layout of different functional areas in Examples 1-3 of the present invention;

[0026] Figure 3 is a diagram for calculating the laser cavity size on the top surface of the micro-rib column of the present invention;

[0027] Figure 4 It is a plan layout design diagram of the microwell array of the present invention;

[0028] Figure 5 This is an electron microscopic characterization image of the laser-processed microhole array of the present invention;

[0029] Figure 6 The process of making the foam grid of super-hydrophilic CuO nano-coating structure;

[0030] Figure 7 Electron microscope characterization of copper foam grid with super hydrophilic CuO nano-coating structure;

[0031] Figure 8 Schematic diagrams of structures of three embodiments of the present invention;

[0032] Fig. 9 It is a structural schematic diagram of the pool boiling experimental device of the present invention;

[0033] Fig.10 A schematic diagram of placing test samples in the pool boiling experimental device of the present invention;

[0034] Fig.11 The figure is a comparison chart of boiling heat transfer performance between three embodiments of the present invention and a comparative example.

[0035] Reference numerals:

[0036] 1. Boiling water pool chamber; 11. Cover plate; 12. Vent; 13. Serpentine condenser; 14. Observation glass; 15. Auxiliary heating rod; 2. Test sample; 3. Bottom heating module; 31. Copper column; 32. Heating copper base; 33. Insert heating rod; 34. Mica stone; 35. Alumina high temperature resistant ceramic; 36. High thermal conductivity gallium oxide based liquid alloy; 37. Stainless steel support layer; 4. Heat transfer surface performance test part; 41. T-type thermocouple; 5. Liquid temperature control unit; 6. Data acquisition and processing system; 7. Computer; 8. High illumination lamp; 9. High-speed camera. DETAILED DESCRIPTION

[0037] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0038] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.

[0039] In addition, it should be understood that although this specification is described according to the implementation modes, not every implementation mode includes only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation modes that can be understood by those skilled in the art. These other implementation modes are also covered within the protection scope of the present invention.

[0040] The present invention provides a hybrid micro / nanostructure matrix array surface, which divides a 10mm×10mm copper surface into a matrix grid array, wherein the matrix grid array includes micro-ribs as nucleate boiling activation areas and micro-channels as liquid siphon replenishment areas, and the surface of the micro-ribs is evenly arranged with a micropore array as a boiling activation core to accelerate the start of nucleate boiling and realize efficient phase change heat transfer at the solid-liquid interface; the micro-channels are arranged at the gaps between the micro-ribs. The micro-channels are embedded with a copper foam grid with a super-hydrophilic CuO nano-coating structure, which is responsible for the rapid siphoning and storage of the liquid and the resistance to the wall drying phenomenon caused by high heat flux density working conditions. The height of the copper foam grid is not higher than the height of the micro-ribs. The cavity radius of the micropore array is 40um to 100um.

[0041] The working principle of the hybrid micro / nanostructure matrix array surface is as shown in the attached manual. Figure 1 As shown in the figure, A illustrates the boiling phase change behavior of the hybrid micro / nanostructure matrix array surface proposed by the present invention under normal working conditions. The functionally partitioned hybrid surface can promote the generation and growth of boiling bubbles, with high liquid-gas phase change conversion efficiency and high heat transfer coefficient (HTC); on the other hand, it can significantly enhance the siphon effect of the liquid, keep the bottom of the copper-based surface moist, and prevent drying or burning at extremely high heat dissipation density, thereby improving the performance limit value (CHF) of the boiling phase change.

[0042] Figure B shows that at the onset of boiling (ONB), the artificial laser cavity on the top of the copper micro-rib can promote and accelerate the generation of bubbles, reduce the minimum starting energy required for the nucleate boiling phase transition, and greatly promote nucleate boiling.

[0043] Figure C shows that in the full boiling stage (FDB), as the heat flux density gradually increases, the bubbles merge with each other to form bubbles of larger volume. At the same time, the copper foam grid with CuO nano-coating at the bottom of the copper micro-rib column can continuously siphon and store liquid, maintain good wettability of the solid-liquid interface for a long time, and maintain a stable boiling phase change process.

[0044] D in the figure shows that when the critical heat flux density (CHF) is approaching, the bubbles form a huge volume and cover the solid surface. At this time, the solid surface has lost the replenishment of the surrounding liquid, but the liquid stored in the copper foam grid of the CuO nano-coating at the bottom of the copper micro-rib column can continue to maintain the wet state of the heated solid surface for a certain period of time, thereby maintaining the normal boiling phase change. Ultimately, the micro / nanostructure hybrid surface can obtain an ultra-high heat dissipation flux without being burned.

[0045] A method for preparing a hybrid micro / nanostructure matrix array surface comprises the following steps:

[0046] S1, dividing a 10 mm × 10 mm copper surface into a matrix grid array to form micro-ribs and micro-channels with height differences;

[0047] S2. Use a laser cutting machine to cut the pure copper foam into copper foam grids that match the size of the microchannel. After cleaning with an ultrasonic water bath device, perform oxidation treatment to form a super-hydrophilic CuO nano-coating structure on the surface of the copper foam grid. Embed the copper foam grid into the microchannel. The process is as shown in the attached manual. Figure 6 The cleaning solution in the ultrasonic water bath device is dilute hydrochloric acid, the oxidation treatment solution is a mixed solution of sodium hydroxide and ammonium persulfate, and the oxidation treatment condition is heating in a 70°C water bath for 30 minutes;

[0048] The principle of oxidation treatment is:

[0049] Cu+2NaOH+(NH4)2S2O8→Cu(OH)2+(NH4)2SO4+Na2SO4

[0050] Cu(OH)2+2OH - →[Cu(OH)4] 2-

[0051] [Cu(OH)4] 2- →CuO↓+H2O+2OH - ;

[0052] Among them, the electron microscope characterization of the copper foam grid of the super hydrophilic CuO nano-coating structure is shown in the attached manual. Figure 7 As shown, a large amount of nano-sized CuO coating (nanoflower-like) is covered on the surface of the copper foam grid. This copper foam grid with porous CuO nano-coating with super-hydrophilic properties can greatly accelerate liquid replenishment and storage under high heat flow conditions.

[0053] S3. Calculate the preferred diameter range of the pore size of the micropore array for nucleate boiling based on the boiling phase change activation theory. The calculation results are shown in the attached manual. Figure 3As shown; combined with the specific size of the selected cavity, the plane layout design is carried out, and the design result is as shown in the attached manual Figure 4 Finally, according to the design, a microhole array is drilled on the surface of the top of the micro-rib column by laser etching, wherein the instruction manual is attached. Figure 5 This is a picture of the laser processed cavity array. It can be seen that there is a microhole array distributed on the surface of the micro-rib column.

[0054] Example 1

[0055] S1. Divide the single copper surface of the 10mm×10mm×10mm standard sample into a matrix grid array to form micro-ribs and micro-channels with a height difference of 1.2mm; the surface structure diagram is shown in the attached manual. Figure 2 As shown, micro-ribs and micro-channels are alternately distributed on the copper surface, with an edge width of 0.5 mm and a normal width of 1.0 mm;

[0056] S2, using a laser cutting machine to cut the pure copper foam into a copper foam grid that matches the size of the microchannel, wherein the copper foam grid is cleaned by an ultrasonic water bath device, and then oxidized to form a super-hydrophilic CuO nano-coating structure on the surface of the copper foam grid, and the copper foam grid is embedded in the microchannel, wherein the height of the copper foam grid is 0.8 mm;

[0057] S3. Based on the boiling phase change activation theory, the preferred diameter range of the pore size of the micropore array for nucleate boiling is calculated, and the pore diameter is 80μm. Then, based on the specific size of the selected pore, a planar layout design is performed, and the distance between the centers of the two micropores is 120μm. Finally, according to the design drawing, a micropore array is drilled on the surface of the top of the micro-rib column by laser etching.

[0058] Example 2

[0059] S1. Divide the single copper surface of the 10mm×10mm×10mm standard sample into a matrix grid array to form micro-ribs and micro-channels with a height difference of 1.2mm; the surface structure diagram is shown in the attached manual. Figure 2 As shown, micro-ribs and micro-channels are alternately distributed on the copper surface, with an edge width of 0.5 mm and a normal width of 1.0 mm;

[0060] S2, using a laser cutting machine to cut the pure copper foam into a copper foam grid that matches the size of the microchannel, wherein the copper foam grid is cleaned by an ultrasonic water bath device, and then oxidized to form a super-hydrophilic CuO nano-coating structure on the surface of the copper foam grid, and the copper foam grid is embedded in the microchannel, wherein the height of the copper foam grid is 1.0 mm;

[0061] S3. Based on the boiling phase change activation theory, the preferred diameter range of the pore size of the micropore array for nucleate boiling is calculated, and the pore diameter is 80μm. Then, based on the specific size of the selected pore, a planar layout design is performed, and the distance between the centers of the two micropores is 120μm. Finally, according to the design drawing, a micropore array is drilled on the surface of the top of the micro-rib column by laser etching.

[0062] Example 3

[0063] S1. Divide the single copper surface of the 10mm×10mm×10mm standard sample into a matrix grid array to form micro-ribs and micro-channels with a height difference of 1.2mm; the surface structure diagram is shown in the attached manual. Figure 2 As shown, micro-ribs and micro-channels are alternately distributed on the copper surface, with an edge width of 0.5 mm and a normal width of 1.0 mm;

[0064] S2, using a laser cutting machine to cut the pure copper foam into a copper foam grid that matches the size of the microchannel, wherein the copper foam grid is cleaned by an ultrasonic water bath device, and then oxidized to form a super-hydrophilic CuO nano-coating structure on the surface of the copper foam grid, and the copper foam grid is embedded in the microchannel, wherein the height of the copper foam grid is 1.2 mm;

[0065] S3. Based on the boiling phase change activation theory, the preferred diameter range of the pore size of the micropore array for nucleate boiling is calculated, and the pore diameter is 80μm. Then, based on the specific size of the selected pore, a planar layout design is performed, and the distance between the centers of the two micropores is 120μm. Finally, according to the design drawing, a micropore array is drilled on the surface of the top of the micro-rib column by laser etching.

[0066] The structures of the samples prepared in Examples 1 to 3 are as shown in the attached manual. Figure 8 As shown. Three samples were tested, and a pool boiling test device was used to continuously provide heat to the test samples on the surface of the hybrid micro / nanostructure matrix array to estimate the surface temperature of the test samples. Fig. 9 shown.

[0067] The pool boiling experimental device includes: a boiling water pool cavity 1, a bottom heating module 3, a heat transfer surface performance test part 4, a liquid temperature control unit 5, a data acquisition and processing system 6, a computer 7, a high-speed camera 9 and a high-illuminance lamp 8. The heat transfer surface performance test part 4 is arranged between the boiling water pool cavity 1 and the bottom heating module 3, the boiling water pool cavity 1 is electrically connected to the liquid temperature control unit 5, the heat transfer surface performance test part 4 and the liquid temperature control unit 5 are connected to the data acquisition and processing system 6, and the computer 7 controls the data acquisition and processing system 6, the high-speed camera 9 and the high-illuminance lamp 8.

[0068] The upper part of the boiling water pool cavity 1 is provided with a serpentine condenser 13 for maintaining the water level and a cover plate 11, and a vent hole 12 is left on the cover plate 11. The interior of the boiling water pool cavity 1 is provided with an auxiliary heating rod 15 electrically connected to the liquid temperature control unit 5. The test sample 2 is sealed and fixed to the bottom partition of the boiling water pool cavity 1 by using high temperature resistant glue;

[0069] The bottom heating module 3 includes a copper column 31, a heating copper base 32 arranged below the copper column 31, three T-type thermocouples 41 are inserted into the copper column 31, and an inserted heating rod 33 (100W×7) is arranged below the heating copper base 32 to provide heating power for the test sample 2, which is controlled by an AC power regulator.

[0070] The test sample 2 is set on the copper column 31 of the bottom heating module 3. The contact surface between the copper column 31 and the test sample 2 is made of high thermal conductivity gallium-based liquid alloy 36. The gap between the inserted heating rod 33 and the heating copper base 32 is filled with silicone grease with good thermal conductivity. The outer side of the heating copper base 33 is wrapped with mica 34 and alumina high temperature resistant ceramic 35. The T-type thermocouple 41 is connected to the heat transfer surface performance test part 4.

[0071] During the test, as shown in the instruction manual Fig.10 As shown, the test sample 2 is inserted with a T-type thermocouple 41 for detecting the temperature of the test sample 2, and the copper column 31 is longitudinally inserted with three T-type thermocouples 41. The distance Δx between the three adjacent T-type thermocouples 41 on the copper column 31 is 7 mm. The three adjacent T-type thermocouples 41 measure the temperature of different positions of the copper column 31 from bottom to top. The distance L between the T-type thermocouple 41 located in the middle of the test sample 2 and the surface of the mixed micro / nano structure matrix array of the test sample 2 is 4 mm. The temperature of the middle part of the test sample 2 is measured, and the surface temperature of the mixed micro / nano structure matrix array of the test sample 2 is calculated according to the temperature of the four T-type thermocouples 41. During the test, the heating power starts from 0 and gradually increases. When boiling bubbles begin to appear, a high-speed camera 9 is used to shoot the generation and development behavior of boiling bubbles. As the power continues to increase, it eventually reaches the critical heat flux density (CHF) limit value of the test sample 2.

[0072] After testing, the results showed that the 1.2mm thick CuO foam mesh has the greatest improvement in the comprehensive heat transfer performance. Compared with the ordinary traditional smooth copper surface, the hybrid micro / nanostructure matrix array surface achieves: reducing the superheated wall temperature by nearly 7°C to trigger the start of boiling phase change (ONB), obtaining a maximum increase of 85% in the two-phase heat transfer coefficient (HTC), and an increase of up to 226% in the critical heat flux density.

[0073] At the same time, according to the test results, the boiling heat transfer performance of the three samples prepared in the three embodiments was compared with the existing different surfaces as a comparative example. The results are shown in the attached specification. Fig.11 As shown in the figure, the hybrid micro / nanostructure matrix array surface achieves nucleate boiling when the wall superheat is only 2°C. Compared with the existing copper-treated surface in the comparative example, the two-phase heat transfer coefficient HTC increment is as high as 85%, and the critical heat flux density CHF increment is significantly increased by 226% (332.4 W / cm 2 ). It far exceeds the boiling phase change comprehensive heat transfer performance of other ordinary traditional smooth copper wall or single structure surface.

[0074] Therefore, the hybrid micro / nanostructure matrix array surface and its preparation and testing method provided by the present invention can significantly improve the comprehensive performance of boiling heat transfer, and is particularly suitable for application scenarios with high-power cooling requirements such as evaporators, thermal power plants, nuclear reactors, laser weapons, high-power radars, and immersion cooling in data centers.

[0075] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A hybrid micro / nanostructure matrix array surface, characterized in that: The copper surface is divided into a matrix grid array, which includes micro-ribs as nucleate boiling activation areas and micro-channels as liquid siphon replenishment areas. The surface of the micro-ribs is arranged with a micropore array as a boiling activation core, and the micro-channels are arranged in the gaps between the micro-ribs.

2. A hybrid micro / nanostructure matrix array surface according to claim 1, characterized in that: The micro-ribs are made of pure copper, and the micro-channels are filled with copper foam grids, and the height of the copper foam grids is not higher than the height of the micro-ribs.

3. A hybrid micro / nanostructure matrix array surface according to claim 1, characterized in that: The cavity radius of the micropore array is 40um to 100um.

4. A hybrid micro / nanostructure matrix array surface according to claim 2, characterized in that: The surface of the copper foam grid is provided with a super-hydrophilic CuO nano-coating structure.

5. A method for preparing a hybrid micro / nanostructure matrix array surface based on any one of claims 1 to 4, characterized in that: The following steps are involved: S1, dividing a 10 mm × 10 mm copper surface into a matrix grid array to form micro-ribs and micro-channels with height differences; S2, using a laser cutting machine to cut the pure copper foam into a copper foam grid that matches the size of the microchannel, cleaning it with an ultrasonic water bath device, and then performing an oxidation treatment to form a super-hydrophilic CuO nano-coating structure on the surface of the copper foam grid, and embedding the copper foam grid into the microchannel; S3. Calculate the preferred diameter range of the pore size of the micropore array for nucleate boiling based on the boiling phase change activation theory; then design the planar layout based on the specific size of the selected pores; finally, according to the design drawing, use laser etching to drill the cavity array on the surface of the top of the micro-rib column.

6. The method for preparing a hybrid micro / nanostructure matrix array surface according to claim 5, characterized in that: In step S2, the cleaning solution in the ultrasonic water bath device is dilute hydrochloric acid, the oxidation treatment solution is a mixed solution of sodium hydroxide and ammonium persulfate, and the oxidation treatment condition is heating in a 70° C. water bath for 30 minutes.

7. A method for testing a hybrid micro / nanostructure matrix array surface based on any one of claims 1 to 4, characterized in that: A pool boiling experimental device is used to continuously provide heat to the test sample on the surface of the hybrid micro / nanostructure matrix array to infer the surface temperature of the test sample.

8. A method for testing a hybrid micro / nanostructure matrix array surface according to claim 7, characterized in that: The pool boiling experimental device includes: a boiling water pool cavity, a bottom heating module, a heat transfer surface performance test part, a liquid temperature control unit, a data acquisition and processing system, a computer, a high-speed camera and a high-illuminance lamp. The heat transfer surface performance test part is arranged between the boiling water pool cavity and the bottom heating module. The boiling water pool cavity is electrically connected to the liquid temperature control unit. The heat transfer surface performance test part and the liquid temperature control unit are connected to the data acquisition and processing system. The computer controls the data acquisition and processing system, the high-speed camera and the high-illuminance lamp.

9. A method for testing a hybrid micro / nanostructure matrix array surface according to claim 8, characterized in that: A serpentine condenser and a cover plate for maintaining the water level are arranged on the upper part of the boiling water pool cavity, an auxiliary heating rod electrically connected to the liquid temperature control unit is arranged inside the boiling water pool cavity, and the test sample is sealed and fixed to the bottom partition of the boiling water pool cavity by using high temperature resistant glue; The bottom heating module includes a copper column and a heating copper base arranged below the copper column. Three T-type thermocouples are inserted into the copper column. An insert heating rod is arranged below the heating copper base. The test sample is set on the copper column of the bottom heating module. The contact surface between the copper column and the test sample is made of high thermal conductivity gallium-based liquid alloy. The gap between the inserted heating rod and the heating copper base is filled with silicone grease with good thermal conductivity. The outer side of the heating copper base is wrapped with mica stone and alumina high-temperature resistant ceramics.

10. A method for testing a hybrid micro / nanostructure matrix array surface according to claim 9, characterized in that: The test sample is inserted with a T-type thermocouple for detecting the temperature of the test sample. The copper column is longitudinally inserted with three T-type thermocouples, which are connected to the heat transfer surface performance test part. The surface temperature of the test sample is calculated based on the temperatures of the four T-type thermocouples.

Citation Information

Patent Citations

  • Composite hydrophilic / hydrophobic enhanced boiling heat transfer sheet with columnar microstructure

    CN106102414A

  • Preparation method of copper oxide with nano flower-like structure

    CN112897567A

  • Preparation method of working medium heat dissipation element

    CN113237366A

  • Composite microstructure surface for synergistically enhancing boiling heat transfer by utilizing microtubes and micropores

    CN116182614A

  • Enhanced boiling heat transfer experimental device and experimental method based on capillary acting force

    CN116482172A