Gallium oxide junction barrier Schottky diode based on p-i-n junction terminal and preparation method thereof
By forming a p-i-n junction terminal in the gallium oxide Schottky diode, the high-resistance i-Ga2O3 layer is used to reduce the current and heat of NiO, the NiO thermal denaturation problem is solved, and the reliability and pressure resistance of the gallium oxide Schottky diode are improved. .
Patent Information
- Application Number
- CN202410813672.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-22
AI Technical Summary
At the forward voltage, the existing gallium oxide Schottky diodes cause a large amount of current to flow through NiO due to the Ga2O3 epitaxial layer below the NiO layer, resulting in thermal denaturation of NiO, affecting device reliability and withstand voltage.
By converting n-Ga2O3 into a high-resistance state i-Ga2O3 and depositing p-NiO on i-Ga2O3 to form a p-i-n junction terminal. p-NiO is only responsible for alleviating the peak electric field and does not participate in conduction, thereby reducing heat generation and protecting p -NiO does not deteriorate, improving device reliability.
The current in p-NiO is greatly reduced under the forward voltage, prevent heat generation, improve the thermal stability and voltage withstand voltage of the device, and enhance the reliability and performance of the device.
Smart Images

Figure CN119008709A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of semiconductor device technology, specifically relating to a gallium oxide junction barrier Schottky diode, which can be used as a gallium oxide device in high-voltage equipment. Technical Background
[0002] Gallium oxide is a typical example of ultra-wide bandgap semiconductors, possessing superior properties such as ultra-high breakdown field strength of 8MV / cm and ultra-wide bandgap (4.8~4.9eV). It has become one of the ideal technologies for power electronic devices with high voltage, high power, high temperature, high energy efficiency, and high cost performance. It has significant application prospects in fields such as smart grids, new energy electric vehicles, high-speed rail, and data centers. Therefore, gallium oxide semiconductors have become one of the most popular new areas of semiconductor research in recent years.
[0003] The lack of effective p-type doping in β-Ga₂O₃ severely limits its device performance and application prospects. Currently, p-NiO or other p-type semiconductors are commonly used internationally to replace p-Ga₂O₃ in the fabrication of gallium oxide jB devices, as jB devices offer advantages such as high breakdown voltage and low turn-on voltage. However, p-NiO and other p-type semiconductors often suffer from poor thermal stability, leading to increased leakage current and decreased breakdown voltage after prolonged operation, severely impacting device reliability and stability.
[0004] Patent application CN202211540275.5 discloses a "vertical β-Ga2O3 Schottky barrier diode and its fabrication method." This structure, from bottom to top, includes: a cathode metal, an n-type gallium oxide substrate, an n-type gallium oxide epitaxial layer, a p-type NiO layer, and an anode metal layer. Part of the anode metal layer is on the n-type gallium oxide epitaxial layer, and another part is on the p-type NiO layer. Because the Ga2O3 epitaxial layer is below the NiO layer, a large current will flow through the NiO under forward voltage, causing the NiO to thermally deform and leading to device failure, severely limiting device reliability. Summary of the Invention
[0005] The purpose of this invention is to address the shortcomings of the prior art by proposing a gallium oxide junction barrier Schottky diode based on pin junction termination and its fabrication method, which can significantly reduce the current in NiO under forward voltage, prevent NiO from generating heat, improve the thermal stability and reliability of the device, and effectively improve the device's withstand voltage.
[0006] The technical approach to achieve the objective of this invention is as follows: n-Ga2O3 is transformed into a high-resistivity i-Ga2O3 through ion implantation, and p-NiO is deposited on i-Ga2O3. The p-NiO is only responsible for mitigating the peak electric field of the device and does not participate in conduction, thereby reducing the generated heat, protecting the p-NiO from deterioration, improving the reliability of the device, and realizing a high-voltage and high-reliability gallium oxide device.
[0007] Based on the above ideas, the technical solution of the present invention includes the following:
[0008] 1. A gallium oxide junction barrier Schottky diode based on a pin junction termination, comprising, from bottom to top: a cathode electrode, an n-Ga2O3 substrate, an n-Ga2O3 epitaxial layer, a p-NiO layer, and an anode electrode, characterized in that: an i-Ga2O3 annular groove formed by ion implantation is provided between the p-NiO layer and the n-Ga2O3 epitaxial layer, and the p-NiO layer, the i-Ga2O3 annular groove, and the n-Ga2O3 epitaxial layer form a pin junction to reduce the current in the p-NiO layer, reduce heat generation, and improve device reliability.
[0009] Furthermore, the thickness of the n-Ga2O3 epitaxial layer is 100nm-100μm.
[0010] Furthermore, the depth of the i-Ga2O3 is 100nm-10μm, and its area is slightly larger than that of the p-NiO to form a pin junction terminal, so that the p-NiO is only responsible for mitigating the peak electric field and does not participate in conduction, thus avoiding the generation of heat by the p-NiO.
[0011] Furthermore, the p-NiO can also be SnO2 or other p-type semiconductors.
[0012] Furthermore, the cathode electrode has a first metal layer made of Ti with a thickness of 10nm-200nm, and a second metal layer made of either Au or Al with a thickness of 20nm-5μm.
[0013] Furthermore, the anode electrode has a first metal layer made of any one of Ni, Mo, or Pt with a thickness of 10 nm to 200 nm, and a second metal layer made of any one of Au or Al with a thickness of 20 nm to 5 μm.
[0014] Furthermore, the p-NiO adopts a single-layer or multi-layer structure, with each layer having a thickness of 10 nm-10 μm and a background hole concentration of 1 × 10⁻⁶. 15 cm -3 -1×10 20 cm -3 .
[0015] 2. A method for fabricating a gallium oxide junction barrier Schottky diode based on a pin junction termination, comprising the following steps:
[0016] 1) Select gallium oxide epitaxial wafers and clean them. Place the gallium oxide epitaxial wafers in acetone solution and anhydrous ethanol solution in sequence and ultrasonically clean them for 5 min-10 min each. Then rinse them with a large amount of deionized water and dry them with nitrogen gas.
[0017] 2) After cleaning, deposit Ti with a thickness of 10nm-200nm and Au or Al with a thickness of 20nm-5μm on the n+ substrate of the gallium oxide epitaxial wafer, and then perform annealing in a nitrogen atmosphere.
[0018] 3) Ion implantation region patterns are photolithographically patterned on the Ga2O3 epitaxial layer of the gallium oxide epitaxial wafer. N, P, or other ions are implanted into the ion implantation region at a depth of 100 nm-10 μm and an implantation concentration of 1 × 10⁻⁶. 15 -1×10 19 cm -3 This causes the n-Ga2O3 at the injection site to become a high-resistivity state;
[0019] 4) After ion implantation, a junction termination pattern is photolithographically formed on the Ga2O3 epitaxial layer, and after depositing p-NiO, the p-NiO outside the junction termination is stripped off to form a pin junction;
[0020] 5) Photolithographically pattern the anode electrode on the Ga2O3 epitaxial layer, deposit one of the following metals with a thickness of 10nm-200nm: Ni, Mo, or Pt, and Au or Al with a thickness of 20nm-5μm, and peel off the metals other than the anode to form the anode electrode. The edge of the anode forms a pin junction terminal on p-NiO to complete the device fabrication.
[0021] Compared with the prior art, the present invention has the following advantages due to the presence of a high-resistivity i-Ga2O3 layer beneath p-NiO:
[0022] Firstly, it can reduce the current in p-NiO under forward voltage, thereby reducing the heat in p-NiO, which can effectively protect p-NiO from thermal deterioration and improve device reliability.
[0023] Secondly, it enables the pin junction of the device to withstand higher voltages than the pn junction of existing ordinary devices, while reducing device leakage current and improving device performance. Attached Figure Description
[0024] Figure 1 This is a structural diagram of the device of the present invention.
[0025] Figure 2 Schematic diagram of device fabrication process Detailed Implementation
[0026] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments.
[0027] Reference Figure 1This example is a gallium oxide junction barrier Schottky diode with a pin junction termination, comprising, from bottom to top: a cathode electrode 1, an n-Ga₂O₃ substrate 2, an n-Ga₂O₃ epitaxial layer 3, an i-Ga₂O₃ annular groove 4, a p-NiO layer 5, and an anode electrode 6, wherein:
[0028] The cathode electrode 1 is divided into two layers. The first layer is metallic Ti with a thickness of 10nm-200nm, which is located on the lower surface of the n-Ga2O3 substrate 2, and is located on the lower surface of the first metallic layer.
[0029] The n-Ga2O3 substrate 2 has a thickness of 10nm-1000μm and is located on the upper surface of the cathode electrode 1.
[0030] The n-Ga2O3 epitaxial layer 3 has a thickness of 100nm-100μm and is located on the upper surface of the n-Ga2O3 substrate 2.
[0031] The i-Ga2O3 annular groove 4 is embedded inside the outer edge of the upper surface of the n-Ga2O3 epitaxial layer 3, and its area is slightly larger than that of the p-NiO layer 5. It is formed by ion implantation with a depth of 100nm-10μm.
[0032] The p-NiO layer 5 adopts a single-layer or multi-layer structure of SnO2 or other p-type semiconductors, with a thickness of 10nm-10μm per layer and a background hole concentration of 1×10⁻⁶. 15 cm -3 -1×10 20 cm -3 It is located on the upper surface of the i-Ga2O3 annular groove 4 and the Ga2O3 epitaxial layer 3.
[0033] The anode electrode 6 is divided into two layers. The first layer is any one of the metals Ni, Mo, and Pt, with a thickness of 10nm-200nm, located on the upper surface of the p-NiO layer 5 and above the Ga2O3 surrounded by the p-NiO layer 5. The second layer is any one of the metals Au and Al, with a thickness of 20nm-5μm, located on the upper surface of the first metal layer.
[0034] The p-NiO layer 5, the i-Ga2O3 annular groove, and the n-Ga2O3 epitaxial layer 3 form a pin junction to reduce the current in the p-NiO layer 5, reduce heat generation, improve device reliability and withstand voltage, and reduce device leakage current.
[0035] Reference Figure 2 This invention provides three embodiments of a method for fabricating gallium oxide junction barrier Schottky diodes based on pin junction terminations.
[0036] Example 1: A gallium oxide diode with an i-Ga2O3 annular groove depth of 500nm and a p-NiO layer thickness of 100nm was fabricated using an epitaxial wafer with a gallium oxide substrate thickness of 300μm and an epitaxial layer thickness of 10μm.
[0037] Step 1, clean the epitaxial wafer, such as... Figure 2 (a).
[0038] Select homoepitaxial gallium oxide epitaxial wafers and clean them by sequentially immersing them in acetone solution and anhydrous ethanol solution for ultrasonic cleaning for 5 minutes each, then rinsing them with a large amount of deionized water, and finally drying them with nitrogen gas.
[0039] Step 2, prepare the cathode electrode, such as Figure 2 (b)
[0040] Ti / Au = 60 / 120 nm was deposited on the cleaned epitaxial substrate, and then annealed in a nitrogen atmosphere at a temperature of 475 °C for 1 min to form a cathode electrode with good ohmic contact.
[0041] Step 3: Ion implantation forms an i-Ga2O3 annular groove, such as... Figure 2 (c)
[0042] A ring-shaped groove pattern was first lithographically patterned on the gallium oxide epitaxial layer, followed by ion implantation into the ring-shaped groove at a depth of 900 nm and a concentration of 1 × 10⁻⁶. 16 cm -3 The concentration of N ions is 2 × 10⁻⁶. 17 cm -3 P ions form i-Ga2O3 annular grooves;
[0043] The sample was then cleaned sequentially with acetone, isopropanol, and deionized water.
[0044] Step 4, deposit a p-NiO layer, such as Figure 2 (d)
[0045] A second photolithography was performed on the gallium oxide epitaxial layer with i-Ga2O3 annular grooves. After photolithography, a 100nm thick p-NiO was deposited, with a coverage area slightly smaller than i-Ga2O3, so that the anode metal could partially contact i-Ga2O3.
[0046] After deposition, acetone was used to strip p-NiO, followed by washing with acetone, isopropanol and deionized water in sequence to clean the sample.
[0047] Step 5, fabricate the anode electrode, such as Figure 2 (e).
[0048] Photolithography was performed on the gallium oxide epitaxial layer and p-NiO. After photolithography, Ni / Au = 60 / 120nm was deposited to form the anode electrode. The metal outside the anode was then stripped using an acetone solution.
[0049] The stripped sample is then cleaned in acetone, isopropanol, and deionized water in sequence to complete the device fabrication.
[0050] Example 2: A gallium oxide diode with an i-Ga2O3 annular groove depth of 2μm and a p-NiO layer thickness of 20nm was fabricated using an epitaxial wafer with a substrate thickness of 100μm and an epitaxial layer thickness of 100μm.
[0051] Step 1: Clean the sample, such as... Figure 2 (a).
[0052] Select homoepitaxial gallium oxide epitaxial wafers and clean them by immersing them in a piranha solution of H2SO4:H2O2 = 3:1 for 10 minutes, then rinsing them with deionized water, and finally drying them with nitrogen gas.
[0053] Step two, prepare the cathode electrode, such as Figure 2 (b)
[0054] Ti / Au = 40 / 200 nm was deposited on the cleaned epitaxial substrate, and then annealed in a nitrogen atmosphere at 450 °C for 60 s to form a good ohmic contact.
[0055] Step 3: Ion implantation forms an i-Ga2O3 annular groove, such as... Figure 2 (c)
[0056] A ring-shaped groove pattern was first lithographically patterned on the gallium oxide epitaxial layer, followed by ion implantation into the ring-shaped groove at a depth of 500 nm and a concentration of 5 × 10⁻⁶. 18 cm -3 The concentration of N ions is 9 × 10⁻⁶. 16 cm -3 The P ions are used to form an i-Ga2O3 annular groove; then the sample is cleaned with acetone, isopropanol and deionized water in sequence.
[0057] Step four, deposit a p-NiO layer, such as Figure 2 (d)
[0058] A second photolithography process was performed on the gallium oxide epitaxial layer with i-Ga2O3 annular grooves. After photolithography, a 10 nm thick p-NiO low-doped layer with a doping concentration of 1 × 10⁻⁶ was deposited. 17 cm -3 A 10 nm thick p-NiO highly doped layer was then deposited, with a doping concentration of 1 × 10⁻⁶. 18 cm-3 Its coverage area is slightly smaller than that of the i-Ga2O3 annular groove, so that the anode metal can partially contact the i-Ga2O3;
[0059] After deposition, acetone was used to strip p-NiO, followed by washing with acetone, isopropanol and deionized water in sequence to clean the sample.
[0060] Step 5: Fabricate the anode electrode, such as... Figure 2 (e).
[0061] Photolithography was performed on the gallium oxide epitaxial layer and p-NiO. After photolithography, Ni / Au = 20 / 300nm was deposited to form the anode electrode. The metal outside the anode was stripped using acetone solution. The stripped sample was then placed in acetone, isopropanol and deionized water for cleaning to complete the device fabrication.
[0062] Example 3: A gallium oxide diode with a substrate thickness of 600 μm, an epitaxial layer thickness of 20 μm, an i-Ga2O3 annular groove depth of 1 μm, and a p-NiO layer thickness of 300 nm was fabricated.
[0063] Step A: Clean the sample, such as... Figure 2 (a).
[0064] A1) Select homoepitaxial gallium oxide epitaxial wafers and clean them by immersing them in a piranha solution of H2SO4:H2O2 = 3:1 for 10 minutes, and then rinsing them with deionized water.
[0065] A2) Place the sample in acetone solution and anhydrous ethanol solution in sequence and sonicate for 5 minutes each, then rinse with plenty of deionized water, and finally dry with nitrogen.
[0066] Step B, prepare the cathode electrode, such as Figure 2 (b)
[0067] B1) Ti / Al was deposited on the cleaned epitaxial wafer substrate with thicknesses of 30 / 300 nm, respectively.
[0068] B2) Annealing is performed in a nitrogen atmosphere at a temperature of 425°C for 90 seconds to form good ohmic contact.
[0069] Step C, ion implantation forms an i-Ga2O3 annular groove, such as Figure 2 (c)
[0070] C1) A ring-shaped groove pattern is first lithographically patterned on the gallium oxide epitaxial layer, and then ion implantation is performed in the ring-shaped groove to a depth of 800 nm and a concentration of 1 × 10⁻⁶. 19 cm -3 The N ions and their concentration are 1×1019 cm -3 P ions form i-Ga2O3 annular grooves;
[0071] C2) Use positive adhesive stripping solution to heat in a 70°C water bath for 1 hour, then wash with acetone, isopropanol and deionized water in sequence to clean the sample.
[0072] Step D, deposit a p-NiO layer, as follows Figure 2 (d)
[0073] D1) Perform secondary photolithography on the gallium oxide epitaxial layer with i-Ga2O3 annular grooves, and deposit a 300nm thick p-NiO after photolithography. Its coverage area is slightly smaller than i-Ga2O3 so that the anode metal can partially contact i-Ga2O3.
[0074] D2) After deposition, acetone was used to strip p-NiO, followed by washing with acetone, isopropanol and deionized water in sequence to clean the sample.
[0075] Step E, fabricate the anode electrode, such as Figure 2 (e).
[0076] E1) Photolithography was performed on gallium oxide epitaxial layer and p-NiO. After photolithography, Pt / Au with thicknesses of 50 / 100nm were deposited to form the anode electrode. The metal outside the anode was removed by heating in a water bath at 75℃ for 40min with positive stripping solution.
[0077] E2) The stripped sample is then placed in acetone, isopropanol, and deionized water for cleaning to complete the device fabrication.
[0078] The above are merely three embodiments of the present invention and do not constitute any limitation on the present invention. Obviously, those skilled in the art, after understanding the content and principle of the present invention, may make various modifications and changes in form and details without departing from the principle and structure of the present invention. For example, the p-NiO layer may also be SnO2 or other p-type semiconductors. However, these modifications and changes based on the ideas of the present invention are still within the scope of protection of the claims of the present invention.
Claims
1. A gallium oxide junction barrier Schottky diode based on a pin junction terminal, comprising from bottom to top: A cathode electrode (1), an n-Ga2O3 substrate (2), an n-Ga2O3 epitaxial layer (3), a p-NiO layer (5), and an anode electrode (6), characterized in that an i-Ga2O3 annular groove (4) formed by ion implantation is provided between the p-NiO layer (5) and the n-Ga2O3 epitaxial layer (3), and the p-NiO layer (5), the i-Ga2O3 annular groove (4), and the n-Ga2O3 epitaxial layer (3) form a pin junction to reduce the current in the p-NiO layer (5), reduce heat generation, and improve device reliability.
2. The gallium oxide diode according to claim 1, characterized in that: The thickness of the n-Ga2O3 epitaxial layer (3) is 100nm-100μm.
3. The gallium oxide diode according to claim 1, characterized in that: The depth of i-Ga2O3 (4) is 100nm-10μm, and its area is slightly larger than that of the p-NiO layer (5) to form a pin junction terminal, so that p-NiO is only responsible for alleviating the peak electric field and does not participate in conduction, thereby avoiding heat generation by p-NiO.
4. The gallium oxide diode according to claim 1, characterized in that: The cathode electrode (1) has a first metal layer made of metal Ti with a thickness of 10nm-200nm, and a second metal layer made of any one of Au and Al with a thickness of 20nm-5μm.
5. The gallium oxide diode according to claim 1, characterized in that: The anode electrode (6) has a first metal layer made of any one of Ni, Mo and Pt with a thickness of 10nm-200nm, and a second metal layer made of any one of Au and Al with a thickness of 20nm-5μm.
6. The gallium oxide diode according to claim 1, characterized in that: The p-NiO layer (5) is a single-layer or multi-layer structure, each layer has a thickness of 10 nm-10 μm, and the background hole concentration is 1×10 15 cm -3 -1×10 20 cm -3 .
7. A method for manufacturing a gallium oxide junction barrier Schottky diode based on a pin junction terminal, comprising the following steps: 1) Selecting a gallium oxide epitaxial wafer and cleaning it, that is, placing the gallium oxide epitaxial wafer in an acetone solution and an anhydrous ethanol solution in turn for ultrasonic cleaning for 5 min to 10 min each, then rinsing it with a large amount of deionized water, and then drying it with nitrogen; 2) depositing Ti with a thickness of 10 nm to 200 nm and Au or Al with a thickness of 20 nm to 5 μm on the n+ substrate layer of the cleaned gallium oxide epitaxial wafer, and then performing annealing in a nitrogen environment; 3) Photolithography of the ion implantation region pattern is performed on the Ga2O3 epitaxial layer of the gallium oxide epitaxial wafer, and N, P or other ions are implanted into the ion implantation region with an implantation depth of 100nm-10μm and an implantation concentration of 1×10 15 -1×10 19 cm -3 , so that the n-Ga2O3 in the injection area becomes a high-resistance state; 4) Photolithography of the junction terminal pattern on the Ga2O3 epitaxial layer after ion implantation, and after depositing p-NiO, peeling off the p-NiO outside the junction terminal to form a pin junction; 5) Photolithography of an anode electrode pattern is performed on the Ga2O3 epitaxial layer, and one of the metals Ni, Mo or Pt with a thickness of 10nm-200nm and Au or Al with a thickness of 20nm-5μm are deposited. The metal other than the anode is peeled off to form an anode electrode. The edge of the anode forms a pin junction terminal on the p-NiO to complete the device manufacturing.
8. The method according to claim 7, characterized in that The annealing temperature in step 2) is 400°C-550°C, and the annealing time is 30s-5min.
Citation Information
Patent Citations
Vertical beta-Ga2O3 Schottky barrier diode and preparation method thereof
CN116190417A