Zr-based amorphous alloy and preparation method and application thereof
By preparing micron-scale groove arrays on the surface of Zr-based amorphous alloy, the materials and accuracy limitations of traditional micro-nano structure processing technology are solved, and efficient and low-cost microstructure preparation is achieved, which significantly improves the light absorption of solar photovoltaic panels Rate and stain resistance.
Patent Information
- Application Number
- CN202410935909.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional micro-nano structure processing technology has problems such as limited material range, long time consumption, high cost and low accuracy, which limits the feasibility of mass production of micro-nano structures, and solar photovoltaic panel components are susceptible to stain accumulation, corrosion, and scale corrosion.
A micron-scale groove array was prepared on the surface by thermoplastic forming using Zr-based amorphous alloy. Combined with the high tempering resistance and thermal stability of the mold steel, the precision replication of the microarray structure is achieved, with anti-reflection and hydrophobic effects.
It improves the light absorption rate of photovoltaic panels, reduces the risks of stain accumulation, corrosion, and scale, and achieves high-precision and low-cost microstructure preparation, which is suitable for solar photovoltaic panel components.
Smart Images

Figure CN119008752A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional materials, and specifically relates to a Zr-based amorphous alloy and a preparation method and application thereof. Background Art
[0002] With the rapid development of science and technology, more and more scientific research focuses on the micro-field, and the size of products designed and manufactured is getting smaller and smaller, even reaching the micro-nano scale. When the size of an object reaches the micro-nano level, its optical properties will change significantly, which will have a great impact on the characteristics of light absorption and transmission. Studies have found that surface microstructures can improve the radiation characteristics of objects, significantly increase the absorption rate of light, and can be used as components of solar photovoltaic panels. In addition, solar photovoltaic panels are exposed to the air for a long time and are easily eroded by dust, rain and snow. Therefore, they need to have the ability to prevent stain accumulation, corrosion, scaling, etc. Inspired by the lotus leaf effect in nature, it was found that surface microstructures can effectively improve the material's ability to remove dirt. Based on this, it is of great research significance to prepare efficient functional microstructures on the surface of advanced materials.
[0003] There are relatively mature methods for processing micro-nano structures, and structures of various scales and shapes can be processed within a certain range. However, on the one hand, the range of materials that can be used by traditional preparation technologies such as electrical discharge machining (EDM), laser processing, diamond cutting and reactive ion etching is limited. On the other hand, the processing is time-consuming, costly and has low precision, which limits its mass production. Exploring and developing new materials and new preparation technologies suitable for micro-nano structures has become a key issue in current research.
[0004] Amorphous alloys have the characteristics of short-range order and long-range disorder, and have no defects such as grain boundaries and dislocations. This makes amorphous alloys have many excellent properties, such as high strength, high hardness, high elasticity, wear resistance, electrical properties, superconductivity, etc. Therefore, amorphous alloys have great application potential in the fields of medicine, aerospace, and shipbuilding, especially in optics, electromagnetics, and coatings. In the preparation of optical devices, compared with other traditional materials, the high surface finish and reflectivity of amorphous alloys can greatly improve the surface quality and performance of gratings. In addition, optical gratings require precise geometric dimensions, ranging from tens of microns to nanometers. Amorphous alloys show excellent forming ability in this microscopic scale range. They have superplasticity and low forming resistance in the supercooled liquid phase (glass transition temperature Tg ~ crystallization temperature Tx), which makes it possible to achieve net forming of amorphous alloys through secondary processing, and also provides new ideas for preparing gratings using amorphous alloys in the supercooled liquid phase. Summary of the invention
[0005] In view of the above-mentioned prior art, the present invention provides a Zr-based amorphous alloy and a preparation method and application thereof. A micron-scale groove array is prepared on the surface of the amorphous alloy material by a thermoplastic forming method. The prepared amorphous alloy has good performance, high shape and size accuracy, and low manufacturing cost. It has anti-reflection and hydrophobic effects and can be used to prepare solar photovoltaic panel components.
[0006] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is: to provide the application of Zr-based amorphous alloy in the preparation of solar photovoltaic panel components, the surface of the Zr-based amorphous alloy has a micron-scale groove array, the depth of the micron-scale groove array is 50 to 100 μm, the width is 50 to 100 μm, and the spacing between two adjacent grooves is 50 to 100 μm.
[0007] The beneficial effects of the above technical solution adopted in the present invention are: the surface microstructure can improve the radiation characteristics of the object, significantly increase the light absorption rate, and can be used as a solar photovoltaic panel component; and the solar photovoltaic panel is exposed to the air for a long time and is easily corroded by dust, rain and snow, so it is necessary to have the ability to prevent stain accumulation, corrosion, scaling, etc.; the Zr-based amorphous alloy prepared by the present invention also has good anti-reflection and hydrophobic effects, which can effectively solve the problems encountered in solar photovoltaic panel components in the prior art.
[0008] Based on the above technical solution, the present invention can also be improved as follows.
[0009] Furthermore, the depth of the micrometer-scale groove array is 85 μm, 93 μm or 100 μm, the width is 100 μm, and the interval between two adjacent grooves is 100 μm.
[0010] Furthermore, the preparation method of the Zr-based amorphous alloy comprises the following steps:
[0011] S1: A micron-scale groove array is processed on the mold surface by a micro-engraving method. The depth of the micron-scale groove array is 50-100 μm, the width is 50-100 μm, and the spacing between two adjacent grooves is 50-100 μm;
[0012] S2: Assemble the Zr-based amorphous alloy block sample with the mold obtained in step S1 and perform thermoplastic forming, and demold after cooling to obtain the product.
[0013] The beneficial effect of the above-mentioned further technical scheme adopted by the present invention is: a microarray structure is prepared on the surface of an amorphous alloy by a thermoplastic forming method, firstly a mold required for the thermoplastic forming process is prepared, the amorphous alloy is placed in the mold cavity and heated to a suitable temperature in its supercooled liquid phase region, and then a certain force is applied to it to make it undergo viscous rheology and fill the mold cavity, thereby replicating the morphology of the mold steel surface, and the amorphous alloy is obtained after cooling and demolding; the preparation method provided by the present invention is convenient to operate, has a short processing cycle, low manufacturing cost and is convenient for mass production, and the obtained amorphous alloy has good performance and high shape and size accuracy.
[0014] Furthermore, the material of the mold in step S1 is hot working die steel RM2, LM1 or Y4.
[0015] The beneficial effect of the above further technical solution adopted by the present invention is that RM2, LM1 and Y4 die steels have high tempering resistance and thermal stability, thermal strength, high temperature hardness and wear resistance, and are suitable for making hot working dies that require high temperature strength and wear resistance.
[0016] Furthermore, in step S1 , the depth of the micrometer-scale groove array is 100 μm, the width is 100 μm, and the spacing between two adjacent grooves is 100 μm.
[0017] Furthermore, in step S2, the temperature of the thermoplastic forming is 430°C, the pressure is 400-1200N, and the processing rate is 0.001s -1 .
[0018] Furthermore, the pressure of the thermoplastic forming in step S2 is 400, 800 or 1200N.
[0019] The beneficial effect of the present invention adopting the above further technical solution is that the prepared Zr-based amorphous alloy has good hydrophobicity and anti-reflection effect.
[0020] Furthermore, the chemical composition of the Zr-based amorphous alloy bulk sample is (Zr 0.6336 Cu 0.1452 Ni 0.1012 Al 0.12 ) 97.4 Er 2.6 .
[0021] The beneficial effects of the above further technical solution of the present invention are: the Zr-based amorphous alloy has a strong amorphous forming ability and a wide supercooled liquid phase region, and has a series of excellent comprehensive properties; the strength, elasticity, toughness and hardness of the Zr-based amorphous alloy are very high; it also has good corrosion resistance and biocompatibility; the chemical composition is (Zr 0.6336 Cu 0.1452 Ni 0.1012 Al 0.12) 97.4 Er 2.6 The amorphous alloy has good glass-forming ability and thermal stability.
[0022] Further, the Zr-based amorphous alloy bulk sample is prepared by the following steps:
[0023] S1: Put a Zr-based amorphous alloy raw material into a water-cooled copper crucible magnetic suspension melting furnace, introduce argon gas with a purity of 99.99wt% as a protective gas, heat and melt three times to obtain an alloy ingot;
[0024] S2: placing a pressure valve and a copper mold in the water-cooled copper crucible magnetic suspension melting furnace of step S1, heating to remelt the alloy ingot of step S1, and preparing a Zr-based amorphous alloy plate sample by negative pressure copper mold suction casting;
[0025] S3: Cut the Zr-based amorphous alloy plate sample into a Zr-based amorphous alloy block sample using an electric spark wire cutting machine.
[0026] The beneficial effects of the above further technical solution adopted by the present invention are: simple process, convenient operation, good quality of the obtained Zr-based amorphous alloy bulk sample, and easy preparation of Zr-based amorphous alloy with micron-scale groove array on the surface.
[0027] Furthermore, a Zr-based amorphous alloy is prepared by the preparation method of a Zr-based amorphous alloy.
[0028] The beneficial effect of the above further technical solution of the present invention is that the Zr-based amorphous alloy prepared by the present invention has a contact angle of 115° to 125°, an absorptivity of 90% to 95%, and has good anti-reflection and hydrophobic effects.
[0029] The beneficial effects of the present invention are as follows: the present invention provides a method for preparing a Zr-based amorphous alloy having a micron-scale groove array on the surface by thermoplastic forming. Compared with the prior art, the method has a short processing cycle, a simple process, and is easy to carry out mass production. The microstructure of the mold surface can be precisely replicated, the forming effect is good, and the manufacturing cost is low. The prepared Zr-based amorphous alloy has good performance, high shape and size accuracy, excellent anti-reflection (light absorption rate is 94.21%) and hydrophobicity (contact angle is 121.278°), and can be used to prepare solar photovoltaic panel components, significantly improving the light absorption rate of solar photovoltaic panel components and at the same time having the ability to prevent stain accumulation, corrosion, scaling, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The XRD diagram of the cast Zr-based amorphous alloy prepared by the present invention;
[0031] Figure 2 An optical microscope image of a mold steel having a micron-scale groove array on its surface used in the present invention;
[0032] Figure 3 XRD patterns of Zr-based amorphous alloys with micron-scale groove arrays on the surface prepared in Examples 2 to 4;
[0033] Figure 4 The SEM morphology of the Zr-based amorphous alloy having a micron-scale groove array on the surface prepared in Examples 2 to 4;
[0034] Figure 5 CLSM images of Zr-based amorphous alloys with micron-scale groove arrays on the surface prepared in Examples 2 to 4;
[0035] Figure 6 The contact angle diagram of the Zr-based amorphous alloy having a micron-scale groove array on the surface prepared in Examples 2 to 4;
[0036] Figure 7 The light absorption rate curves of the Zr-based amorphous alloys with micron-scale groove arrays on the surface prepared in Examples 2 to 4. DETAILED DESCRIPTION
[0037] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.
[0038] Example 1
[0039] A chemical composition of (Zr 0.6336 Cu 0.1452 Ni 0.1012 Al 0.12 ) 97.4 Er 2.6 The Zr-based amorphous alloy is prepared by the following steps:
[0040] S1: Add metal raw materials in proportion according to the chemical composition of the Zr-based amorphous alloy, and the raw materials are all high-purity metals of various elements; during the smelting process, the smelting environment is maintained as a high-purity argon gas protection with a purity of 99.99wt%; the metal raw materials are placed in a water-cooled copper crucible magnetic levitation smelting furnace for heating. At the beginning, the heating power is increased once every 30 seconds, each time by 0.1kW, and slowly heated to 0.5kW, and then heated at a frequency of increasing 0.5kW every 30 seconds. When the heating power reaches 8kW, keep warm for 1min, turn off the heating switch to stop heating, and in order to ensure the uniformity of the alloy composition, the smelting process is carried out three times; finally, turn off the power supply, and cool it with cooling water inside the water-cooled copper crucible to obtain an alloy ingot (i.e., cast Zr-based amorphous alloy material).
[0041] S2: Put a pressure valve and a copper mold into the water-cooled copper crucible magnetic levitation melting furnace of step S1, and prepare a Zr-based amorphous alloy plate by copper mold suction casting method; before using the copper mold to suck and cast the sample, it is necessary to adjust the pressure difference by vacuuming and filling with high-purity argon gas with a purity of 99.99wt%. According to the size of the suction-cast plate sample, the pressure difference is adjusted to about 0.03MPa and then the pressure valve is closed, and the operation steps at the beginning of smelting are repeated. When the heating power is increased to 8kW, keep warm for 1min, and then reduce the power by 0.5kW every 30s until it is reduced to 6.5kW, and then preheat the copper mold. After the power drops to 6kW, the alloy melt is quickly sucked into the copper mold by the pressure difference, and the high thermal conductivity of pure copper is used to achieve rapid cooling of the melt in the mold; finally, turn off the power, and take out the prepared Zr-based amorphous alloy plate sample with a size of 20×70×3mm after the copper mold is cooled.
[0042] S3: The Zr-based amorphous alloy sheet is cut into Zr-based amorphous alloy block samples using an electric spark wire cutting machine and a molybdenum wire with a specification of 0.18 mm.
[0043] S4: Grind the Zr-based amorphous alloy block sample as a whole to remove the surface roughness and unevenness; polish the formed surface to ensure that the sample surface is smooth and flat, and clean it with ultrasonic wave.
[0044] Example 2
[0045] A Zr-based amorphous alloy having a micron-scale groove array on its surface, wherein the depth of the micron-scale groove array is 85 μm, the width is 100 μm, and the spacing between two adjacent grooves is 100 μm, is prepared by the following steps:
[0046] S1: Select hot working die steel RM2 as the die material, and use the micro-engraving method to process a micron-scale groove array structure on the die steel surface. The depth of the micron-scale groove array is 100μm, the width is 100μm, and the spacing between two adjacent grooves is 100μm. The working parameters of the micro-engraving machine are: spindle speed is 20000r / min, processing speed is 6000mm / min, cutting speed is 400mm / min, and feed amount is 0.005mm.
[0047] S2: Place the mold and the Zr-based amorphous alloy block sample in the mold frame, place the assembled mold frame in the heating chamber of the high and low temperature mechanical properties testing machine (UTM5105SYXL), close the heating chamber and evacuate it to a vacuum state, introduce high-purity argon gas with a purity of 99.99wt% as a protective gas, and perform thermoplastic forming; the stamping temperature of the forming process is 430℃, the pressure is 400N, and the processing rate is 0.001s -1 .
[0048] S3: After the microstructure of the mold steel surface is precisely replicated on the surface of the Zr-based amorphous alloy block sample, the mold is lowered to the air-cooled copper coil for air cooling and demolding.
[0049] Example 3
[0050] A Zr-based amorphous alloy having a micron-scale groove array on its surface, wherein the micron-scale groove array has a depth of 93 μm, a width of 100 μm, and a spacing between two adjacent grooves of 100 μm; compared with Example 2, the preparation method thereof is characterized in that the pressure of the forming process in step S2 is adjusted to 800 N, and the other conditions remain unchanged.
[0051] Example 4
[0052] A Zr-based amorphous alloy having a micron-scale groove array on its surface, wherein the micron-scale groove array has a depth of 100 μm, a width of 100 μm, and a spacing between two adjacent grooves of 100 μm; compared with Example 2, the preparation method thereof is characterized in that the pressure of the forming process in step S2 is adjusted to 1200 N, and the other conditions remain unchanged.
[0053] Experimental example
[0054] 1. The as-cast Zr-based amorphous alloy material (Zr 0.6336 Cu 0.1452 Ni 0.1012 Al 0.12 ) 97.4 Er 2.6 The amorphous alloy samples for thermoplastic forming were cut by electric spark wire cutting machine. The cast Zr-based amorphous alloy material (represented as As-cast in the figure) that can be used in solar photovoltaic panel components was analyzed by XRD. The results are as follows: Figure 1 As shown, the amorphous alloy material used in solar photovoltaic panel components maintains a completely amorphous structure and is suitable for thermoplastic forming.
[0055] 2. The optical microscope images of the mold steel used in Examples 2 to 4 are as follows: Figure 2 As shown, it can be seen that the surface has a micron-scale groove array. After detection, the depth of the groove array is 100 μm, the width is 100 μm, and the spacing between two adjacent grooves is 100 μm.
[0056] 3. XRD analysis was performed on the Zr-based amorphous alloys having micron-scale groove arrays on the surface after thermoplastic forming in Examples 2 to 4. The results are as follows: Figure 3As shown, 400N represents the sample prepared in Example 2, 800N represents the sample prepared in Example 3, and 1200N represents the sample prepared in Example 4; the curve shows a typical diffuse scattering peak peculiar to amorphous materials, and no crystal peak appears, indicating that the material still maintains an amorphous alloy state after thermoplastic forming.
[0057] 4. The SEM and CLSM images of the Zr-based amorphous alloys prepared in Examples 2 to 4 are as follows: Figure 4 , 5 As shown, (a) represents the sample prepared in Example 2, (b) represents the sample prepared in Example 3, and (c) represents the sample prepared in Example 4. It can be seen that the surface of the Zr amorphous alloy prepared in Examples 2 to 4 has a micron-scale groove array; after testing, the depth of the groove array of the sample prepared in Example 2 is 85μm, the width is 100μm, and the spacing between two adjacent grooves is 100μm; the depth of the groove array of the sample prepared in Example 3 is 93μm, the width is 100μm, and the spacing between two adjacent grooves is 100μm; the depth of the groove array of the sample prepared in Example 4 is 100μm, the width is 100μm, and the spacing between two adjacent grooves is 100μm.
[0058] 5. The contact angle test of the Zr-based amorphous alloy prepared in Examples 2 to 4 was carried out. The results are as follows: Figure 6 As shown, (a) represents the sample prepared in Example 2, (b) represents the sample prepared in Example 3, and (c) represents the sample prepared in Example 4, and the corresponding contact angles of the Zr-based amorphous alloy surface are 116.278°, 118.35°, and 121.278°, respectively, which are better than the existing aluminum alloy surface (contact angle of 90.121°), that is, the Zr-based amorphous alloy with a micron-scale groove array on the surface shows good hydrophobicity.
[0059] 6. The Zr-based amorphous alloys prepared in Examples 2 to 4 were used for light absorption test. The test curves are shown in FIG. Figure 7 As shown, 85 μm represents the sample prepared in Example 2, 93 μm represents the sample prepared in Example 3, and 100 μm represents the sample prepared in Example 4, and the corresponding light absorption rates are 91.39%, 92.61%, and 94.21%, respectively, which are better than the absorption rate of silicon grating prepared by vibration-assisted nanoimprinting (absorption rate is 70%), indicating that the Zr-based amorphous alloy with micron-scale groove array has good anti-reflection properties, meets the functional application requirements, and can be used to prepare solar photovoltaic panel components.
[0060] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.
Claims
1. Application of Zr-based amorphous alloy in the preparation of solar photovoltaic panel components, wherein the surface of the Zr-based amorphous alloy has a micron-scale groove array, the depth of the micron-scale groove array is 50 to 100 μm, the width is 50 to 100 μm, and the spacing between two adjacent grooves is 50 to 100 μm.
2. The use according to claim 1, Features: The micron-scale groove array has a depth of 85 μm, 93 μm or 100 μm, a width of 100 μm, and a spacing between two adjacent grooves of 100 μm.
3. The method for preparing the Zr-based amorphous alloy in the application of claim 1, It is characterized in that The following steps are involved: S1: machining a micron-scale groove array on the surface of the mold by a micro-engraving method, wherein the depth of the micron-scale groove array is 50-100 μm, the width is 50-100 μm, and the spacing between two adjacent grooves is 50-100 μm; S2: Assembling the Zr-based amorphous alloy block sample with the mold obtained in step S1 and performing thermoplastic forming, and demolding after cooling to obtain the product.
4. The method for preparing the Zr-based amorphous alloy according to claim 3, Features: The material of the mold in step S1 is hot working die steel RM2, LM1 or Y4.
5. The method for preparing the Zr-based amorphous alloy according to claim 3, Features: The micron-scale groove array in step S1 has a depth of 100 μm, a width of 100 μm, and a spacing between two adjacent grooves of 100 μm.
6. The method for preparing the Zr-based amorphous alloy according to claim 3, Features: In step S2, the temperature of the thermoplastic forming is 430°C, the pressure is 400-1200N, and the processing rate is 0.001s -1 .
7. The method for preparing the Zr-based amorphous alloy according to claim 6, Features: The pressure of the thermoplastic forming in step S2 is 400, 800 or 1200N.
8. The method for preparing the Zr-based amorphous alloy according to claim 3, Features: The chemical composition of the Zr-based amorphous alloy bulk sample is (Zr 0.6336 Cu 0.1452 Ni 0.1012 Al 0.12 ) 97.4 Er 2.6 .
9. The method for preparing the Zr-based amorphous alloy according to claim 3, It is characterized in that The Zr-based amorphous alloy bulk sample is prepared by the following steps: S1: Put a Zr-based amorphous alloy raw material into a water-cooled copper crucible magnetic suspension melting furnace, introduce argon gas with a purity of 99.99wt% as a protective gas, heat and melt three times to obtain an alloy ingot; S2: placing a pressure valve and a copper mold in the water-cooled copper crucible magnetic suspension melting furnace of step S1, heating to remelt the alloy ingot of step S1, and preparing a Zr-based amorphous alloy plate sample by negative pressure copper mold suction casting; S3: Cutting the Zr-based amorphous alloy plate sample into the Zr-based amorphous alloy block sample by using an electric spark wire cutting machine.
10. The Zr-based amorphous alloy prepared by the method for preparing a Zr-based amorphous alloy according to any one of claims 3 to 9.